Lithium niobate-based waveguide array and method for manufacturing the same

By introducing asymmetric lithium niobate grating structure and wide waveguide design into the lithium niobate optical phased array, the crosstalk problem caused by the small spacing between adjacent waveguides is solved, high transmittance and low insertion loss are achieved, and the beam is expanded Deflection angle range, suitable for optical communication and other fields.

CN112255724BActive Publication Date: 2024-12-03SUZHOU KEWO MICROELECTRONICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011298132.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-18
Publication Date
2024-12-03
Estimated Expiration
2040-11-18

AI Technical Summary

Technical Problem

When the existing lithium niobate optical phased array is in a wide field of view beam scanning range, the small spacing between adjacent waveguides leads to serious crosstalk, making it difficult to independently control the phase or amplitude, and the reduced transmission length cannot effectively suppress crosstalk, limiting beam scanning. Angle range.

Method used

Design a waveguide array based on lithium niobate, including a silicon-based substrate, a silicon dioxide buffer layer, a core layer and a silica cladding, and adds left and right symmetric lithium niobate wide waveguide and asymmetric niobate to the core layer. The lithium grating structure suppresses crosstalk between waveguides through optimization of grating period and duty cycle, and forms a low crosstalk array through a specific manufacturing method.

Benefits of technology

It realizes high transmittance and low insertion loss in the 1550nm optical band, expands the beam deflection angle range, is suitable for optical phased arrays and optical communication fields, and maintains low insertion loss and crosstalk in the range of 1520-1600nm. The bandwidth reaches 80nm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112255724B_ABST
    Figure CN112255724B_ABST
Patent Text Reader

Abstract

The present invention discloses a waveguide array based on lithium niobate, comprising: a silicon-based substrate; a silicon dioxide buffer layer deposited on the silicon-based substrate; a core layer located on the silicon dioxide buffer layer; a silicon dioxide cladding layer located on the core layer and covering the core layer; wherein the core layer comprises: two left-right symmetrical lithium niobate wide waveguides, a first lithium niobate grating and a second lithium niobate grating; the first lithium niobate grating and the second lithium niobate grating are located between the two lithium niobate wide waveguides; the first lithium niobate grating is located on the left of the second lithium niobate grating. The present invention also discloses a method for manufacturing a waveguide array based on lithium niobate. The present invention can suppress crosstalk between waveguides in the 1550nm optical band, and achieve high transmittance and low insertion loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to waveguide arrays based on lithium niobate. Background Art

[0002] Integrated on-chip optical phased array (OPA) is one of the key components of light detection and ranging (Lidar), and is used in many applications (e.g., unmanned driving, aerial mapping, and optical communications) due to its ability of solid-state beam steering.

[0003] With the rapid growth of network traffic, the low optical loss, low driving voltage and compact space occupancy of OPA are particularly important. Traditional silicon optical phased arrays use thermo-optical modulation, which consumes a lot of energy and requires high processing precision. In contrast, thin-film lithium niobate (LN) is one of the best materials for realizing high-performance OPA due to its high electro-optical efficiency and low optical loss. In addition, the second-order nonlinear optical coefficient of lithium niobate material itself is large, and electro-optical modulation technology can be used. It has the characteristics of high speed and low energy consumption, and the material cost is relatively low. Therefore, the integrated OPA based on lithium niobate material has obvious advantages in high-speed modulation.

[0004] For the current lithium niobate optical phased array, in order to achieve a wide angle and wide field of view beam scanning range, the spacing between adjacent waveguides is set very small, and due to the low contrast between the core and cladding materials, coupling is very easy to occur between adjacent waveguides, crosstalk is large, and it is difficult to perform independent phase or amplitude control. However, setting the waveguide spacing to 3-4μm to reduce crosstalk will limit the beam scanning angle range. Therefore, there is a strong trade-off between the deflection angle of the beam and the spacing between adjacent waveguides. For small-pitch OPAs, crosstalk is suppressed by reducing the transmission length, and its size is of no value for commercial applications. Therefore, under the premise of narrow spacing between adjacent waveguides and large transmission length, it is of great value to study low-crosstalk OPAs. Summary of the invention

[0005] The object of the present invention is to provide a waveguide array based on lithium niobate and a method for manufacturing the same, which can suppress crosstalk between waveguides in the 1550nm optical band and achieve high transmittance and low insertion loss.

[0006] The technical solution to achieve the above purpose is:

[0007] A waveguide array based on lithium niobate, comprising:

[0008] Silicon-based substrate;

[0009] a silicon dioxide buffer layer deposited on the silicon-based substrate;

[0010] a core layer located on the silicon dioxide buffer layer; and

[0011] A silicon dioxide cladding layer located on the core layer and covering the core layer;

[0012] Wherein, the core layer comprises: two left-right symmetrical lithium niobate wide waveguides, a first lithium niobate grating and a second lithium niobate grating;

[0013] The first lithium niobate grating and the second lithium niobate grating are located between the two lithium niobate wide waveguides; the first lithium niobate grating is located on the left side of the second lithium niobate grating.

[0014] Preferably, the lithium niobate wide waveguide is a straight waveguide with a width of 0.5 μm and a height of 0.3 μm, and the gap between two lithium niobate wide waveguides is 1.46 μm.

[0015] Preferably, the core layer further comprises: a lithium niobate film located on the silicon dioxide buffer layer and below the lithium niobate wide waveguide, the first lithium niobate grating and the second lithium niobate grating, wherein the thickness of the lithium niobate film is 0.1 μm.

[0016] Preferably, the period of the first lithium niobate grating is 0.35-0.45 μm, the duty cycle is 0.85-0.95, the width is 0.24-0.28 μm, the number of gratings is 250, and the distance between the first lithium niobate grating and the left lithium niobate wide waveguide is 0-0.05 μm;

[0017] The period of the second lithium niobate grating is 0.8-0.9 μm, the duty cycle is 0.15-0.25, the width is 0.05-0.15 μm, the number of gratings is 150, and the distance between the second lithium niobate grating and the right lithium niobate wide waveguide is 0.4-0.45 μm;

[0018] The spacing between the first lithium niobate grating and the second lithium niobate grating is 0.14-0.18 μm.

[0019] Preferably, it also includes a metal electrode attached to the silicon dioxide cladding.

[0020] The method for manufacturing the waveguide array based on lithium niobate of the present invention comprises:

[0021] Step 1, depositing a silicon dioxide buffer layer on a silicon-based substrate, and depositing a lithium niobate layer on the silicon dioxide buffer layer;

[0022] Step 2: Add photoresist on the lithium niobate layer, apply a mask to perform electron beam lithography, bombard the lithium niobate layer with argon ions to perform plasma etching and monitor the etching depth in real time to form a core layer;

[0023] Step 3, cleaning the surface of the core layer by wet chemical process to remove impurities on the surface of lithium niobate;

[0024] Step 4, depositing a silicon dioxide cladding layer on the core layer using a plasma enhanced chemical vapor deposition method;

[0025] Step five: perform mask photolithography, and use corresponding photoresist drying process and metal stripping technology to attach the metal electrode to the silicon dioxide cladding.

[0026] The beneficial effects of the present invention are as follows: 1) The present invention has a compact structure, and the manufacturing process is compatible with semiconductor processing technology. Lithium niobate material has a wide transparent window, low absorption loss, high nonlinear optical coefficient and excellent electro-optical modulation characteristics, high modulation efficiency, low energy consumption, and can be produced in large quantities at low cost; 2) The device can be expanded to an 8-waveguide phased array, achieving a millimeter-level transmission length and low crosstalk, which is meaningful for practical applications; 3) The present invention can suppress crosstalk between waveguides in the 1550nm optical band, achieve high transmittance and low insertion loss, which has important application prospects in the fields of optical phased arrays and optical communications; 4) The present invention still maintains low insertion loss and crosstalk in the wavelength range of 1520-1600nm, and the bandwidth reaches 80nm; 5) In terms of beam deflection, an angle of about ±45° can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a cross-sectional view of a waveguide array based on lithium niobate of the present invention;

[0028] Figure 2 is a structural diagram of the core layer in the present invention;

[0029] Figure 3 The present invention uses simulation software based on the finite difference time domain method to simulate the field distribution diagram of TE mode light incident when the central wavelength is 1550nm and the light beam is transmitted only between the lithium niobate wide waveguide;

[0030] Figure 4 The present invention uses simulation software based on the finite difference time domain method to simulate the field distribution diagram of the light transmitted between the lithium niobate array waveguides when the central wavelength is 1550nm and the TE mode light is incident;

[0031] Figure 5 The present invention uses simulation software based on the finite difference time domain method to simulate the field distribution diagram of TE mode light incident when the central wavelength is 1550nm and the light beam is transmitted only between eight lithium niobate wide waveguides;

[0032] Figure 6 The present invention uses simulation software based on the finite difference time domain method to simulate the field distribution diagram of the light transmitted between eight lithium niobate array waveguides when the central wavelength is 1550nm and the TE mode light is incident;

[0033] Figure 7This is a far-field beam scanning range diagram at a wavelength of 1550nm using simulation software based on the finite-difference time-domain method of the present invention;

[0034] Figure 8 The figure is a flow chart of the production of the waveguide array based on lithium niobate of the present invention. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with the accompanying drawings.

[0036] See also Figure 1-2 The lithium niobate-based waveguide array of the present invention includes: a silicon-based substrate 1, a silicon dioxide buffer layer 2, a core layer 3 and a silicon dioxide cladding layer 4.

[0037] The silicon dioxide buffer layer 2 is deposited on the silicon-based substrate 1. The core layer 3 is located on the silicon dioxide buffer layer 2. The silicon dioxide cladding layer 4 is located on the core layer 3 and covers the core layer 3. The core layer 3 includes: two left-right symmetrical lithium niobate wide waveguides 31, a first lithium niobate grating 32 and a second lithium niobate grating 33.

[0038] The first lithium niobate grating 32 and the second lithium niobate grating 33 are located between the two lithium niobate wide waveguides 31 ; the first lithium niobate grating 32 is located on the left side of the second lithium niobate grating 33 .

[0039] When the wavelength of the present invention is 1550nm, the TE polarized light source reaches the coupling waveguide (two lithium niobate wide waveguides 31) through the designed lithium niobate straight waveguide. By adding a grating structure (a first lithium niobate grating 32 and a second lithium niobate grating 33) therebetween, the coupling between the waveguides is suppressed, thereby achieving the function of reducing the crosstalk between the array waveguides.

[0040] After tests and multiple calculations, in this embodiment, the lithium niobate wide waveguide 31 is a straight waveguide with a width of 0.5 μm and a height of 0.3 μm, and the gap between two lithium niobate wide waveguides 31 is 1.46 μm. The length of the lithium niobate wide waveguide 31 is 100 μm.

[0041] The core layer 3 further includes: a lithium niobate film located on the silicon dioxide buffer layer 2 and below the lithium niobate wide waveguide 31 , the first lithium niobate grating 32 and the second lithium niobate grating 33 , wherein the thickness of the lithium niobate film is 0.1 μm.

[0042] The period of the first lithium niobate grating 32 is 0.4μm, the duty cycle is 0.9, the width is 0.26μm, the number of gratings is 250, and the distance between the first lithium niobate grating 32 and the left lithium niobate wide waveguide 31 is 0μm; the period of the second lithium niobate grating 33 is 0.85μm, the duty cycle is 0.2, the width is 0.1μm, the number of gratings is 150, and the distance between the second lithium niobate grating 33 and the right lithium niobate wide waveguide 31 is 0.44μm; the spacing between the first lithium niobate grating 32 and the second lithium niobate grating 33 is 0.16μm. Two grating structures with different parameters are added to produce a larger mode mismatch between the waveguides and suppress the coupling between the waveguides. A metal electrode 5 is added to the silicon dioxide cladding 4.

[0043] like Figure 8 As shown, the manufacturing method of the waveguide array based on lithium niobate as described above of the present invention comprises the following steps:

[0044] Step 1: deposit a silicon dioxide buffer layer 2 on a silicon-based substrate 1, and deposit a lithium niobate layer on the silicon dioxide buffer layer 2; the thickness of the silicon dioxide buffer layer 2 can be set to 2 μm. The thickness of the lithium niobate layer is set to 400 nm.

[0045] Step 2: Add photoresist on the lithium niobate layer, then place a mask on it for electron beam lithography (EBL), then bombard the lithium niobate layer with argon ions (Ar+) for plasma etching (RIE) and monitor the etching depth in real time to form a core layer 3;

[0046] Step 3, performing a wet chemical process (RCA) cleaning on the surface of the core layer 3 to remove impurities on the surface of the lithium niobate;

[0047] Step 4, depositing a silicon dioxide cladding layer 4 on the core layer 3 using a plasma enhanced chemical vapor deposition method (PECVD);

[0048] Step five: perform mask photolithography, and use corresponding photoresist drying process and metal stripping technology to attach the metal electrode 5 to the silicon dioxide cladding layer 4.

[0049] like Figure 3 The present invention uses simulation software based on the finite difference time domain method to simulate the field distribution diagram of light transmission between lithium niobate wide waveguides when TE mode light is incident at a central wavelength of 1550nm.

[0050] like Figure 4 The present invention uses simulation software based on the finite difference time domain method to simulate the field distribution diagram of light transmission between lithium niobate array waveguides when TE mode light is incident at a central wavelength of 1550nm.

[0051] like Figure 5The present invention uses simulation software based on the finite-difference time-domain method to simulate the field distribution diagram of TE mode light incident when the central wavelength is 1550nm and the light beam is transmitted only between eight lithium niobate wide waveguides.

[0052] like Figure 6 The present invention uses simulation software based on the finite difference time domain method to simulate the field distribution diagram of TE mode light incident and light transmitted between eight lithium niobate array waveguides when the central wavelength is 1550nm.

[0053] like Figure 7 This is a far-field beam scanning range diagram at a wavelength of 1550nm using simulation software based on the finite-difference time-domain method of the present invention. The beam deflection can achieve an angle of ±45°.

[0054] In the present invention, the spacing between adjacent lithium niobate wide waveguides is less than one wavelength. It contains only two basic repeating elements, namely a pair of basic phase-mismatched lithium niobate wide waveguides, which have exactly the same width, but have two asymmetrically placed lithium niobate gratings in the gap. When the two lithium niobate gratings are in the correct position, the change in the mode refractive index will cause a strong phase mismatch, thereby suppressing the power transmission between the waveguides. The asymmetric placement of these lithium niobate gratings also helps to expand this nanostructured dual waveguide design, forming a low-crosstalk lithium niobate waveguide array by alternately flipping the positions of the two lithium niobate gratings in the gap of the waveguide array. Theoretical studies of the present invention show that at a wavelength of 1550nm, for TE (transverse electric mode) polarized light, this array exhibits a peak crosstalk of -20.96dB and an insertion loss (IL) of -0.3dB between the nearest neighbor waveguides at a length of 200μm. In addition, the present invention can achieve an angle of ±45° in terms of beam deflection. This opens up opportunities for solid-state laser radar applications with a wide field of view scanning range.

[0055] The above embodiments are only used to illustrate the present invention, rather than to limit the present invention. Those skilled in the relevant technical field may make various changes or modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions should also belong to the scope of the present invention and should be defined by the claims.

Claims

1. A waveguide array based on lithium niobate, characterized in that: include: Silicon-based substrate; a silicon dioxide buffer layer deposited on the silicon-based substrate; a core layer located on the silicon dioxide buffer layer; as well as A silicon dioxide cladding layer located on the core layer and covering the core layer; Wherein, the core layer comprises: two left-right symmetrical lithium niobate wide waveguides, a first lithium niobate grating and a second lithium niobate grating; The first lithium niobate grating and the second lithium niobate grating are located between the two lithium niobate wide waveguides; the first lithium niobate grating is located on the left side of the second lithium niobate grating; the lithium niobate wide waveguide is a straight waveguide with a width of 0.5 μm and a height of 0.3 μm, and the gap between the two lithium niobate wide waveguides is 1.46 μm; The period of the first lithium niobate grating is 0.35-0.45 μm, the duty cycle is 0.85-0.95, the width is 0.24-0.28 μm, the number of gratings is 250, and the distance between the first lithium niobate grating and the left lithium niobate wide waveguide is 0-0.05 μm; The period of the second lithium niobate grating is 0.8-0.9 μm, the duty cycle is 0.15-0.25, the width is 0.05-0.15 μm, the number of gratings is 150, and the distance between the second lithium niobate grating and the right lithium niobate wide waveguide is 0.4-0.45 μm; The spacing between the first lithium niobate grating and the second lithium niobate grating is 0.14-0.18 μm.

2. The lithium niobate based waveguide array according to claim 1, characterized in that: The core layer further includes: a lithium niobate film located on the silicon dioxide buffer layer and below the lithium niobate wide waveguide, the first lithium niobate grating and the second lithium niobate grating, wherein the thickness of the lithium niobate film is 0.1 μm.

3. The lithium niobate based waveguide array according to claim 1, characterized in that: Also included is a metal electrode attached to the silicon dioxide cladding.

4. A method for manufacturing a waveguide array based on lithium niobate as claimed in claim 1, characterized in that: include: Step 1, depositing a silicon dioxide buffer layer on a silicon-based substrate, and depositing a lithium niobate layer on the silicon dioxide buffer layer; Step 2: Add photoresist on the lithium niobate layer, apply a mask to perform electron beam lithography, bombard the lithium niobate layer with argon ions to perform plasma etching and monitor the etching depth in real time to form a core layer; Step 3, cleaning the surface of the core layer by wet chemical process to remove impurities on the surface of lithium niobate; Step 4, depositing a silicon dioxide cladding layer on the core layer using a plasma enhanced chemical vapor deposition method; Step five: perform mask photolithography, and use corresponding photoresist drying process and metal stripping technology to attach the metal electrode to the silicon dioxide cladding.