Adhesive composition, adhesive layer and protective film
By using an adhesive composition containing alkyl (meth)acrylate, a nitrogen-containing monomer and an oxyalkylene chain-containing acrylic polymer and a cross-linking agent, the bonding force under high temperature and high humidity conditions is solved. rise and contamination issues, achieving low contamination and high bonding stability under more severe conditions.
Patent Information
- Application Number
- CN202011084302.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-17
- Filing Date
- 2020-10-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-10-12
AI Technical Summary
In the processing of electronic equipment, it is difficult for existing adhesive sheets to maintain low adhesion and prevent contamination of the surface of the adherend under high temperature and high humidity conditions.
Using an acrylic polymer containing an alkyl (meth)acrylate, a nitrogen-containing monomer and an oxygen-containing alkylene chain as an adhesive composition, combined with a cross-linking agent, the adhesive formed has excellent Thermal stability and low contamination properties.
Even under high-temperature and high-humidity conditions, there is little increase in adhesion, and there is little surface contamination of the adherend after it peels off, meeting more stringent processing requirements.
Smart Images

Figure BDA0002719819820000041 
Figure BDA0002719819820000151 
Figure BDA0002719819820000161
Abstract
Description
Technical Field
[0001] The invention relates to an adhesive composition, an adhesive layer and a protective film. Background Art
[0002] PSA sheets are used in various fields such as automobiles, construction, and electronic devices. In particular, in recent years, they have been effectively used in various occasions such as surface protection of portable electronic devices such as tablets and smartphones, fixing of components, and protection of components used during processing steps.
[0003] As such adhesive sheets, for example, the following items have been proposed: a transparent adhesive film using a polymer comprising units derived from an alkyl (meth)acrylate and a monomer having a saturated cyclic group (Patent Document 1); an adhesive using an acrylic polymer formed from an alkyl (meth)acrylate monomer, a (meth)acrylate monomer having an aromatic group, a nitrogen-containing vinyl monomer having no hydroxyl group, a vinyl monomer having a carboxyl group, and the like (Patent Documents 2 to 7).
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2017-48328
[0007] [Patent Document 2] Japanese Patent Application Publication No. 2019-70148
[0008] [Patent Document 3] Japanese Patent Application Publication No. 2019-70149
[0009] [Patent Document 4] Japanese Patent Publication No. 2019-70152
[0010] [Patent Document 5] Japanese Patent Application Publication No. 2019-77881
[0011] [Patent Document 6] Japanese Patent Publication No. 2019-77882
[0012] [Patent Document 7] Japanese Patent Publication No. 2019-90040 Summary of the invention
[0013] [Problems to be solved by the invention]
[0014] The components used in electronic equipment need to be processed more highly, so they are processed under more severe conditions than before. Therefore, the surface protective film used in the processing steps of these components needs to be cleanly peeled off from the components after the processing steps are completed, even after being exposed to severe conditions such as high temperature. Therefore, in such protective films, it is required that the increase in the adhesive force after the thermal process is small, or the properties of the adherend will not be contaminated by residual glue, etc. when the adhesive sheet is peeled off from the surface of the adherend. However, the adhesive sheets known from the past are sometimes difficult to achieve the above characteristics when placed under more severe processing conditions (high temperature and high humidity).
[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an adhesive and an adhesive tape which have little increase in adhesive strength even when placed under high temperature conditions and little contamination of the adherend surface after peeling from the adherend.
[0016] [Technical means to solve the problem]
[0017] The present inventors have conducted studies and found that, by using an acrylic polymer of a specific composition, it is possible to provide an adhesive having little increase in adhesive strength even when placed under high temperature and high humidity conditions and little contamination of the adherend surface after peeling from the adherend.
[0018] That is, the adhesive composition of the present invention comprises: an acrylic polymer (A) and a crosslinking agent (B), wherein the acrylic polymer (A) comprises a unit derived from an alkyl (meth)acrylate (a1), a unit derived from a nitrogen-containing monomer (a2), and a unit derived from an oxyalkylene chain-containing monomer (a3), and the content of the unit derived from the nitrogen-containing monomer (a2) in the acrylic polymer (A) is 2% by mass or more.
[0019] [Effects of the Invention]
[0020] According to the present invention, it is possible to provide an adhesive and an adhesive tape which have little increase in adhesive strength even when placed under high temperature and high humidity conditions and which have little contamination on the surface of an adherend after peeling from the adherend. DETAILED DESCRIPTION
[0021] The adhesive composition of the present invention comprises an acrylic polymer (A) and a crosslinking agent (B).
[0022] The acrylic polymer (A) includes a unit derived from an alkyl (meth)acrylate (a1), a unit derived from a nitrogen-containing monomer (a2), and a unit derived from an oxyalkylene chain-containing monomer (a3).
[0023] Examples of the (meth)acrylic acid alkyl ester (a1) include (meth)acrylic acid alkyl esters in which an alkyl group is bonded to an ester bond. The number of carbon atoms in the alkyl group is preferably 1 or more, more preferably 3 or more, and further preferably 4 or more, and is preferably 20 or less, more preferably 15 or less, further preferably 12 or less, further more preferably 10 or less, and particularly preferably 8 or less.
[0024] The alkyl (meth)acrylate (a1) preferably contains a monomer whose homopolymer has a glass transition temperature of -15°C or higher. The glass transition temperature of the homopolymer of the alkyl (meth)acrylate (a1) can be, for example, the value described in "POLYMER HANDBOOK THIRD EDITION" (J. BRANDRUP, EH Immergut, 1989, published by John Wiley & Sons, Inc., pages VI / 209 to VI / 277).
[0025] The alkyl (meth)acrylate (a1) is preferably an alkyl (meth)acrylate (a1-1) having an alkyl group having 3 or more (preferably 4 or more) carbon atoms bonded to an ester bond. The content of the alkyl (meth)acrylate (a1-1) is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 70% by mass or more, and preferably 100% by mass or less in the alkyl (meth)acrylate (a1).
[0026] The alkyl (meth)acrylate (a1) preferably further comprises an alkyl (meth)acrylate (a1-2) in which an alkyl group having a carbon number of 2 or less is bonded to an ester bond. When the alkyl (meth)acrylate (a1-2) is contained, the content thereof is preferably 1% by mass or more, more preferably 2% by mass or more, and preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less.
[0027] Examples of the alkyl group include straight-chain alkyl groups such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, lauryl, and stearyl; and branched-chain alkyl groups such as isopropyl, isobutyl, tert-butyl, isopentyl, neopentyl, isohexyl, isoheptyl, isooctyl, 2-ethylhexyl, isononyl, isodecyl, and isostearyl.
[0028] The (meth)acrylic acid alkyl ester (a1) is preferably an acrylate alkyl ester.
[0029] As the alkyl (meth)acrylate (a1), one or more kinds of alkyl (meth)acrylates can be used, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, etc.
[0030] In the acrylic polymer (A), the content of the unit derived from the alkyl (meth)acrylate (a1) is preferably 50% by mass or more, more preferably 60% by mass or more, and is preferably 98% by mass or less, more preferably 95% by mass or less.
[0031] The nitrogen-containing monomer (a2) is a monomer having a nitrogen atom and a polymerizable double bond in the molecule, preferably a monomer having an amide bond and a polymerizable double bond in the molecule, and examples thereof include: lactam compounds having a vinyl group; (meth)acrylamide monomers; (meth)acrylate compounds having a functional group containing a nitrogen atom (e.g., an amino group, a monosubstituted amino group, a disubstituted amino group, a nitrile group, etc.), and the like.
[0032] Examples of the lactam compound having a vinyl group include N-vinyl pyrrolidone and N-vinyl caprolactam.
[0033] Examples of the (meth)acrylamide monomer include compounds in which a hydrogen atom or a hydrocarbon group (preferably an aliphatic hydrocarbon group; wherein -CH2- contained in the hydrocarbon group may be substituted with -CO-, and a hydrogen atom contained in the hydrocarbon group may be substituted with a hydroxyl group) is bonded to a nitrogen atom of (meth)acrylamide, etc. In addition, when two or more groups (the hydrocarbon groups) replace the nitrogen atom of (meth)acrylamide, these groups may be bonded to each other to form a ring containing the nitrogen atom.
[0034] The number of carbon atoms of the hydrocarbon group (preferably an aliphatic hydrocarbon group) substituted on the nitrogen atom contained in the amide bond is preferably 1 or more and preferably 10 or less, more preferably 6 or less.
[0035] As the (meth)acrylamide monomer, one or two or more may be used. The (meth)acrylamide monomer may be any one of (meth)acrylamide, N-1 substituted (meth)acrylamide, and N,N-2 substituted (meth)acrylamide.
[0036] As the (meth)acrylamide monomer, one or more kinds can be used, for example, (meth)acrylamide; N-isopropyl (meth)acrylamide, N-(1,1-dimethyl-3-oxobutyl)acrylamide, N-hydroxymethyl (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-(2-hydroxymethyl)acrylamide, N-(2-hydroxyethyl)acrylamide and other N-1-substituted (meth)acrylamide compounds; N N-2 substituted (meth)acrylamide compounds such as -(meth)acryloylmorpholine, N-(meth)acryloylpiperidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloyl-4-piperidone, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-methylenebis(meth)acrylamide, and N,N-dimethylaminopropyl(meth)acrylamide.
[0037] Among them, the (meth)acrylamide monomer preferably includes a monomer represented by formula (1).
[0038] [Chemistry 1]
[0039]
[0040] [In formula (1), R 1 Represents a hydrogen atom or a methyl group; R 2 and R 3 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, wherein -CH2- contained in the hydrocarbon group may be substituted by -CO- or -O-, and the hydrogen atom contained in the hydrocarbon group may be substituted by a hydroxyl group, R 2 and R 3 may be bonded to each other to form a ring containing a nitrogen atom]
[0041] As the R 2 and R 3 The hydrocarbon group represented may be one or two or more, and examples thereof include a linear or branched saturated aliphatic hydrocarbon group; a linear or branched unsaturated aliphatic hydrocarbon group, and the like.
[0042] The (meth)acrylamide monomer also preferably comprises R 2 and R 3 Both are (meth)acrylamide monomers of the hydrocarbon group. 2 and R 3When both are (meth)acrylamide monomers having hydrocarbon groups, the content of the units derived from the monomers in the acrylic polymer (A) is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less.
[0043] The content of the unit derived from the acrylamide monomer in the nitrogen-containing monomer (a2) is preferably 30% by mass or more, more preferably 60% by mass or more, further preferably 75% by mass or more, and the upper limit is 100% by mass.
[0044] Examples of the (meth)acrylate compound having the functional group containing a nitrogen atom (e.g., an amino group, a monosubstituted amino group, a disubstituted amino group, a nitrile group, etc.) include (meth)acrylonitrile, tert-butylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, etc. Examples of the (meth)acrylate compound having the functional group containing a nitrogen atom include compounds in which the functional group containing a nitrogen atom is bonded to a (meth)acryloyloxy group via a single bond or a hydrocarbon group (preferably an alkyl group) having 1 to 10 carbon atoms (preferably 1 to 5 carbon atoms), etc.
[0045] The nitrogen-containing monomer (a2) preferably includes a nitrogen-containing monomer having a hydroxyl group. As the nitrogen-containing monomer having a hydroxyl group, it is preferably a (meth)acrylamide monomer having a hydroxyl group, and more preferably, in formula (1), R 2 and R 3 At least one of the above is a hydrocarbon group, and a hydrogen atom contained in the hydrocarbon group is substituted with a monomer of a hydroxyl group.
[0046] The content of the nitrogen-containing monomer having a hydroxyl group in the nitrogen-containing monomer (a2) is preferably 50% by mass or more, more preferably 60% by mass or more, and further preferably 65% by mass or more, and is preferably 100% by mass or less, more preferably 95% by mass or less, and further preferably 90% by mass or less.
[0047] In the acrylic polymer, the content of the unit derived from the nitrogen-containing monomer (a2) is preferably 2% by mass or more, more preferably 2.5% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less.
[0048] The monomer (a3) containing an oxyalkylene chain is a monomer having an oxyalkylene unit and a polymerizable double bond in the molecule. The number of carbon atoms in the oxyalkylene unit is preferably 2 or more, and preferably 5 or less, more preferably 4 or less, further preferably 3 or less, and particularly preferably 2. As the monomer containing an oxyalkylene chain, an alkoxy polyalkylene glycol (meth) acrylate is preferred. As the alkoxy group in the alkoxy polyalkylene glycol (meth) acrylate, alkoxy groups having 1 to 5 carbon atoms (preferably 1 to 3) such as methoxy, ethoxy, and propoxy can be cited.
[0049] As the oxyalkylene chain-containing monomer (a3), one or two or more kinds may be used, and examples thereof include methoxyethylene glycol methacrylate and methoxyethylene glycol acrylate.
[0050] The content of alkoxy polyalkylene glycol (meth) acrylate in the oxyalkylene chain-containing monomer (a3) is 0% by mass or more, preferably 10% by mass or more, more preferably 30% by mass or more, and is 100% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less.
[0051] The number of repetitions of the oxyalkylene unit in the oxyalkylene chain-containing monomer (a3) is preferably 2 or more, more preferably 4 or more, and further preferably 5 or more, and is preferably 100 or less, more preferably 30 or less, and further preferably 20 or less.
[0052] In the acrylic polymer (A), the content of the unit derived from the oxyalkylene chain-containing monomer (a3) is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and further preferably 1.5% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and further preferably 15% by mass or less.
[0053] The acrylic polymer (A) may have a unit derived from another monomer (a4) other than the (meth)acrylic acid alkyl ester (a1), the nitrogen-containing monomer (a2), and the oxyalkylene chain-containing monomer (a3).
[0054] As the other monomers (a4), one or more kinds can be used, for example: unsaturated monocarboxylic acids such as (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, and β-carboxyethyl (meth)acrylate; (meth)acrylic acid monomers having a hydroxyl group; (meth)acrylic acid monomers containing an epoxy ring such as glycidyl (meth)acrylate; (meth)acrylic acid monomers containing an alicyclic ring such as cyclohexyl (meth)acrylate; aromatic vinyl monomers such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, ethylvinylbenzene, α-methylstyrene, p-methoxystyrene, p-tert-butylstyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, and p-hydroxystyrene; monomers having two or more vinyl groups, etc.
[0055] Examples of the (meth)acrylic acid monomer having a hydroxyl group include compounds in which a hydroxyl group is bonded to the alkyl group of an alkyl (meth)acrylate, and polyalkylene (meth)acrylate. Preferably, the compound is in which a hydroxyl group is bonded to the alkyl group of an alkyl (meth)acrylate, and more preferably, the compound is in which a hydroxyl group is bonded to the terminal of the alkyl group of an alkyl (meth)acrylate.
[0056] The number of hydroxyl groups contained in the (meth)acrylic acid monomer having a hydroxyl group is preferably one.
[0057] In addition, as the (meth)acrylic acid monomer having a hydroxyl group, an acrylic acid monomer having a hydroxyl group is preferable.
[0058] Examples of the alkyl acrylate include the same compounds as those exemplified as the alkyl (meth)acrylate (a1).
[0059] As the (meth)acrylic acid monomer having a hydroxyl group, one or more kinds can be used, for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; polyethylene glycol (meth)acrylate, etc.
[0060] In the acrylic polymer (A), the content of the unit derived from the (meth)acrylic acid monomer having a hydroxyl group is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and still more preferably 0.03% by mass or more, and is preferably 15% by mass or less, more preferably 12% by mass or less, and still more preferably 10% by mass or less.
[0061] In the acrylic polymer (A), the content of the units derived from other monomers (a4) is 0% by mass or more, more preferably more than 0% by mass, and further preferably 0.01% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less.
[0062] The weight average molecular weight of the acrylic polymer (A) is preferably 100,000 or more, more preferably 200,000 or more, and even more preferably 300,000 or more, and is preferably 2,000,000 or less, more preferably 1,800,000 or less, and even more preferably 1,500,000 or less.
[0063] In the present specification, the number average molecular weight and weight average molecular weight of the acrylic polymer (A) refer to converted values measured by gel permeation chromatography (GPC) using polystyrene as a standard sample.
[0064] In the adhesive composition of the present invention, the content of the acrylic polymer (A) in the nonvolatile component is preferably 15% by mass or more, more preferably 20% by mass or more, further preferably 25% by mass or more, and is preferably 100% by mass or less.
[0065] In this specification, the non-volatile component of the adhesive composition refers to a portion obtained by removing a solvent component that may be contained in the adhesive composition as necessary.
[0066] The acrylic polymer (A) can be produced by copolymerizing the (meth)acrylic acid alkyl ester (a1), the nitrogen-containing monomer (a2), the oxyalkylene chain-containing monomer (a3), and other monomers (a4) as needed in the presence of a polymerization initiator.
[0067] As the polymerization initiator, for example, one or more thermal polymerization initiators may be used, and examples thereof include peroxide initiators such as benzoyl peroxide and lauroyl peroxide; and azo initiators such as azobisisobutyronitrile.
[0068] The adhesive composition of the present invention contains a crosslinking agent (B). As the crosslinking agent, one or more kinds can be used, for example, isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, polyvalent metal salt crosslinking agents, metal chelate crosslinking agents, ketone-hydrazide crosslinking agents, oxazoline crosslinking agents, carbodiimide crosslinking agents, silane crosslinking agents, glycidyl (alkoxy) epoxy silane crosslinking agents, etc. can be listed.
[0069] Among them, isocyanate crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, carbodiimide crosslinking agents, and glycidyl (alkoxy) epoxy silane crosslinking agents are preferred, isocyanate crosslinking agents, epoxy crosslinking agents, and carbodiimide crosslinking agents are more preferred, and isocyanate crosslinking agents are particularly preferred.
[0070] The content of the isocyanate crosslinking agent in the crosslinking agent (B) is preferably 30% by mass or more, more preferably 50% by mass or more, further preferably 80% by mass or more, further more preferably 90% by mass or more, and is preferably 100% by mass or less.
[0071] The content of the crosslinking agent (B) is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A).
[0072] The adhesive composition of the present invention preferably contains a solvent (D). As the solvent (D), one or more kinds of solvents can be used, for example, aromatic hydrocarbon solvents such as toluene and xylene; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone and methyl ethyl ketone; aliphatic hydrocarbon solvents such as hexane, etc. Among them, it is preferred to contain an ester solvent.
[0073] The content of the ester solvent in the solvent (D) is preferably 50% by mass or more, more preferably 80% by mass or more, further preferably 90% by mass or more, and is preferably 100% by mass or less.
[0074] The content of the solvent (D) in the adhesive composition is preferably 10% by mass or more, more preferably 30% by mass or more, and further preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 70% by mass or less, and further preferably 65% by mass or less.
[0075] In the adhesive composition of the present invention, in order to maintain low yellowing, it is preferred to reduce the content of the adhesion imparting resin, preferably less than 10 parts by mass, more preferably 8 parts by mass or less, further preferably 3 parts by mass or less, further more preferably 1 part by mass or less, and preferably 0 parts by mass, relative to 100 parts by mass of the acrylic polymer. By adopting a structure in which an acrylic polymer (A) having a specific composition and a weight average molecular weight is used and no adhesion imparting resin is contained, the low yellowing property of the adhesive layer can be maintained, and even under high temperature / high humidity conditions, high adhesion can be maintained, and migration of the plasticizer can be suppressed.
[0076] The adhesive composition of the present invention may also contain an alkali (ammonia water, etc.) or acid for adjusting the pH value; a foaming agent; a softener; an antioxidant; a filler such as glass or plastic fibers, balloons, beads, metal powder, etc.; a colorant such as a pigment, a dye, etc.; a pH adjuster; a film forming aid; a leveling agent; a thickener; a hydrophobic agent; a defoaming agent; an acid catalyst; an acid generator, etc. as additives.
[0077] The adhesive layer can be formed by applying the adhesive composition on a support and drying the support. The support may be any substrate such as a release sheet or an adhesive sheet.
[0078] As the coating method, a method using a knife coater, a reverse coater, a die coater, a lip die coater, a slot die coater, a gravure coater, a curtain coater or the like can be used.
[0079] The thickness of the adhesive layer is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more, and is preferably 100 μm or less, more preferably 70 μm or less, and even more preferably 50 μm or less.
[0080] The protective film of the present invention has the adhesive layer. The adhesive sheet or adhesive tape of the present invention has the adhesive layer and the substrate. The substrate may be in any shape such as a film, a sheet, a tape, a plate, or a three-dimensional shape. Examples of the material of the substrate include plastics such as polyester resin, polypropylene resin, polyethylene resin, polyimide resin, vinyl chloride resin, and urethane resin; rubber; nonwoven fabric; metal foil; paper, etc., preferably plastic, and more preferably vinyl chloride resin. In addition, the substrate may be a substrate with a smooth surface, or a substrate with an uneven surface such as a fibrous substrate or a foam substrate.
[0081] The thickness of the substrate is preferably 0.1 μm or more and preferably 1,000 μm or less.
[0082] [Example]
[0083] The present invention is described in more detail below with reference to the following embodiments. However, the present invention is not limited to the following embodiments and can be implemented with appropriate modifications within the scope suitable for the above-mentioned and later-mentioned purposes. All of these are included in the technical scope of the present invention.
[0084] [Synthesis example 1]
[0085] <Synthesis of acrylic resin (A1)>
[0086] In a reaction container equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 830 parts by mass of n-butyl acrylate, 50 parts by mass of methyl acrylate, 50 parts by mass of hydroxyethyl acrylamide, 10 parts by mass of acrylamide, 10 parts by mass of NK ester AM-90G (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), 40 parts by mass of NK ester M-90G (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), 10 parts by mass of hydroxyethyl acrylate, and 1000 parts by mass of ethyl acetate were placed, and the mixture was heated to 70° C. while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) dissolved in ethyl acetate in advance (solid content 5%) was added. After maintaining at 70° C. for 8 hours with stirring, the contents were cooled and filtered through a 200-mesh metal mesh to obtain an acrylic resin (A1) having a nonvolatile content of 50% by mass, a viscosity of 100,000 mPa·s, and a weight average molecular weight of 500,000.
[0087] [Synthesis example 2]
[0088] <Synthesis of acrylic resin (A2)>
[0089] In a reaction container equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 735 parts by mass of n-butyl acrylate, 100 parts by mass of 2-ethylhexyl acrylate, 50 parts by mass of methyl acrylate, 20 parts by mass of acryloylmorpholine, 50 parts by mass of hydroxyethylacrylamide, 20 parts by mass of NK ester AM-90G, 20 parts by mass of NK ester M-90G, 5 parts by mass of hydroxyethyl methacrylate, and 1000 parts by mass of ethyl acetate were placed, and the mixture was heated to 70° C. while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) previously dissolved in ethyl acetate was added. After being kept at 70° C. for 8 hours with stirring, the content was cooled and filtered through a 200-mesh metal mesh to obtain an acrylic resin (A2) having a nonvolatile content of 50% by mass, a viscosity of 80,000 mPa·s, and a weight average molecular weight of 450,000.
[0090] [Synthesis example 3]
[0091] <Synthesis of acrylic resin (A3)>
[0092] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 400 parts by mass of n-butyl acrylate, 310 parts by mass of 2-ethylhexyl acrylate, 100 parts by mass of methyl acrylate, 100 parts by mass of hydroxyethyl acrylamide, 20 parts by mass of dimethyl acrylamide, 40 parts by mass of NK ester AM-130G (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), 30 parts by mass of 4-hydroxybutyl acrylate, and 1000 parts by mass of ethyl acetate were placed, and the mixture was heated to 70°C while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) dissolved in ethyl acetate in advance (solid content 5%) was added. After that, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered through a 200-mesh metal mesh to obtain an acrylic resin (A3) having a non-volatile content of 50% by mass, a viscosity of 120,000 mPa·s, and a weight average molecular weight of 440,000.
[0093] [Synthesis Example 4]
[0094] <Synthesis of acrylic resin (A4)>
[0095] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 825 parts by mass of n-butyl acrylate, 50 parts by mass of methyl acrylate, 20 parts by mass of acryloylmorpholine, 50 parts by mass of dimethylacrylamide, 50 parts by mass of NK ester M-230G (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), 5 parts by mass of 4-hydroxybutyl acrylate, and 1000 parts by mass of ethyl acetate were placed, and the mixture was heated to 70°C while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. Thereafter, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered using a 200-mesh metal mesh to obtain an acrylic resin (A4) having a non-volatile content of 50% by mass, a viscosity of 150,000 mPa·s, and a weight average molecular weight of 650,000.
[0096] [Synthesis example 5]
[0097] <Synthesis of acrylic resin (A5)>
[0098] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 710 parts by mass of 2-ethylhexyl acrylate, 150 parts by mass of methyl acrylate, 50 parts by mass of hydroxyethyl acrylamide, 20 parts by mass of NK ester AM-130G, 20 parts by mass of NK ester M-90G, 50 parts by mass of hydroxyethyl acrylate, and 1000 parts by mass of ethyl acetate were placed, and the mixture was heated to 70°C while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. Thereafter, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered through a 200-mesh metal mesh to obtain an acrylic resin (A5) having a non-volatile content of 50% by mass, a viscosity of 110,000 mPa·s, and a weight average molecular weight of 550,000.
[0099] [Synthesis example 6]
[0100] <Synthesis of acrylic resin (A6)>
[0101] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 875 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of acryloylmorpholine, 40 parts by mass of acrylamide, 50 parts by mass of NK ester AM-90G, 10 parts by mass of hydroxyethyl methacrylate, 5 parts by mass of acrylic acid, and 1000 parts by mass of ethyl acetate were added, and the mixture was heated to 70°C while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. Thereafter, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered using a 200-mesh metal mesh to obtain an acrylic resin (A6) having a non-volatile content of 50% by mass, a viscosity of 90,000 mPa·s, and a weight average molecular weight of 420,000.
[0102] [Synthesis Example 7]
[0103] <Synthesis of acrylic resin (A7)>
[0104] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 270 parts by mass of n-butyl acrylate, 400 parts by mass of 2-ethylhexyl acrylate, 50 parts by mass of hydroxyethyl acrylamide, 20 parts by mass of dimethyl acrylamide, 120 parts by mass of NK ester M-90G, 40 parts by mass of 4-hydroxybutyl acrylate, 100 parts by mass of cyclohexyl acrylate, and 1000 parts by mass of ethyl acetate were added, and the temperature was raised to 70°C while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. Thereafter, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered using a 200-mesh metal mesh to obtain an acrylic resin (A7) having a non-volatile content of 50% by mass, a viscosity of 80,000 mPa·s, and a weight average molecular weight of 400,000.
[0105] [Synthesis example 8]
[0106] <Comparative Synthesis of Acrylic Resin (A1')>
[0107] In a reaction vessel including a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 50 parts by mass of n-butyl acrylate, 670 parts by mass of 2-ethylhexyl acrylate, 210 parts by mass of methyl acrylate, 60 parts by mass of 4-hydroxybutyl acrylate, 10 parts by mass of acrylic acid, and 1000 parts by mass of ethyl acetate were added, and the temperature was raised to 70°C while blowing nitrogen gas under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. Thereafter, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered using a 200-mesh metal mesh to obtain a comparative acrylic resin (A1') having a non-volatile component of 50% by mass, a viscosity of 130,000 mPa·s, and a weight average molecular weight of 650,000.
[0108] [Synthesis Example 9]
[0109] <Comparative Synthesis of Acrylic Resin (A2')>
[0110] In a reaction vessel including a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 300 parts by mass of n-butyl acrylate, 350 parts by mass of 2-ethylhexyl acrylate, 150 parts by mass of methyl acrylate, 100 parts by mass of dimethyl acrylamide, 100 parts by mass of hydroxyethyl acrylate, and 1000 parts by mass of ethyl acetate were added, and the temperature was raised to 70°C while blowing nitrogen gas under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. Thereafter, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered using a 200-mesh metal mesh to obtain a comparative acrylic resin (A2') having a non-volatile component of 50% by mass, a viscosity of 110,000 mPa·s, and a weight average molecular weight of 550,000.
[0111] [Synthesis Example 10]
[0112] <Comparative Synthesis of Acrylic Resin (A3')>
[0113] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 790 parts by mass of 2-ethylhexyl acrylate, 150 parts by mass of NK ester AM-90G, 50 parts by mass of hydroxyethyl methacrylate, 10 parts by mass of acrylic acid, and 1000 parts by mass of ethyl acetate were added, and the temperature was raised to 70°C while blowing nitrogen gas under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. Thereafter, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered using a 200-mesh metal mesh to obtain a comparative acrylic resin (A3') having a non-volatile content of 50% by mass, a viscosity of 110,000 mPa·s, and a weight average molecular weight of 520,000.
[0114] [Synthesis Example 11]
[0115] <Comparative Synthesis of Acrylic Resin (A4')>
[0116] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 700 parts by mass of n-butyl acrylate, 100 parts by mass of 2-ethylhexyl acrylate, 15 parts by mass of acryloyl morpholine, 50 parts by mass of NK ester AM-130G, 50 parts by mass of NK ester M-90G, 80 parts by mass of 4-hydroxybutyl acrylate, 5 parts by mass of acrylic acid, and 1000 parts by mass of ethyl acetate were added, and the mixture was heated to 70°C while nitrogen was blown in under stirring. After 1 hour, 10 parts by mass of a 2,2'-azobis(2-methylbutyronitrile) solution (solid content 5%) preliminarily dissolved in ethyl acetate was added. After that, the mixture was kept at 70°C for 8 hours under stirring, and the contents were cooled and filtered using a 200-mesh metal mesh to obtain a comparative acrylic resin (A4') having a non-volatile content of 50% by mass, a viscosity of 100,000 mPa·s, and a weight average molecular weight of 490,000.
[0117] [Example 1]
[0118] 4 parts by mass of an isocyanate crosslinking agent (Finetack hardener D-40; manufactured by DIC Corporation) was stirred and mixed with 100 parts by mass of the acrylic resin (A1) obtained in Synthesis Example 1 so as to be uniform, thereby obtaining an acrylic adhesive composition (1).
[0119] [Example 2 to Example 7, Comparative Example 1 to Comparative Example 4]
[0120] Acrylic adhesive compositions (2) to (7) and comparative acrylic adhesive compositions (1') to (4') were obtained in the same manner as in Example 1, except that 100 parts by mass of acrylic resin (A2) to (A7) or comparative acrylic resin (A1') to (A4') were used instead of 100 parts by mass of acrylic resin (A1).
[0121] [Adhesive film processing method]
[0122] The acrylic adhesive compositions and comparative acrylic adhesive compositions obtained in Examples 1 to 7 and Comparative Examples 1 to 4 were applied to the surface of a 50 μm thick polyethylene terephthalate film (release PET50) with a release treatment so that the film thickness after solvent drying was 12 μm. After the solvent was volatilized in a dryer at 80° C. for 3 minutes, a PET 38 μm film was attached.
[0123] [Measurement method of adhesive strength]
[0124] The adhesive film prepared by the above method was cut into 25 mm wide pieces, and the obtained article was used as a test piece. The adherend was set as a glass plate, and it was attached to the adherend by 2 kg roller × 2 round trips. After 1 hour of attachment, the 180 degree peel strength was measured at a peeling speed of 300 mm / min under an environment of 23°C and 50% RH, and was used as the adhesive strength.
[0125] [Method for measuring adhesive strength after heat resistance]
[0126] The test piece was attached to the adherend in the same manner as the above-mentioned adhesive strength measurement method. After that, it was placed in a 140°C environment for 1 hour and then removed. After being placed in a 23°C, 50% RH environment for 30 minutes, the 180-degree peel strength was measured at a peeling speed of 300 mm / min and was taken as the adhesive strength after heat resistance.
[0127] [Evaluation method for contamination of adherends]
[0128] The test piece was attached to the adherend in the same manner as the above-mentioned method for measuring the adhesive force. After that, it was placed in an environment of 60°C and 90% RH for 3 days and then removed. After being placed in an environment of 23°C and 50% RH for 30 minutes, the test piece was peeled off and the peeled adherend surface (the part where the adhesive force was attached) was irradiated with a light emitting diode (LED) to confirm whether the adherend surface was contaminated or not, which was used as an evaluation of contamination resistance.
[0129] 0:No pollution
[0130] △: There is no adhesive left on the surface of the adherend, but there are white marks
[0131] ×: Adhesive remains on the adherend surface
[0132] The results are shown in Tables 1 and 2.
[0133] [Table 1]
[0134]
[0135] [Table 2]
[0136]
[0137] Examples 1 to 7 are examples of the present invention, and even after being placed under high temperature conditions, the increase in adhesive force is small, and the surface of the adherend after peeling off from the adherend is less contaminated. Comparative Example 1 is an example of a monomer that does not contain a nitrogen-containing monomer and an oxyalkylene chain. After being placed under high temperature conditions, the adhesive force increases, and after being placed under high temperature and high humidity conditions, the adhesive residue is confirmed on the surface of the adherend. Comparative Example 2 is an example of a monomer that does not contain an oxyalkylene chain. After being placed under high temperature conditions, the adhesive force increases, and after being placed under high temperature and high humidity conditions, the adhesive residue is confirmed on the surface of the adherend. Comparative Example 3 is an example that does not contain a nitrogen-containing monomer. After being placed under high temperature conditions, the adhesive force increases, and after being placed under high temperature and high humidity conditions, the adhesive residue is confirmed on the surface of the adherend. Comparative Example 4 is an example in which the content of units derived from nitrogen-containing monomers (a2) is less than 2% by mass. After being placed under high temperature conditions, the adhesive force increases, and after being placed under high temperature and high humidity conditions, the adhesive residue is confirmed on the surface of the adherend.
Claims
1. An adhesive composition comprising: an acrylic polymer (A) and a crosslinking agent (B), The acrylic polymer (A) comprises a unit derived from an alkyl (meth)acrylate (a1), a unit derived from a nitrogen-containing monomer (a2), and a unit of an alkoxy polyalkylene glycol (meth)acrylate (a3), wherein the alkoxy group in the alkoxy polyalkylene glycol (meth)acrylate is an alkoxy group having 1 to 5 carbon atoms, The (meth)acrylic acid alkyl ester (a1) comprises a monomer whose homopolymer has a glass transition temperature of -15°C or higher. The nitrogen-containing monomer (a2) includes a nitrogen-containing monomer (a2-1) having a hydroxyl group and a nitrogen-containing monomer (a2-2) not having a hydroxyl group. The content of the unit derived from the nitrogen-containing monomer (a2) in the acrylic polymer (A) is 2% by mass or more. 2 . The adhesive composition according to claim 1 , wherein the nitrogen-containing monomer (a2) is a (meth)acrylamide monomer. 3 . An adhesive layer formed from the adhesive composition according to claim 1 or 2 . A protective film comprising the adhesive layer according to claim 3 .