Positive electrode active material for secondary battery and secondary battery

By using specific positive active materials and aqueous electrolytes in secondary batteries, combined with appropriate lithium salts and additives, the problem of unstable lithium ion absorption and detachment in secondary batteries in aqueous solutions is solved, and the durability of the battery is improved. and safety, inhibiting battery deterioration during charging and storage.

CN112689917BActive Publication Date: 2024-10-29PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN201980059039.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-25
Publication Date
2024-10-29
Estimated Expiration
2039-07-25

AI Technical Summary

Technical Problem

When existing secondary batteries use aqueous solutions as electrolytes, it is difficult to stably absorb and detach lithium ions within the potential range where water electrolysis reactions do not occur, resulting in battery degradation during charging and storage.

Method used

The specific cathode active material LiaNixCoyMnzMbO2 is used, combined with an aqueous electrolyte and appropriate lithium salts and additives. By controlling the ratio of water and lithium salts and the content of additives, battery degradation during charging and storage is suppressed.

Benefits of technology

It effectively expands the potential area where electrolysis does not occur, improves the durability and safety of secondary batteries, and suppresses battery degradation during charging and storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112689917B_ABST
    Figure CN112689917B_ABST
Patent Text Reader

Abstract

The positive electrode active material is a general formula Li a Ni x Co y Mn z M b O2 means, and satisfies 0.9
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a positive electrode active material for a secondary battery and a secondary battery. Background Art

[0002] It is known that secondary batteries using aqueous solutions are used as electrolytes. Secondary batteries using aqueous solutions as electrolytes are required to be used within a potential range where no electrolysis reaction of water occurs. It is necessary to use an active material that is stable in an aqueous solution and can reversibly absorb and detach a large amount of lithium within a potential range where oxygen and hydrogen are not produced by the electrolysis of water. In other words, it is necessary to use an active material that can exert a large capacity within a specific potential range. In addition, as an electrolyte, it is desirable to use a neutral to alkaline electrolyte. When using a neutral, i.e., pH=7 electrolyte, the decomposition voltage of water is as follows: the hydrogen evolution potential is 2.62V and the oxygen evolution potential is 3.85V. In addition, when using a strongly alkaline, i.e., pH=14 electrolyte, the decomposition voltage of water is as follows: the hydrogen evolution potential is 2.21V and the oxygen evolution potential is 3.44V.

[0003] Therefore, as a positive electrode active material, a material that can absorb more Li up to a minimum of 3.85 V (pH=7) is desired, and as a negative electrode active material, a material that can absorb more Li up to 2.21 V (pH=14) is desired.

[0004] Patent Document 1 describes a positive electrode active material having the general formula Li s Ni x Co y Mn z M t A layered structure compound represented by O2 (0.9≤s≤1.2, 0.25≤x≤0.4, 0.25≤y≤0.4, 0.25≤z≤0.4, 0≤t≤0.25; M is one or more selected from Mg, Al, Fe, Ti, Ga, Cu, V and Nb) is used as the main component.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 4581524 Summary of the invention

[0008] For secondary batteries using an aqueous solution as an electrolyte, a technology is required that can expand the potential region where electrolysis does not occur and improve the durability, that is, suppress battery degradation during charged storage.

[0009] The present application relates to a secondary battery using an aqueous solution as an electrolyte, and an object of the present application is to provide a positive electrode active material for a secondary battery and a secondary battery capable of suppressing battery degradation during charged storage.

[0010] A secondary battery positive electrode active material according to one embodiment of the present invention is a secondary battery positive electrode active material having an electrolyte solution prepared by dissolving a lithium salt in water. The positive electrode active material is a secondary battery having a general formula Li a Ni x Co y Mn z M b O2 represents and satisfies:

[0011] 0.9 <a<1.1、

[0012] 0.4≤x<1.0,

[0013] 0≤y<0.4,

[0014] 0≤z<0.4,

[0015] 0≤b<0.2,

[0016] 0.9<(x+y+z+b)<1.1 composite oxide,

[0017] The element M includes at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Ga, and In, and the ratio (B / A) of the BET specific surface area (B) of the composite oxide particles after the particle compression test to the BET specific surface area (A) before the particle compression test is greater than 1.0 and less than 3.0.

[0018] According to the present application, it is possible to suppress battery degradation during charged storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a diagram for explaining the function of the implementation method. DETAILED DESCRIPTION

[0020] As a result of intensive studies, the present inventors have found that deterioration of a secondary battery during charged storage can be suppressed by using a specific material as a positive electrode active material in an electrolyte solution containing water as a solvent and a lithium salt as an electrolyte salt.

[0021] Hereinafter, an embodiment of a positive electrode active material and a secondary battery according to one embodiment of the present application will be described. However, the embodiment described below is an example, and the present application is not limited thereto.

[0022] [Aqueous electrolyte]

[0023] The aqueous electrolyte described in this embodiment contains at least water and a lithium salt. It should be noted that when using an electrolyte containing water as a solvent, since water theoretically decomposes at a voltage of 1.23V, it is also desired to develop a secondary battery that can work stably without decomposing water even when a higher voltage is applied.

[0024] (Solvent)

[0025] The aqueous electrolyte contains water as the main solvent. Here, containing water as the main solvent means that the content of water is 50% or more by volume relative to the total amount of solvent contained in the electrolyte. The content of water contained in the electrolyte is preferably 90% or more by volume relative to the total amount of solvent. The solvent contained in the electrolyte can be a mixed solvent containing water and a non-aqueous solvent. Examples of the non-aqueous solvent include alcohols such as methanol; carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethylene carbonate, and propylene carbonate; acetone; acetonitrile; and non-protonic polar solvents such as dimethyl sulfoxide.

[0026] The aqueous electrolyte contains non-flammable water as the main solvent, so the safety of the secondary battery using the aqueous electrolyte can be improved. From this viewpoint, the content of water is preferably 8% by mass or more, more preferably 10% by mass or more relative to the total amount of the electrolyte. In addition, the content of water is preferably 50% by mass or less, more preferably 20% by mass or less relative to the total amount of the electrolyte.

[0027] (Lithium Salt)

[0028] The lithium salt contained in the aqueous electrolyte can be used as long as it is a compound that can be dissolved in a solvent containing water and dissociated so that lithium ions are present in the aqueous electrolyte. The lithium salt preferably does not cause deterioration of battery characteristics due to its reaction with the materials constituting the positive electrode and the negative electrode. Examples of such lithium salts include salts formed with inorganic acids such as perchloric acid, sulfuric acid and nitric acid; salts formed with halide ions such as chloride ions and bromide ions; and salts formed with organic anions containing carbon atoms in the structure.

[0029] Examples of the organic anions constituting the lithium salt include anions represented by the following general formulae (i) to (iii).

[0030] (R 1 SO2)(R 2 SO2)N - (i)

[0031] (R 1 , R 2 R is independently selected from a halogen atom, an alkyl group or a halogen-substituted alkyl group. 1 and R 2 They are optionally bonded to each other to form a ring.)

[0032] R 3 SO3 - (ii)

[0033] (R 3 is selected from a halogen atom, an alkyl group or a halogen-substituted alkyl group. )

[0034] R 4 CO2 - (iii)

[0035] (R 4 is selected from alkyl or halogen-substituted alkyl. )

[0036] In the above general formulae (i) to (iii), the number of carbon atoms in the alkyl group or the halogen-substituted alkyl group is preferably 1 to 6, more preferably 1 to 3, and even more preferably 1 to 2. The halogen in the halogen-substituted alkyl group is preferably fluorine. The number of halogen substitutions in the halogen-substituted alkyl group is less than the number of hydrogen atoms in the original alkyl group. The halogen atom in the above general formulae (i) to (ii) is preferably a fluorine atom.

[0037] R 1 ~R 4 are, for example, saturated alkyl or saturated halogen-substituted alkyl and R 1 ~R 2 When they are not bonded to each other to form a ring, they may be a group represented by the following general formula (iv).

[0038] C n H a F b Cl c Br d I e (iv)

[0039] (n is an integer greater than or equal to 1, a, b, c, d, and e are integers greater than or equal to 0, and 2n+1=a+b+c+d+e is satisfied.)

[0040] In the above general formula (iv), from the viewpoint of oxidation resistance, a is preferably smaller, more preferably a=0, and most preferably 2n+1=b.

[0041] Specific examples of the organic anion represented by the general formula (i) include bis(fluorosulfonyl)imide (FSI; [N(FSO2)2] - ), bis(trifluoromethanesulfonyl)imide (TFSI; [N(CF3SO2)2] - ), bis(perfluoroethanesulfonyl)imide (BETI; [N(C2F5SO2)2] - ), (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([N(C2F5SO2)(CF3SO2)]- ) etc. In addition, as R 1 ~R 2 Specific examples of organic anions that are bonded to each other to form a ring include cTFSI; ([N(CF2SO2)2] - ) etc. Specific examples of organic anions represented by the general formula (ii) include FSO3 - CF3SO3 - 、C2F5SO3 - As specific examples of the organic anion represented by the general formula (iii), for example, CF3CO2 - 、C2F5CO2 - wait.

[0042] Examples of organic anions other than those of the general formula (i) include bis(1,2-benzenediol (2-)-O,O')borate, bis(2,3-naphthalenediol (2-)-O,O')borate, bis(2,2'-biphenylenediol (2-)-O,O')borate, and bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O')borate.

[0043] As the anion constituting the lithium salt, the imide anion is preferably used. As suitable specific examples of the imide anion, in addition to the imide anion exemplified as the organic anion represented by the general formula (i), (fluorosulfonyl) (trifluoromethanesulfonyl) imide (FTI; [N(FSO2)(CF3SO2)] - )wait.

[0044] Specific examples of lithium salts having lithium ions and imide anions include lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(perfluoroethanesulfonyl)imide (LiBETI), lithium (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide (LiFSI), and lithium (fluorosulfonyl)(trifluoromethanesulfonyl)imide (LiFTI).

[0045] Specific examples of other lithium salts include CF3SO3Li, C2F5SO3Li, CF3CO2Li, C2F5CO2Li, bis(1,2-benzenediol (2-)-O,O') lithium borate, bis(2,3-naphthalenediol (2-)-O,O') lithium borate, bis(2,2'-biphenylenediol (2-)-O,O') lithium borate, bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O') lithium borate, lithium perchlorate (LiClO4), lithium chloride (LiCl), lithium bromide (LiBr), lithium hydroxide (LiOH), lithium nitrate (LiNO3), lithium sulfate (Li2SO4), lithium sulfide (Li2S), lithium hydroxide (LiOH), etc.

[0046] In the aqueous electrolyte described in the present embodiment, the ratio of water to lithium salt is preferably 15:1 or less, more preferably 4:1 or less in terms of molar ratio. This is because: if the ratio of water to lithium salt is within these ranges, the potential window of the aqueous electrolyte is expanded, and the applied voltage to the secondary battery can be further increased. From the perspective of the safety of the secondary battery, the ratio of water to lithium salt is preferably 1.5:1 or more in terms of molar ratio.

[0047] (additive)

[0048] The aqueous electrolyte solution described in this embodiment may further contain additives or other electrolytes known in the art. As other electrolytes, a lithium ion conductive solid electrolyte may be further contained.

[0049] As additives, for example, fluorophosphates, carboxylic anhydrides, alkaline earth metal salts, sulfur compounds, acids and bases can be cited. The aqueous electrolyte preferably further contains at least one of fluorophosphates, carboxylic anhydrides, alkaline earth metal salts and sulfur compounds. The content of these additives is, for example, 0.1% by mass or more and 5.0% by mass or less relative to the total amount of the aqueous electrolyte.

[0050] As the fluorophosphate that can be added to the aqueous electrolyte, for example, lithium fluorophosphate salts represented by the general formula LixPFyOz (1 ≤ x < 3, 0 < y ≤ 2, 2 ≤ z < 4) can be cited. By making the aqueous electrolyte contain fluorophosphate, the electrolysis of water can be inhibited. As specific examples of the lithium fluorophosphate salt, for example, lithium difluorophosphate (LiPF2O2) and lithium monofluorophosphate (Li2PFO3) can be cited, and LiPF2O2 is preferred. It should be noted that the fluorophosphate represented by the general formula LixPFyOz can be a mixture of multiple substances selected from LiPF2O2, Li2PFO3, and Li3PO4. In this case, x, y, and z can be values other than integers. The content of the fluorophosphate only needs to be, for example, 0.1% by mass or more based on the total amount of the aqueous electrolyte, and preferably 0.3% by mass or more. In addition, the content of the lithium fluorophosphate salt only needs to be, for example, 3.0% by mass or less based on the total amount of the aqueous electrolyte, and preferably 2.0% by mass or less.

[0051] The alkaline earth metal salt that can be added to the aqueous electrolyte is a salt having an ion of an alkaline earth metal (Group 2 element) and an anion such as an organic anion. As the alkaline earth metal, for example, beryllium (Be), magnesium (Mg), calcium (Ca), and strontium (Sr) can be cited, and magnesium and calcium are preferred.

[0052] As the organic anion constituting the alkaline earth metal salt, for example, the organic anions represented by the general formulas (i) to (iii) described as the organic anions constituting the above lithium salts can be cited. However, the anion constituting the alkaline earth metal salt can be an organic anion other than the organic anions represented by the general formulas (i) to (iii), or can also be an inorganic anion.

[0053] The dissociation constant of the alkaline earth metal salt in the aqueous electrolyte is preferably large. For example, suitable examples include alkaline earth metal salts of perfluoroalkanesulfonic acid imides such as Ca[N(CF3SO3)2]2(CaTFSI), Ca[N(CF3CF3SO2)2]2(CaBETI), Mg[N(CF3SO3)2]2(MgTFSI), and Mg[N(CF3CF3SO2)2]2(MgBETI); alkaline earth metal salts of trifluoromethanesulfonic acid such as Ca(CF3SO3)2 and Mg(CF3SO3)2; alkaline earth metal salts of perchloric acid such as Ca[ClO4]2 and Mg[ClO4]2; and tetrafluoroborates such as Ca[BF4]2 and Mg[BF4]2. Among these, alkaline earth metal salts of perfluoroalkanesulfonic acid imides are more preferred from the viewpoint of plasticizing effect, and CaTFSI and CaBETI are particularly preferred. In addition, as alkaline earth metal salt, it is also preferred to have an alkaline earth metal salt with the same anion as the lithium salt contained in the electrolyte. The alkaline earth metal salt can be used alone or in combination of two or more. From the viewpoint of the expansion of the potential window to the low potential side, the content of the alkaline earth metal salt is, for example, 0.5 mass % or more and 3 mass % or less relative to the total amount of the aqueous electrolyte, preferably 1.0 mass % or more and 2 mass % or less.

[0054] The carboxylic anhydride that can be added to the aqueous electrolyte includes cyclic carboxylic anhydride and chain carboxylic anhydride. As cyclic carboxylic anhydride, for example, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, diglycolic anhydride, cyclohexane dicarboxylic anhydride, cyclopentane tetracarboxylic anhydride, phenyl succinic anhydride, etc. can be listed. Chain carboxylic anhydride is an anhydride of two identical or different carboxylic acids selected from carboxylic acids having 1 to 12 carbon atoms such as acetic acid, propionic acid, butyric acid, isobutyric acid, etc. As a specific example thereof, acetic anhydride, propionic anhydride, etc. can be listed. When added to the aqueous electrolyte, the carboxylic anhydride can be used alone or in combination of two or more. The content of the carboxylic anhydride is, for example, 0.1% by mass or more and 5.0% by mass or less relative to the total amount of the aqueous electrolyte, preferably 0.3% by mass or more and 2.0% by mass or less.

[0055] As sulfur compounds that can be added to the aqueous electrolyte, there can be listed, for example, organic compounds containing sulfur atoms in the molecule, and the compound does not contain the above-mentioned lithium salts, polycarboxylic acids and alkaline earth metal salts. By including the sulfur compound in the aqueous electrolyte, it is possible to compensate for the coating containing components derived from the reduction reaction of anions represented by general formulas (i) to (iii) such as TFSI and BETI, and it is possible to efficiently block the parasitic hydrogen evolution in the negative electrode. As specific examples of sulfur compounds, there can be listed, for example, cyclic sulfur compounds such as ethylene sulfite, 1,3-propane sultone, 1,4-butane sultone, cyclopentane sulfone, cyclobutene sulfone; sulfonic acid esters such as methyl methanesulfonate and busulfan; sulfones such as dimethyl sulfone, diphenyl sulfone, and methyl phenyl sulfone; sulfides or disulfides such as dibutyl disulfide, dicyclohexyl disulfide, and tetramethylthiuram monosulfide; sulfonamides such as N,N-dimethylmethanesulfonamide and N,N-diethylmethanesulfonamide, etc. Among these sulfur compounds, ethylene sulfite, 1,3-propane sultone, 1,4-butane sultone, cyclopentane sulfone, etc. are preferred, and ethylene sulfite is particularly preferred. When added to the aqueous electrolyte, the sulfur compound can be used alone or in combination of two or more. The content of the sulfur compound can be, for example, 0.1% by mass or more and 5.0% by mass or less relative to the total amount of the aqueous electrolyte, preferably 0.3% by mass or more and 2.0% by mass or less.

[0056] The method for preparing the aqueous electrolyte according to the present embodiment is not particularly limited, and the aqueous electrolyte may be prepared by, for example, appropriately mixing water, a lithium salt, and the above-mentioned additives when adding.

[0057] The pH of the aqueous electrolyte is not particularly limited, for example, as long as it is greater than 3 and less than 14, preferably greater than 10. This is because: when the pH of the aqueous electrolyte is within these ranges, the stability of the positive electrode active material in the positive electrode and the negative electrode active material in the negative electrode in the aqueous solution can be improved, and the absorption and desorption reactions of lithium ions in the positive electrode active material and the negative electrode active material can become smoother.

[0058] [Secondary battery]

[0059] Hereinafter, a secondary battery described in an example of an embodiment of the present application will be described. A secondary battery as an example of an embodiment comprises the above-mentioned aqueous electrolyte, a positive electrode and a negative electrode. The secondary battery has a structure in which, for example, an electrode body comprising a positive electrode, a negative electrode and a separator and an aqueous electrolyte are contained in a battery case. As the electrode body, for example, a wound electrode body in which a positive electrode and a negative electrode are wound with a separator therebetween, a stacked electrode body in which a positive electrode and a negative electrode are stacked with a separator therebetween, etc. can be cited, and the form of the electrode body is not limited thereto.

[0060] Examples of the battery case that houses the electrode body and the aqueous electrolyte include metal or resin cases such as cylindrical, square, coin-shaped, and button-shaped cases; and resin cases (laminated batteries) obtained by molding a sheet obtained by laminating a resin sheet and a metal foil, etc.

[0061] The secondary battery according to the present embodiment can be manufactured by a known method. For example, a wound or laminated electrode body is housed in a battery case main body, an aqueous electrolyte is injected, and then the opening of the battery case main body is sealed with a gasket and a sealing body.

[0062] [Positive electrode]

[0063] The positive electrode of the secondary battery according to the present embodiment is composed of, for example, a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode active material layer can be formed on one surface of the positive electrode current collector or on both surfaces. The positive electrode active material layer contains, for example, a positive electrode active material, a binder material, a conductive material, etc.

[0064] As the positive electrode current collector, a foil of a metal that is stable within the potential range of the positive electrode, and a thin film having the metal disposed on the surface layer, etc. can be used. As the positive electrode current collector, a porous body such as a mesh, a punched sheet, or a wire mesh of the metal can be used. As the material of the positive electrode current collector, stainless steel, aluminum, aluminum alloy, titanium, etc. can be used. From the viewpoints of current collection property, mechanical strength, etc., the thickness of the positive electrode current collector is preferably, for example, 3 μm or more and 50 μm or less.

[0065] The positive electrode can be obtained, for example, by coating a positive electrode composite material slurry containing a positive electrode active material, a conductive material, a binder material, etc. on the positive electrode current collector and drying it, thereby forming a positive electrode active material layer on the positive electrode current collector and calendering the positive electrode active material layer. As the dispersion medium used in the positive electrode composite material slurry, for example, water, alcohols such as ethanol, ethers such as tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), etc. can be used. The thickness of the positive electrode active material layer is not particularly limited, and is, for example, 10 μm or more and 100 μm or less.

[0066] The positive electrode active material is a lithium transition metal oxide containing lithium (Li) and transition metal elements such as cobalt (Co), manganese (Mn), and nickel (Ni). As a specific example of the lithium transition metal oxide, it is a composite oxide represented by Li a Ni x Co y Mn z M b O2 (0.9 < a < 1.1, 0.4 ≤ x < 1.0, 0 ≤ y < 0.4, 0 ≤ z < 0.4, 0 ≤ b < 0.2, 0.9 < (x + y + z + b) < 1.1).

[0067] Here, the element M is at least one selected from the group consisting of titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), aluminum (Al), gallium (Ga), and indium (In).

[0068] From the viewpoint of high capacity, the lithium transition metal oxide preferably contains 40 mol% or more of Ni relative to the total amount of transition metals other than lithium, and more preferably 80 mol% or more. That is, preferably 0.4≤x<1.0, more preferably 0.8≤x<1. In addition, as the ratio of Li, preferably 0.95

[0069] The ratio (B / A) of the BET specific surface area (B) of the composite oxide particles of the positive electrode active material after the particle compression test to the BET specific surface area (A) before the particle compression test is preferably greater than 1.0 and less than 3.0. The BET specific surface area (A) before the particle compression test is the BET specific surface area of ​​the composite oxide particles disassembled and taken out of the secondary battery or the composite oxide particles used in the secondary battery. The BET specific surface area is a value measured according to the BET method (nitrogen adsorption method) described in JIS R1626. In addition, the BET specific surface area (B) after the particle compression test is the BET specific surface area of ​​the composite oxide particles after the compression test is carried out for the composite oxide particles disassembled and taken out of the secondary battery or the composite oxide particles used in the secondary battery using the following conditions.

[0070] The particle compression test mentioned in this specification refers to a test in which a positive electrode composite material slurry comprising the above-mentioned composite oxide particles, a conductive material, a binding material, etc. is coated on a positive electrode collector and dried to form a positive electrode active material layer, and the positive electrode composite material layer is pressed until the composite material density reaches 3.4 g / cc, thereby compressing the composite oxide particles.

[0071] ​The ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test is greater than 1.0 and less than 3.0, indicating that almost all of the primary particle surfaces are exposed, for example, particles in a non-aggregated state satisfy the above range. The non-aggregated state includes not only a state in which primary particles are completely separated into individual particles, but also a state in which several (for example, 2 to 15) primary particles are aggregated. It should be noted that in the following description, the "ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test" is sometimes referred to as B / A.

[0072] Figure 1 A schematic diagram of the positive electrode active material 10 described in this embodiment is shown. It is generally believed that in a secondary battery, self-discharge is achieved by embedding protons from the electrolyte into the positive electrode active material 10, thereby reducing the positive electrode potential, and the capacity may deteriorate when a positive electrode active material with a high Ni ratio is used. In contrast, it can be considered that when non-aggregated composite particles with a B / A of 1.0 or more and 3.0 or less are used as positive electrode active materials, both the embedding / de-embedding of lithium ions is allowed and the embedding of protons is suppressed, and as a result, the reduction in the positive electrode potential is suppressed.

[0073] On the other hand, B / A exceeding 3.0 means that the composite particles exist in the positive electrode active material layer in the form of secondary particles, and the primary particle surface of the composite particles is almost not exposed. It means, for example, secondary particles formed by the aggregation of dozens or more primary particles. Although the present inventors may not have a clear mechanism, they have confirmed that the proton embedding degree of primary particles is different from that of secondary particles formed by the aggregation of primary particles. In the case of secondary particles, proton embedding occurs significantly compared with that of primary particles. Therefore, by making B / A greater than 1.0 and less than 3.0, a non-aggregated state can be achieved, and the Ni ratio can be increased without causing a significant decrease in the positive electrode potential, and a Ni ratio of more than 80 mol% can be achieved. "Non-aggregated state" refers to a state separated into individual primary particles, and also refers to a state that can be said to be essentially a non-aggregated state. Specifically, it is a state where 2 to 15 primary particles are aggregated.

[0074] The non-aggregated state of the composite oxide particles can be observed by a cross-sectional SEM image based on a scanning electron microscope (SEM). For example, the positive electrode is embedded in a resin, the cross section of the positive electrode is made by cross-sectional polishing (CP) processing, and the cross section of the positive electrode active material layer at the cross section is photographed by SEM. Alternatively, the powder of the lithium transition metal oxide is embedded in a resin, the particle cross section of the lithium transition metal oxide is made by cross-sectional polishing (CP) processing, and the cross section is photographed by SEM. Regarding the quantification of the aggregation state of the primary particles, first, the particles whose particle diameter can be confirmed by the cross-sectional SEM image and the error of the volume average particle diameter is within 10% are selected, and the size of the primary particles is confirmed. In addition, the primary particles and the particles in the aggregated state are respectively set as spheres, and the volume of the primary particles is calculated by the ratio of the volume of the primary particles to the volume assumed by the volume average particles.

[0075] The average particle size (D50) of the composite oxide particles is preferably, for example, greater than 2 μm and less than 20 μm. When the average particle size (D50) is less than 2 μm and greater than 20 μm, the packing density in the positive electrode active material layer is sometimes reduced and the capacity is reduced compared to the case where the above range is satisfied. It should be noted that the particles that are the object of measurement of the average particle size include not only the state in which they are completely separated into individual primary particles, but also the state in which several (for example, 2 to 15) primary particles are gathered to form one particle. The average particle size (D50) of the positive electrode active material can be measured by laser diffraction method using, for example, MT3000II manufactured by MICROTRAC BELL.

[0076] The compressive strength of the composite oxide particles is preferably 250 MPa or more, more preferably 350 MPa or more. When the compressive strength of the composite oxide particles meets the above range, the particle breakage caused by charging and discharging is suppressed compared to the case where the above range is not met. The breakage of the particles will cause the particles to generate new surfaces, resulting in the occurrence of surface modification that will generate nickel and oxygen compounds. Therefore, by making the compressive strength of the composite oxide particles meet the above range, the increase in the capacity degradation rate after storage can be further suppressed. It should be noted that the upper limit of the compressive strength of the composite oxide particles is not particularly limited. For example, from the perspective of material performance, it is preferably 1500 MPa or less. The compressive strength is measured using the method specified in JIS-R1639-5.

[0077] The content of the composite oxide particles is preferably 30% by mass or more and 100% by mass or less, and more preferably 80% by mass or more and 95% by mass or less, relative to the total amount of the positive electrode active material. If the content of the composite oxide particles containing a large amount of Ni in the positive electrode active material layer is less than 30% by mass, the effect of suppressing the increase in the capacity degradation rate of the battery after charging and storage, for example, may be reduced compared to the case where the above range is satisfied.

[0078] The content of the positive electrode active material is, for example, preferably 70 mass % or more and 99 mass % or less, and more preferably 80 mass % or more and 95 mass % or less, based on the total amount of the positive electrode composite material layer.

[0079] An example of a method for producing composite oxide particles will be described.

[0080] The method for manufacturing composite oxide particles includes: a composite hydroxide synthesis step of obtaining Ni, Co, Al composite hydroxide or Ni, Co, Mn composite hydroxide; a raw material mixing step of mixing the composite hydroxide with a lithium compound to obtain a raw material mixture; and a calcining step of calcining the raw material mixture to obtain composite oxide particles containing a large amount of Ni.

[0081] The composite hydroxide synthesis process can include, for example, a coprecipitation method in which a Ni, Co, Al composite hydroxide or a Ni, Co, Mn composite hydroxide is precipitated (coprecipitated) by stirring a solution containing a metal salt of Ni, Co, Al (or Mn) or the like while dropping an alkaline solution such as sodium hydroxide to adjust the pH to the alkaline side (e.g., 8.5 to 11.5). In the composite hydroxide synthesis process, it is preferred to include a aging process in which the composite hydroxide is directly stored in the reaction solution after the composite hydroxide is precipitated. Thus, the composite oxide particles finally obtained are easily obtained in the form of particles in a non-aggregated state.

[0082] The raw material mixing step is a method of obtaining a raw material mixture by mixing the composite hydroxide with a lithium compound such as lithium hydroxide, lithium carbonate, lithium nitrate, etc. In order to set the ratio (B / A) of the BET specific surface area (B) after the particle compression test of the finally obtained composite oxide particles to the BET specific surface area (A) before the particle compression test to 1.0 or more and 3.0 or less, it is preferred that the mixing ratio of the composite hydroxide and the lithium compound is set to, for example, a molar ratio of metal element (Ni+Co+Al or Mn):Li in the range of 1.0:1.02 to 1.0:1.2.

[0083] The calcination process is a method of obtaining composite oxide particles by calcining the raw material mixture under an oxygen atmosphere, for example. In order to set the ratio (B / A) of the BET specific surface area (B) after the particle compression test of the composite oxide particles finally obtained to the BET specific surface area (A) before the particle compression test to 1.0 or more and 3.0 or less, it is preferred to set the calcination temperature of the raw material mixture to, for example, a range of 750°C or more and 1100°C or less. The calcination temperature is preferably 20 hours to 150 hours, more preferably 20 hours to 100 hours. It should be noted that when the calcination time of the composite oxide particles exceeds 150 hours, it sometimes causes, for example, deterioration of material properties and electrochemical characteristics compared to the case of less than 150 hours.

[0084] Examples of the conductive material contained in the positive electrode active material layer include carbon black, acetylene black, Ketjen black, graphite and other carbon powders, etc. These may be used alone or in combination of two or more.

[0085] As the binding material contained in the positive electrode active material layer, for example, fluorine-based polymers, rubber-based polymers, etc. can be listed. As fluorine-based polymers, for example, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF) or their modified bodies can be listed, and as rubber-based polymers, for example, ethylene-propylene-isoprene copolymers, ethylene-propylene-butadiene copolymers, etc. can be listed. They can be a single one, or two or more can be used in combination.

[0086] The positive electrode of the present embodiment can be obtained by, for example, applying a positive electrode composite material slurry containing a positive electrode active material, a conductive material, a binder, etc., on a positive electrode current collector, drying the slurry to form a positive electrode active material layer, and rolling the positive electrode composite material layer.

[0087] [negative electrode]

[0088] The negative electrode constituting the secondary battery described in this embodiment is composed of, for example, a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode active material layer may be formed on one surface of the negative electrode current collector or on both surfaces. The negative electrode active material layer includes, for example, a negative electrode active material, a binding material, and the like.

[0089] As the negative electrode current collector, a foil of a metal that is stable within the potential range of the negative electrode, and a thin film of the metal disposed on the surface layer, etc. can be used. As the negative electrode current collector, a porous body such as a mesh body, a punched sheet, and a metal plate net of the metal can be used. As the material of the negative electrode current collector, copper, copper alloy, aluminum, aluminum alloy, stainless steel, nickel, etc. can be used. From the viewpoints of current collection, mechanical strength, etc., the thickness of the negative electrode current collector is preferably, for example, 3 μm or more and 50 μm or less.

[0090] The negative electrode can be prepared by, for example, coating a negative electrode composite material slurry containing a negative electrode active material, a binding material and a dispersion medium on a negative electrode collector and drying the coating film, and then rolling to form a negative electrode active material layer on one or both sides of the negative electrode collector. The negative electrode active material layer may contain any component such as a conductive agent as needed. The thickness of the negative electrode active material layer is not particularly limited, for example, 10 μm or more and 100 μm or less.

[0091] The negative electrode active material is not particularly limited as long as it is a material that can absorb / release lithium ions. The material constituting the negative electrode active material may be a non-carbon material, a carbon material, or a combination thereof. Examples of non-carbon materials include lithium metal, alloys containing lithium elements, and metal compounds such as metal oxides, metal sulfides, and metal nitrides containing lithium. Examples of alloys containing lithium elements include lithium aluminum alloys, lithium tin alloys, lithium lead alloys, and lithium silicon alloys. Examples of metal oxides containing lithium include metal oxides containing lithium and containing titanium, tantalum, or niobium, preferably lithium titanate (Li4Ti5O 12 wait).

[0092] As carbon materials used as negative electrode active materials, for example, graphite and hard carbon can be listed. Among them, graphite is preferred due to its high capacity and small irreversible capacity. Graphite is a general term for carbon materials with a graphite structure, including natural graphite, artificial graphite, expanded graphite, graphitized mesophase carbon particles, etc. When graphite is used as a negative electrode active material, in order to reduce the activity of reduction and decomposition of aqueous electrolytes, it is preferred to cover the surface of the negative electrode active material layer with a coating. These negative electrode active materials can be used alone or in combination of two or more.

[0093] As the binding material contained in the negative electrode active material layer, for example, fluorine-based polymers, rubber-based polymers, etc. can be used in the same manner as in the case of the positive electrode. In addition, styrene-butadiene copolymer (SBR) or its modified body can also be used. The content of the binding material contained in the negative electrode active material layer is preferably 0.1% by mass or more and 20% by mass or less relative to the total amount of the negative electrode active material, more preferably 1% by mass or more and 5% by mass or less. As the thickener contained in the negative electrode active material layer, for example, carboxymethyl cellulose (CMC), polyethylene oxide (PEO), etc. can be listed. They can be a single kind, or two or more kinds can be used in combination.

[0094] [Separator]

[0095] As a separator, there is no particular limitation as long as it has the function of passing lithium ions and electrically separating the positive electrode from the negative electrode, and for example, a porous sheet composed of a resin, an inorganic material, etc. can be used. Specific examples of porous sheets include microporous films, woven fabrics, non-woven fabrics, etc. As resin materials constituting the separator, olefin resins such as polyethylene and polypropylene; polyamide, polyamide-imide, cellulose, etc. can be listed. As inorganic materials constituting the separator, glasses and ceramics such as borosilicate glass, silica, alumina, and titanium dioxide can be listed. The separator can be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, it can be a multilayer separator comprising a polyethylene layer and a polypropylene layer, and a separator coated with a material such as an aromatic polyamide resin, ceramic, etc. on the surface of the separator can also be used.

[0096] It should be noted that, in the above embodiment, a secondary battery having an aqueous electrolyte is described, but the aqueous electrolyte described in one example of this embodiment can be used in a storage device other than a secondary battery, and can be used in, for example, a capacitor. In this case, the capacitor has, for example, an aqueous electrolyte described in one example of this embodiment and two electrodes. The electrode material constituting the electrode can be any material that can be used in a capacitor and can absorb and release lithium ions, and materials such as graphite-containing materials such as natural graphite or artificial graphite, and materials such as lithium titanate can be listed.

[0097] Example

[0098] Hereinafter, examples and comparative examples of the present application will be described in detail, but the present application is not limited to the following examples.

[0099] (Example 1)

[0100] The [Ni 0.5 Co 0.2 Mn 0.3 ](OH)2 and lithium carbonate were mixed in such a manner that the molar ratio of Li to the total amount of Ni, Co, and Mn reached 1.1:1.0. Thereafter, the mixture was calcined at 1000°C for 20 hours in an air atmosphere to obtain composite oxide particles. a Ni x Co y Mn z Al b In O2, x:y:z=5:2:3, and the ratio of Li, that is, a / (x+y+z+b), is 1.03.

[0101] The obtained composite oxide particles are embedded in a resin, and the cross section of the particles is prepared by cross-section polishing (CP), and the cross section is observed by SEM. As a result, the composite oxide particles exist in a state of being completely separated into individual primary particles, or in a state of being aggregated by 2 to 10 primary particles, and are particles in a non-aggregated state. It should be noted that in the positive electrode prepared below, when the cross section is observed by SEM, the composite oxide particles exist in a state of being completely separated into individual primary particles in the positive electrode composite material layer, or in a state of being aggregated by 2 to 5 primary particles, and exist in a non-aggregated state in the positive electrode active material layer. The BET specific surface area of ​​the obtained composite oxide particles is measured, and a compression test is carried out under the above conditions, and the BET specific surface area of ​​the composite oxide particles after the compression test is measured. In the obtained composite oxide particles, the ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test reaches 1.4.

[0102] [Production of positive electrode]

[0103] The composite oxide particles as the positive electrode active material, acetylene black as the conductive material, and polyvinylidene fluoride as the binding material were mixed in a mass ratio of 100:1:1, and N-methyl-2-pyrrolidone was added to prepare a positive electrode composite material slurry. Next, the positive electrode composite material slurry was applied to both sides of a positive electrode collector composed of aluminum foil, dried, and then rolled using a rolling roller, thereby preparing a positive electrode having a positive electrode active material layer formed on both sides of the positive electrode collector.

[0104] [Production of negative electrode]

[0105] Graphite as a negative electrode active material, styrene-butadiene copolymer (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a mass ratio of 100:1:1, and water was added to prepare a negative electrode composite material slurry. Next, the negative electrode composite material slurry was applied to both sides of a negative electrode collector formed of copper foil, dried, and then rolled using a calendering roller, thereby producing a negative electrode having a negative electrode active material layer formed on both sides of the negative electrode collector.

[0106] [Preparation of aqueous electrolyte]

[0107] Lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2), lithium bis(perfluoroethanesulfonyl)imide (LiN(SO2C2F5)2), lithium hydroxide and water (ultrapure water) were mixed in a molar ratio of 0.7:0.3:0.034:1.932. The content of water was 10% by mass relative to the total amount of the electrolyte, and the molar ratio of water to lithium salt contained in the electrolyte was 2:1.

[0108] [Manufacturing of Secondary Batteries]

[0109] The positive electrode and the negative electrode were wound with a separator interposed therebetween to produce an electrode body, which was housed in a bottomed cylindrical battery case together with the aqueous electrolyte, and the opening of the battery case was sealed with a gasket and a sealing body.

[0110] (Example 2)

[0111] The [Ni 0.82 Co 0.15 Al 0.03 ](OH)2 and lithium hydroxide were mixed in such a manner that the molar ratio of Li to the total amount of Ni, Co, and Al reached 1.1:1.0. Thereafter, the mixture was calcined at 780°C in an oxygen atmosphere for 50 hours to obtain the composite oxide particles described in Example 2. a Ni x Co y Al b In O2, the ratio x of Ni is 82%, and the ratio of Li, i.e., a / (x+y+z+b), is 0.98. The obtained composite oxide particles are embedded in a resin, and the cross section of the particles is made by cross-section polishing (CP) processing, and the cross section is observed by SEM. As a result, the composite oxide particles exist in a state of being completely separated into individual primary particles, or in a state of being aggregated into 2 to 10 primary particles, and are particles in a non-aggregated state. It should be noted that in the positive electrode prepared below, when its cross section is observed by SEM, the composite oxide particles exist in the positive electrode composite material layer in a state of being completely separated into individual primary particles, or in a state of being aggregated into 2 to 5 primary particles, and exist in the positive electrode active material layer as particles in a non-aggregated state.

[0112] The BET specific surface area of ​​the obtained composite oxide particles was measured, and a compression test was carried out using the above-mentioned conditions. The BET specific surface area of ​​the composite oxide particles after the compression test was measured. In the obtained composite oxide particles, the ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test reached 1.9.

[0113] In Example 2, a secondary battery was prepared in the same manner as in Example 1 except that the composite oxide particles described in Example 2 were used as the positive electrode active material.

[0114] (Comparative Example 1)

[0115] In the preparation of the composite oxide particles, the composite oxide particles were obtained in the same manner as in Example 1 except that the calcination temperature was changed to 900° C. The Li ratio of the composite oxide particles in Comparative Example 1, that is, a / (x+y+z+b), was 1.06.

[0116] The composite oxide particles obtained in Comparative Example 1 were embedded in a resin and processed by cross-section polishing (CP) to prepare a cross section of the particles. When the cross section was observed by SEM, the composite oxide particles in Comparative Example 1 were aggregated particles composed of dozens or more primary particles.

[0117] In the positive electrode produced using the composite oxide particles of Comparative Example 1, when the cross section was observed by SEM, the composite oxide particles were present in the positive electrode active material layer as aggregated particles composed of several tens or more primary particles.

[0118] The BET specific surface area of ​​the composite oxide particles described in Comparative Example 1 was determined, a compression test was carried out using the aforementioned conditions, and the BET specific surface area of ​​the composite oxide particles after the compression test was determined. In the obtained composite oxide particles, the ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test reached 5.0.

[0119] In Comparative Example 1, a secondary battery was produced in the same manner as in Example 1 except that the composite oxide particles described in Comparative Example 1 were used as a positive electrode active material.

[0120] (Comparative Example 2)

[0121] In the preparation of the composite oxide particles, the composite oxide particles were obtained in the same manner as in Example 2 except that the calcination temperature was changed to 900° C. The Li ratio of the composite oxide particles in Comparative Example 2, that is, a / (x+y+z+b), was 0.98.

[0122] The composite oxide particles obtained in Comparative Example 2 were embedded in a resin and processed by cross-section polishing (CP) to prepare a cross section of the particles. When the cross section was observed by SEM, the composite oxide particles in Comparative Example 2 were particles in an aggregated state composed of dozens or more primary particles.

[0123] In the positive electrode produced using the composite oxide particles of Comparative Example 2, when the cross section was observed by SEM, the composite oxide particles were present in the positive electrode active material layer as aggregated particles composed of several tens or more primary particles.

[0124] The BET specific surface area of ​​the composite oxide particles described in Comparative Example 2 was determined, a compression test was carried out using the aforementioned conditions, and the BET specific surface area of ​​the composite oxide particles after the compression test was determined. In the obtained composite oxide particles, the ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test reached 6.9.

[0125] In Comparative Example 2, a secondary battery was produced in the same manner as in Example 1, except that the composite oxide particles described in Comparative Example 2 were used as a positive electrode active material.

[0126] (Comparative Example 3)

[0127] In Comparative Example 3, in the preparation of the composite oxide particles, [Ni 0.82 Co 0.15 Al 0.03 The composite oxide particles were prepared in the same manner as in Comparative Example 2 except that ](OH)2 and lithium hydroxide were mixed in such a manner that the molar ratio of Li to the total amount of Ni, Co, and Al reached 1.15:1.0. The ratio of Li in the composite oxide particles in Comparative Example 3, i.e., a / (x+y+z+b), was 1.02.

[0128] The composite oxide particles obtained in Comparative Example 3 were embedded in a resin and processed by cross-section polishing (CP) to prepare a cross section of the particles. When the cross section was observed by SEM, the composite oxide particles in Comparative Example 3 were particles in an aggregated state composed of dozens or more primary particles.

[0129] In the positive electrode produced using the composite oxide particles of Comparative Example 3, when the cross section was observed by SEM, the composite oxide particles were present in the positive electrode active material layer as aggregated particles composed of several tens or more primary particles.

[0130] The BET specific surface area of ​​the composite oxide particles described in Comparative Example 3 was determined, a compression test was carried out using the aforementioned conditions, and the BET specific surface area of ​​the composite oxide particles after the compression test was determined. In the obtained composite oxide particles, the ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test reached 6.9.

[0131] In Comparative Example 3, a secondary battery was produced in the same manner as in Example 1, except that the composite oxide particles described in Comparative Example 3 were used as a positive electrode active material.

[0132] [Measurement of voltage drop after charging and storage]

[0133] For the secondary batteries of each embodiment and each comparative example, the voltage drop after charging and storage was measured under the following conditions. After charging at a constant current of 0.1C until the closed circuit voltage of the battery reached 2.75V, the battery was stored at 25°C for 72 hours, and the change in the open circuit voltage of the battery (V) was calculated. The charging and storage test was carried out in an environment of 25°C. The change in open circuit voltage (V) was used as an indicator of stability during charging and storage.

[0134] Table 1 shows the results of a charge storage test (25° C., 3 days) of the secondary batteries of each Example and each Comparative Example.

[0135] [Table 1]

[0136]

[0137] In the above-mentioned composite oxide particles, the ratio (B / A) of the BET specific surface area (B) after the particle compression test to the BET specific surface area (A) before the particle compression test is greater than 1.0 and less than 3.0, and in Examples 1 and 2 using an aqueous electrolyte, the voltage drop after the charge storage test shows a low value compared with Comparison Examples 1 to 3 in which the B / A ratio does not satisfy the above-mentioned range, and the battery degradation during charge storage is suppressed.

Claims

1. A secondary battery comprising: A positive electrode containing a positive active material; a negative electrode comprising a negative electrode active material; and An electrolyte made by dissolving lithium salt in water. The positive electrode active material is a general formula Li a Ni x Co y Mn z M b O2 represents and satisfies: 0.9<a<1.1、 0.4≤x<1.0、 0≤y<0.4、 0≤z<0.4、 0≤b<0.2、 0.9<(x+y+z+b)<1.1 composite oxide, The element M includes at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Ga, and In, The ratio (B / A) of the BET specific surface area (B) of the composite oxide particles after a particle compression test to the BET specific surface area (A) before the particle compression test is greater than 1.0 and less than or equal to 3.

0.

2. The secondary battery according to claim 1, wherein a, x, y, z, and b in the general formula satisfy 0.95; x in the general formula satisfies 0.8 <x<1。 3. The secondary battery according to claim 1, wherein The element M contains at least Al.

4. The secondary battery according to claim 1, wherein The pH of the electrolyte is greater than 10.

5. The secondary battery according to claim 1, wherein 6. A secondary battery comprising: A positive electrode containing a positive active material; a negative electrode comprising a negative electrode active material; and An electrolyte made by dissolving lithium salt in water. 0.9<(x+y+z+b)<1.1 composite oxide, The positive electrode active material is a general formula Li a Ni x Co y Mn z M b O2 represents and satisfies: 0.9<a<1.1、 0.4≤x<1.0、 0≤y<0.4、 0≤z<0.4、 0≤b<0.2、 The element M includes at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Ga, and In, The composite oxide particles are in a state where individual primary particles are separated and 2 to 15 primary particles are aggregated; or 2 to 15 primary particles are aggregated. ​

Citation Information

Patent Citations

  • Positive electrode active material, positive electrode material, positive electrode, and nonaqueous electrolyte secondary battery

    CN105051952A

  • Lithium metal oxide containing batteries having improved rate capability

    CN106716689A

  • Water system secondary battery

    CN107403968A

  • Cathode active material for secondary battery, and secondary battery comprising same

    CN108140829A

  • Lithium secondary battery

    JP2001052747A