Composite plate and preparation method thereof, and heat soaking plate
By using the composite structure of the first copper foil, graphene layer and electroplated copper foil in the vapor chamber, the problem of insufficient thermal conductivity of the existing vapor chamber is solved, achieving higher thermal conductivity and structural strength, and improving the chip operational stability.
Patent Information
- Application Number
- CN202110017035.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-01-06
AI Technical Summary
The thermal conductivity of the existing vapor chamber is insufficient, causing the chip temperature to be too high and performance to degrade when operating under high load.
A composite board composed of a first copper foil, a graphene layer and an electroplated copper foil is used. By growing a graphene layer on the first copper foil and electroplating copper foil on the graphene layer, a composite board with better thermal conductivity and structural strength is formed. of composite panels used to construct vapor chambers.
The thermal conductivity and strength of the vapor chamber are improved, effectively reducing the chip temperature and improving performance stability.
Smart Images

Figure CN112760644B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of materials, and in particular, to a composite board and a preparation method thereof, and a heat spreader. Background Art
[0002] When the chip is running at a high load continuously, a large amount of heat will be generated, resulting in excessive chip temperature, running jams, frame drops, frequency reduction and other phenomena, and the chip performance will be significantly reduced. A heat spreader can be used to dissipate the heat. The main structure of the heat spreader consists of an upper cover plate, a lower cover plate, a sealed cavity, a capillary structure and a cooling medium. Usually the upper / lower cover plates are made of pure copper plates and welded into a vacuum cavity with a fine structure on the inner wall. The heat spreader is a vacuum cavity with a fine structure on the inner wall, usually made of copper. However, the thermal conductivity of the existing heat spreader needs to be improved. Summary of the invention
[0003] The purpose of the embodiments of the present application is to provide a composite plate and a preparation method thereof, and a vapor chamber, which are intended to improve the thermal conductivity of the vapor chamber.
[0004] The present application provides a composite board, the composite board comprising a first copper foil, a graphene layer and a second copper foil stacked in sequence;
[0005] Wherein, the first copper foil has a crystal domain number less than or equal to 5 / square centimeter;
[0006] The second copper foil is electroplated copper.
[0007] The first copper foil with a crystal domain number less than or equal to 5 / square centimeter has better thermal conductivity. A graphene layer is arranged on the first copper foil, and then electroplated copper is arranged on the graphene layer. The electroplated copper and the first copper foil can overcome the problem that the graphene layer cannot be used as a structural material. The composite board composed of the first copper foil with a smaller crystal domain number and the electroplated copper located on both sides of the graphene layer can have a better thermal conductivity.
[0008] In some embodiments of the present application, the thickness of the first copper foil is 3-150 μm.
[0009] In some embodiments of the present application, the hardness of the first copper foil and the graphene layer is 30-60 HV.
[0010] In some embodiments of the present application, the thickness of the second copper foil is 1-1000 μm;
[0011] In some embodiments of the present application, the hardness of the composite plate is 100-200 HV.
[0012] In some embodiments of the present application, the composite board includes a plurality of graphene layers and a plurality of second copper foils; the graphene layers and the second copper foils are arranged crosswise, and the graphene layers cover the first copper foils.
[0013] The present application also provides a method for preparing the above-mentioned composite board, comprising:
[0014] growing a graphene layer on the first copper foil;
[0015] preparing a second copper foil on the graphene layer by electroplating;
[0016] Wherein, the number of crystal domains of the first copper foil is less than or equal to 5 per square centimeter.
[0017] In some embodiments of the present application, before growing the graphene layer on the first copper foil, the step further includes preparing the first copper foil, specifically including:
[0018] In an inert atmosphere, the electrolytic copper foil or rolled copper foil is heated to 800-1075°C and then annealed in a reducing atmosphere.
[0019] In some embodiments of the present application, in the step of growing a graphene layer on the first copper foil, the graphene layer is grown by chemical vapor deposition.
[0020] The present application also provides a vapor chamber, wherein the vapor chamber is formed by connecting composite plates.
[0021] The heat spreader provided in the embodiment of the present application has the advantages of the above-mentioned composite plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 A schematic structural diagram of a heat spreader provided in an embodiment of the present application is shown.
[0024] Icon: 100 - composite board; 110 - first copper foil; 120 - graphene layer; 130 - second copper foil. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0026] The heat spreader must meet the requirements of being thin and light and large in size, which will weaken the structural strength of the board and make it easy to deform under certain conditions, eventually leading to structural failure and adversely affecting heat dissipation. Using "copper + stainless steel or titanium alloy, etc." composite materials as the upper and lower cover plates, although the board strength and surface hardness can be increased and not easily deformed, the thermal conductivity of the stainless steel or titanium alloy material is seriously insufficient, which will affect the thermal conductivity and welding performance of the overall heat spreader. Some "Cu+Gr" or "Cu+CNT" composite materials are prepared by doping graphite sheets or CNTs in the copper cover plate material. Due to the discontinuity of graphite and CNT, the overall thermal conductivity and strength performance of the heat spreader are limited.
[0027] The composite plate and its preparation method and the heat spreader of the embodiment of the present application are described in detail below.
[0028] Figure 1 The structure diagram of the composite board 100 provided in the embodiment of the present application is shown in FIG. Figure 1 The composite board 100 includes a first copper foil 110 , a graphene layer 120 and a second copper foil 130 . The graphene layer 120 covers the first copper foil 110 , and the second copper foil 130 covers the graphene layer 120 .
[0029] In the present application, the number of crystal domains of the first copper foil 110 is less than or equal to 5 / cm2. For example, the number of crystal domains of the first copper foil 110 may be 5 / cm2, 4 / cm2, 3 / cm2, 2 / cm2 or 1 / cm2.
[0030] The first copper foil 110 with a crystal domain number less than or equal to 5 / cm2 has better thermal conductivity and electrical conductivity.
[0031] In some embodiments of the present application, the thickness of the first copper foil 110 may be 3-150 μm, for example, 3 μm, 5 μm, 8 μm, 18 μm, 28 μm, 36 μm, 42 μm, 70 μm, 100 μm, 150 μm, etc. The thickness of the first copper foil 110 of 3-150 μm can make it have high strength and good thermal conductivity and electrical conductivity.
[0032] In other embodiments of the present application, the thickness of the first copper foil 110 may be other values, which may be set according to the purpose and usage scenario of the composite board 100 .
[0033] In the present application, the first copper foil 110 having a crystal domain number less than or equal to 5 / cm2 can be prepared by the following method:
[0034] In an inert atmosphere, the electrolytic copper foil or rolled copper foil is heated to 800-1075°C and then annealed in a reducing atmosphere.
[0035] As an example, the inert atmosphere may be N2, Ar or He, etc.; the electrolytic copper foil or rolled copper foil is heated to 800-1075°C and then annealed in a reducing atmosphere.
[0036] For example, electrolytic copper or rolled copper (thickness 3-150 μm, number of domains > 10,000 / cm 2 ) is sent into an annealing device, and an inert gas such as N2, Ar or He is introduced to increase the temperature;
[0037] When the temperature in the annealing equipment reaches 800-1075°C, a reducing gas such as H2 or CO is introduced to start annealing. The above high temperature annealing method can be used to obtain a copper foil with a large crystal domain, and then the copper foil is selected, for example, a copper foil with a crystal domain number N less than or equal to 5 per square centimeter, that is, N≤5 / cm 2 .
[0038] It should be noted that, in other embodiments of the present application, the above-mentioned high-temperature annealing method may not be used to prepare the ultra-large crystal domain copper foil. For example, the ultra-large crystal domain copper foil may be obtained by commercial methods.
[0039] As described above, the graphene layer 120 covers the first copper foil 110 , and the graphene layer 120 and the first copper foil 110 can increase the thermal and electrical conductivity of the composite board 100 .
[0040] In the embodiment of the present application, the graphene layer 120 can be prepared by chemical vapor deposition.
[0041] For example, the first copper foil 110 is placed in a furnace, CH 4 and H 2 are introduced, and the first copper foil 110 is used as a substrate to grow a single layer or multiple layers of graphene to obtain the graphene layer 120 .
[0042] In some embodiments of the present application, the hardness of the first copper foil 110 and the graphene layer 120 can be set to 30-60 HV by setting the thickness of the graphene layer 120; in other words, the hardness of the first copper foil 110 and the graphene layer 120 together is 30-60 HV, for example, 30 HV, 35 HV, 40 HV, 50 HV or 60 HV, etc.
[0043] In other embodiments of the present application, the graphene layer 120 may be prepared by other preparation methods, and the present application does not limit the preparation method.
[0044] The second copper foil 130 covers the graphene layer 120 . In the present application, the second copper foil 130 is an electrolytic copper foil. In other words, the second copper foil 130 is formed by electrolytic copper.
[0045] In this embodiment, a layer of copper is electroplated on the graphene layer 120 to form the second copper foil 130 .
[0046] In some embodiments of the present application, the thickness of the second copper foil 130 is 1-1000 μm. For example, the thickness of the second copper foil 130 may be 1 μm, 5 μm, 10 μm, 100 μm, 135 μm, 150 μm, 250 μm, 300 μm, 500 μm, etc.
[0047] In the embodiment of the present application, the second copper foil 130 has the same crystal domain and crystal plane index as the first copper foil 110 , and the same crystal domain size.
[0048] In an embodiment of the present application, the hardness of the second copper foil 130 , the graphene layer 120 , and the first copper foil 110 is 100-200 HV; for example, it may be 100 HV, 135 HV, 140 HV, 150 HV, 160 HV, 182 HV, 190 HV, 200 HV, etc.
[0049] In some embodiments of the present application, the thickness of the composite board 100 can be set according to the requirements, and multiple layers of graphene layers 120 and multiple layers of second copper foil 130 can be prepared, and the graphene layers 120 and the second copper foil 130 are arranged at intervals. In other words, the composite board 100 may include multiple layers of graphene layers 120 and multiple layers of second copper foil 130; a layer of second copper foil 130 is arranged between two adjacent layers of graphene layers 120. The graphene layer 120 is arranged on the first copper foil 110, and the second copper foil 130 is arranged on the graphene layer 120. In order to increase the thickness of the composite board 100, the graphene layer 120 can be continuously arranged on the second copper foil 130, and then the second copper foil 130 can be arranged on the graphene layer 120, and the arrangement is performed in sequence until the preset thickness is reached.
[0050] Accordingly, in the embodiment of the present application, the number of layers and thickness of the graphene layer 120 and the second copper foil 130 can be set according to specific requirements.
[0051] The composite plate 100 provided in the embodiment of the present application has at least the following advantages:
[0052] The composite board 100 includes a first copper foil 110 having a crystal domain number less than or equal to 5 / square centimeter, a second copper foil 130 formed by copper electroplating, and a graphene layer 120 located between the first copper foil 110 and the second copper foil 130; the graphene layer 120 has excellent tensile strength (>1GPa) and thermal conductivity (approximately 5000W / m·k in the transverse direction), which can reduce the thickness of the composite board 100 while improving its strength. The first copper foil 110 and the second copper foil 130 located on both sides of the graphene layer 120 can overcome the problem that the graphene layer 120 cannot be used as a structural material alone, and the first copper foil 110 having a smaller crystal domain number and the second copper foil 130 formed by electroplating combined with the graphene layer 120 will have a higher thermal conductivity.
[0053] The present application also provides a method for preparing the composite plate 100, which mainly comprises the following steps:
[0054] A graphene layer 120 is grown on the first copper foil 110; the number of crystal domains of the first copper foil 110 is less than or equal to 5 / cm2. The specific method of growing the graphene layer 120 on the first copper foil 110 is described above, for example, the graphene layer 120 is prepared by chemical vapor deposition. The method includes: placing the first copper foil 110 in a furnace, introducing CH4 and H2, using the first copper foil 110 as a substrate, and growing at least one layer of graphene to obtain the graphene layer 120. As an example, one, two or more layers of graphene can be grown to form the graphene layer 120.
[0055] Before growing the graphene layer 120 on the first copper foil 110, the first copper foil 110 is prepared. The first copper foil 110 with a crystal domain number less than or equal to 5 / cm2 can be prepared, for example, by a high-temperature annealing process; the process includes: electrolytic copper or rolled copper (thickness 3-150 μm, crystal domain number > 10000 / cm2) is added. 2 ) is sent into the annealing equipment, and an inert gas such as N2, Ar or He is introduced to increase the temperature; when the temperature is increased to 800℃-1075℃ (for example, it can be 800℃, 900℃, 1000℃, etc.), a reducing gas such as H2 or CO is introduced to start annealing.
[0056] After the graphene layer 120 is prepared, a second copper foil 130 is prepared on the graphene layer 120. In the present application, the second copper foil 130 is prepared by electroplating.
[0057] The preparation method provided in the embodiment of the present application can obtain the composite board 100 having the above advantages, and the second copper foil 130 obtained by the preparation method has the same number of crystal domains, consistent crystal plane index, and consistent crystal domain size as the first copper foil 110. The preparation method can improve the thermal conductivity of the composite board 100.
[0058] The present application also provides a vapor chamber, which is made by using the composite plate 100. For example, the vapor chamber can be made by welding the composite plate 100.
[0059] The heat spreader includes an upper cover plate and a lower cover plate, and a cavity is formed between the upper cover plate and the lower cover plate; in the present application, the upper cover plate and the lower cover plate are both made of the above-mentioned composite plate.
[0060] The embodiments of the present application do not limit the specific preparation method, shape and size of the heat sink, and can be configured according to needs and application scenarios.
[0061] The heat spreader provided in the present application has the advantages of the composite plate 100 described above, and has higher strength and better thermal conductivity.
[0062] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0063] Example 1
[0064] This embodiment provides a vapor chamber, which is mainly manufactured by the following steps:
[0065] S1, the original multi-grain boundary electrolytic copper or rolled copper (thickness 25μm, number of crystal domains> 10000 / cm 2 ) is sent into the annealing equipment and N2 is introduced to increase the temperature.
[0066] S2, the copper foil is sent to the annealing equipment, and when the temperature reaches 950°C, H2 is introduced to start annealing.
[0067] S3, after keeping at 950°C for 4h, a large-domain copper foil (first copper foil) is obtained, N≤5 / cm 2 , copper foil with a crystal domain number of 5 was selected for subsequent experiments.
[0068] S4, after keeping warm for 4 hours, introducing CH4 and H2, and growing at least one graphene layer on the ultra-large crystal domain copper foil substrate by CVD process; after preparing the graphene layer, measuring the hardness of the graphene layer and the first copper foil.
[0069] S5, on the grown graphene layer, a second copper foil is prepared by copper electroplating process, the copper of the second copper foil has the same crystal plane index as the above-mentioned ultra-large crystal domain, the crystal domain size is consistent, the electroplated copper thickness is 150μm, and a composite board is obtained after preparing the second copper foil, and the hardness of the composite board is 100HV.
[0070] S6, using the composite plate as the upper / lower cover plate material, welding it into a vacuum cavity structure with a microstructure on the inner wall to obtain a heat spreader.
[0071] Examples 2-5 and Comparative Examples 1-4
[0072] Examples 2-5 and Comparative Examples 1-4 respectively provide a vapor chamber, which differs from Example 1 in that first copper foils with different numbers of crystal domains are selected and made into composite plates for subsequent experiments. See Table 1 for details.
[0073] Test Case
[0074] The composite boards of Examples 1-5 and Comparative Examples 1-4 were tested, and the test results are shown in Table 1.
[0075] (1) Crystal domain number detection: Observe under a metallographic microscope and randomly select the number of grain boundaries within a range of 10*10mm.
[0076] (2) Hardness: GB-T4340.1.
[0077] (3) Copper purity and oxygen content testing: GB / T 5121.
[0078] (4) Thermal conductivity test: GB / T 22588-2008.
[0079] Table 1
[0080]
[0081]
[0082] It can be seen from Table 1 that the composite plate provided in the embodiment of the present application has higher hardness and higher thermal conductivity than the composite plate provided in the comparative example, and can be used as a high-strength and high-thermal-conductivity heat spreader.
[0083] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A composite board, characterized in that: The composite board comprises a first copper foil, a graphene layer and a second copper foil which are stacked in sequence; Wherein, the first copper foil has a crystal domain number of 3 to 5 per square centimeter; The second copper foil is electroplated copper, and the second copper foil has the same number of crystal domains as the first copper foil; The thickness of the first copper foil is 3 μm-150 μm, and the thickness of the second copper foil is 150 μm-350 μm.
2. The composite panel according to claim 1, characterized in that: The hardness of the first copper foil and the graphene layer is 30HV-60HV.
3. The composite panel according to claim 1, characterized in that: The hardness of the composite plate is 100HV-200HV.
4. The composite board according to any one of claims 1 to 3, characterized in that: The composite board includes a plurality of the graphene layers and a plurality of the second copper foils; the graphene layers and the second copper foils are stacked and cross-arranged, and the graphene layers cover the first copper foils.
5. The method for preparing the composite board according to any one of claims 1 to 4, characterized in that: include: growing a graphene layer on the first copper foil; preparing a second copper foil on the graphene layer by electroplating; Wherein, the number of crystal domains of the first copper foil is 3 to 5 per square centimeter.
6. The method for preparing a composite board according to claim 5, characterized in that: Before growing the graphene layer on the first copper foil, the first copper foil is also prepared, which specifically includes: In an inert atmosphere, the electrolytic copper foil or the rolled copper foil is heated to 800°C-1075°C and then annealed in a reducing atmosphere.
7. The method for preparing a composite board according to claim 5, characterized in that: In the step of growing the graphene layer on the first copper foil, the graphene layer is grown by chemical vapor deposition.
8. A heat spreader, characterized in that: The heat sink is formed by connecting the composite plates according to any one of claims 1 to 4.
Citation Information
Patent Citations
Method for cloning and growing single crystal metal
CN111621846A
Bending-resistant copper foil, preparation method of bending-resistant copper foil, and FPC flexible circuit board
CN112064071A
Vapor chamber
CN214218863U
KR1018513140000B1