High-frequency low-loss rare earth soft magnetic composite material and preparation method thereof

CN118919206APending Publication Date: 2024-11-08ZHEJIANG UNIV +1

Patent Information

Application Number
CN202411203137.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

然而,现有软磁材料的磁导率和截止频率无法同时提升,难以满足第三代半导体技术频段的需求,因此开发新型软磁材料以适应高频应用具有很大的必要性

Benefits of technology

[0020] 1) The rare earth soft magnetic composite material of the present invention has high saturation magnetic flux density, high cut-off frequency and low power loss, can be used in high frequency bands above 10MHz, and can meet the requirements of power devices in terms of high frequency, high efficiency and miniaturization;

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-frequency low-loss rare earth soft magnetic composite material and a preparation method thereof. The material is a compound of rare earth compound Ce2 (FexCo1-x) 17 powder, magnetic metal powder and an adhesive. The preparation method mainly comprises the steps of ingredient smelting, homogenizing annealing, crushing and ball milling, surface treatment, insulating coating, tape casting, drying and curing, hot press molding and the like. The rare earth soft magnetic composite material has the characteristics of high saturation magnetic flux density, high cut-off frequency, low loss and the like, is easy to process and form, is controllable in shape, size and thickness, can meet the requirements of power devices on high frequency, high efficiency and miniaturization, and has a wide application prospect in modern electronic power equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-frequency, low-loss rare earth soft magnetic composite material and a preparation method thereof, and belongs to the field of new materials and new processes for electronic components. Background Art

[0002] Soft magnetic materials are widely used in electronic power equipment such as inductors, transformers and motors, and play a vital role in the field of energy conversion and transmission. With the rapid development of the electronic information industry, the power density and operating frequency of power electronic devices are constantly increasing, which puts forward requirements for high frequency, high efficiency and miniaturization of supporting soft magnetic materials. The third-generation wide bandgap semiconductor power devices represented by SiC and GaN require soft magnetic materials to maintain high magnetic permeability and high magnetic flux density above 10MHz. However, the magnetic permeability and cutoff frequency of existing soft magnetic materials cannot be improved at the same time, and it is difficult to meet the requirements of the third-generation semiconductor technology frequency band. Therefore, it is very necessary to develop new soft magnetic materials to adapt to high-frequency applications.

[0003] At present, the main problems faced by soft magnetic materials in high-frequency applications are low cutoff frequency, rapid attenuation of magnetic permeability with increasing frequency, and sharp increase in eddy current loss and residual loss. Traditional high-frequency soft magnetic materials are mainly ferrites, which have low saturation magnetization and cutoff frequency, which is not conducive to the miniaturization and integration of electronic devices, and it is difficult to meet the application requirements of frequency bands above 10MHz. Unlike ferrite materials, rare earth soft magnetic materials have multiple easy magnetization axes in the same crystal plane, and there are two anisotropic equivalent fields in the crystal, in-plane and out-of-plane. This magnetic property effectively increases the cutoff frequency of soft magnetic materials and enables them to maintain a high magnetic permeability at higher frequencies.

[0004] Rare earth soft magnetic materials are a series of rare earth-3d metal intermetallic compounds with soft magnetic properties formed by rare earth (R) and transition metal (M) elements. Currently, they mainly include R2[(Fe,Co) 1-x M x ] 17 Compounds and R2(Fe,Co) mainly in the 2:14:1 type 14 B compound. In the megahertz frequency band, eddy current loss is the main reason for the power loss of rare earth soft magnetic materials. Eddy current loss is proportional to the square of the operating frequency and inversely proportional to the resistivity. Therefore, in order to reduce the high-frequency loss of rare earth soft magnetic materials, it is necessary to perform insulation coating treatment on them to prepare rare earth soft magnetic composite materials with high resistivity.

[0005] The coated rare earth soft magnetic composite material can have excellent properties such as high saturation flux density, high cutoff frequency and low loss, and is easy to process and shape. It can better meet the requirements of modern electronic devices in high frequency, high efficiency and miniaturization, and has broad application prospects in modern electronic power equipment. Summary of the invention

[0006] In order to solve the problems in the prior art, the present invention proposes a high-frequency, low-loss rare earth soft magnetic composite material and a preparation method thereof.

[0007] The high-frequency low-loss rare earth soft magnetic composite material of the present invention is a rare earth intermetallic compound Ce2(Fe x Co 1-x ) 17 A composite of powder, magnetic metal powder and adhesive, wherein 0<x≤1, the magnetic metal powder is one or more of reduced iron powder, carbonyl iron powder, iron-silicon-aluminum alloy powder, iron-nickel alloy powder, iron-nickel-molybdenum alloy powder, iron-silicon-boron amorphous powder, iron-silicon alloy powder or iron-silicon-nickel alloy powder, and the adhesive is one or more of polyurethane, epoxy resin, W-6C magnetic powder glue, phenolic resin, polyvinyl alcohol, polyvinyl butyral or glass powder.

[0008] Among them, rare earth intermetallic compounds Ce2(Fe x Co 1-x ) 17 The mass percentage content of the powder is 5%-45%, the mass percentage content of the magnetic metal powder is 45%-85%, and the mass percentage content of the adhesive is 5%-10%.

[0009] The high-frequency and low-loss rare earth soft magnetic composite material of the present invention has high-frequency and low-loss soft magnetic properties, a cut-off frequency of more than 50 MHz, and a power loss of less than 3000 kW·m at 5 MHz and 10 mT. -3 .

[0010] The present invention provides a method for preparing a high-frequency, low-loss rare earth soft magnetic composite material, the preparation method comprising the following steps:

[0011] 1) Ingredient smelting: According to the rare earth compound Ce2(Fe x Co 1-x ) 17 , and the alloy components of the magnetic metals are respectively prepared with raw materials, and are smelted separately in a high vacuum environment to obtain two alloy ingots, which are then sealed and stored in a vacuum quartz tube;

[0012] 2) Homogenization annealing: Place the quartz tube in a muffle furnace for homogenization annealing at a temperature of 1000°C. After annealing, water cool the quartz tube to room temperature.

[0013] 3) Crushing and ball milling: Coarsely crush the two alloy ingots, then add ball milling media, surfactants and protective solvents to each, and ball mill the crushed particles for 4 to 6 hours, with a 6-minute interval between positive and negative rotations, and a ball milling speed of 250 r / min to obtain two kinds of metal magnetic powders;

[0014] 4) Surface treatment: high temperature oxidation or chemical passivation of two kinds of metal magnetic powder to form a high resistance coating layer on the surface, the oxidation temperature is 150-350℃, the passivation temperature is 25-100℃, and the insulation or passivation time is 10-30min;

[0015] 5) Insulation coating: the two treated metal magnetic powders are mixed, and then an organic solvent, a dispersant and the binder are added, and ultrasonic dispersion treatment is performed for 10 to 30 minutes to obtain a mixed slurry;

[0016] 6) Tape casting: inject the mixed slurry into a tape casting machine, with a scraper height of 0.4-2 mm and a tape casting speed of 0.2-2 cm / s to obtain a magnetic powder blank;

[0017] 7) Drying and curing: Dry the green blank at room temperature with a relative humidity of 30% to 50% to a thickness of 0.1 to 1 mm, and then cure the green blank in an inert gas at a curing temperature of 80-250° C. for 1 to 5 hours;

[0018] 8) Hot pressing: Use a stamping die to punch the blank into a ring with an outer diameter of 12 mm and an inner diameter of 6 mm. After the rings are stacked, hot pressing is performed at a pressure of 200 to 300 MPa, a pressing temperature of 50 to 100°C, and a holding time of 10 to 30 min. Then, the rare earth soft magnetic composite material is naturally cooled and demolded to obtain.

[0019] Compared with existing soft magnetic materials, the present invention has the following advantages:

[0020] 1) The rare earth soft magnetic composite material of the present invention has high saturation magnetic flux density, high cut-off frequency and low power loss, can be used in high frequency bands above 10MHz, and can meet the requirements of power devices in terms of high frequency, high efficiency and miniaturization;

[0021] 2) The rare earth soft magnetic composite material of the present invention is easy to process and shape, and its shape, size and thickness are controllable, which can meet the diverse shape requirements of electronic devices;

[0022] 3) The method for preparing the rare earth soft magnetic composite material of the present invention can reduce the thickness of the magnetic material through the tape casting process, and at the same time enhance the planar anisotropy, which is beneficial to reduce eddy current loss and increase the cut-off frequency. DETAILED DESCRIPTION

[0023] The present invention is further described and illustrated below in conjunction with specific embodiments. The embodiments are merely exemplary of the present disclosure and do not define the scope of limitation. The technical features of each embodiment of the present invention may be combined accordingly without conflicting with each other.

[0024] In the high-frequency low-loss rare earth soft magnetic composite material of the present invention, the rare earth intermetallic compound Ce2(Fe x Co 1-x ) 17 The mass percentage content of the powder is 5%-45%, the mass percentage content of the magnetic metal powder is 45%-85%, and the mass percentage content of the adhesive is 5%-10%. The composite material can be prepared specifically according to the following preparation method:

[0025] 1) Ingredient smelting: According to the rare earth compound Ce2(Fe x Co 1-x ) 17 , and the alloy composition ratio of the magnetic metals are respectively prepared with raw materials, the purity of the raw materials is higher than 99.9%, and two alloy ingots are obtained by smelting in a high vacuum environment, and then sealed and stored in a vacuum quartz tube;

[0026] 2) Homogenization annealing: Place the quartz tube in a muffle furnace for homogenization annealing at a temperature of 1000°C for 7 days. After annealing, water cool the quartz tube to room temperature.

[0027] 3) Crushing and ball milling: The two alloy ingots were coarsely crushed, and then the ball milling medium, surfactant and protective solvent were added to the two crushed particles, and the crushed particles were ball milled for 4 to 6 hours, with a 6-minute interval and a forward and reverse rotation. The ball milling speed was 250 r / min to obtain two metal magnetic powders (i.e., rare earth intermetallic compound Ce2(Fe x Co 1-x ) 17 powders and magnetic metal powders);

[0028] 4) Surface treatment: high temperature oxidation or chemical passivation of two kinds of metal magnetic powder to form a high resistance coating layer on the surface, the oxidation temperature is 150-350℃, the passivation temperature is 25-100℃, and the insulation or passivation time is 10-30min;

[0029] 5) Insulation coating: the two treated metal magnetic powders are mixed according to the formula ratio, and then an organic solvent, a dispersant and a binder in the formula are added, and ultrasonic dispersion treatment is performed for 10 to 30 minutes to obtain a mixed slurry;

[0030] 6) Tape casting: inject the mixed slurry into a tape casting machine, with a scraper height of 0.4-2 mm and a tape casting speed of 0.2-2 cm / s to obtain a magnetic powder blank;

[0031] 7) Drying and curing: Dry the green blank at room temperature with a relative humidity of 30% to 50% to a thickness of 0.1 to 1 mm, and then cure the green blank in an inert gas at a curing temperature of 80-250° C. for 1 to 5 hours;

[0032] 8) Hot pressing: Use a stamping die to punch the blank into a ring with an outer diameter of 12 mm and an inner diameter of 6 mm. After the rings are stacked, hot pressing is performed at a pressure of 200 to 300 MPa, a pressing temperature of 50 to 100°C, and a holding time of 10 to 30 min. Then, the rare earth soft magnetic composite material is naturally cooled and demolded to obtain.

[0033] According to a preferred embodiment of the present invention, the ball milling medium can be a stainless steel ball, a zirconia ball or an agate ball with a diameter of 1 to 10 mm; the mass ratio of the ball milling medium to the ball milling material is 10:1 to 25:1. The surfactant can be dimethyl silicone oil, polyethylene glycol ester-20, oleic acid or oleylamine, and the protective solvent can be n-hexane, ethanol or n-heptane; the volume ratio of the surfactant and the protective solvent is preferably 1:50, and the mass ratio of the two (surfactant and protective solvent) to the ball milling material is 10:1 to 25:1. The magnetic metal powder is one or more of reduced iron powder, carbonyl iron powder, iron-silicon-aluminum alloy powder, iron-nickel alloy powder, iron-nickel-molybdenum alloy powder, iron-silicon-boron amorphous powder, iron-silicon alloy powder or iron-silicon-nickel alloy powder; rare earth compound Ce2 (Fe x Co 1-x ) 17 When the powder and magnetic metal powder are mixed, they are mixed at a mass ratio of 1:1 to 1:17. The chemical passivation is nitric acid passivation, sodium nitrate passivation or phosphoric acid passivation, and the mass fraction of the passivation liquid is 0.1% to 10%. The organic solvent can be ethanol, methyl ethyl ketone, butanone, acetone, trichloroethylene, xylene, and the volume fraction of the organic solvent is 30% to 80% of the mixed slurry. The dispersant can be herring oil, phosphate ester, trioleyl glycerol or triethanolamine, and the volume fraction of the dispersant is 0.2% to 5% of the mixed slurry.

[0034] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments:

[0035] Embodiment 1:

[0036] 1) Ingredient smelting: In this embodiment, the rare earth compound Ce2(Fe x Co 1-x ) 17wherein x is selected as 0.8, and the magnetic metal powder is sendust magnetic powder (85wt.% Fe, 9.6wt.% Si, 5.4wt.% Al); raw materials are prepared according to the above alloy component ratios, and the purity of the raw materials is higher than 99.9%, and two alloy ingots are obtained by smelting in a high vacuum environment, and then sealed and stored in a vacuum quartz tube;

[0037] 2) Homogenization annealing: Place the quartz tube in a muffle furnace for homogenization annealing at a temperature of 1000°C for 7 days. After annealing, water cool the quartz tube to room temperature.

[0038] 3) Crushing and ball milling: The two alloy ingots were coarsely crushed, and then 100.0 g of zirconia balls with a diameter of 5 mm were added to the two crushed particles as ball milling media, 0.1 g of dimethyl silicone oil as a surfactant, and 100 ml of n-hexane as a protective solvent, and the crushed particles were ball milled for 4 h, with a forward and reverse rotation interval of 6 min, and a ball milling speed of 250 r / min to obtain two metal magnetic powders;

[0039] 4) Surface treatment: Surface oxidation Ce2(Fe 0.8 Co 0.2 ) 17 Magnetic powder, oxidation temperature is 250℃, passivation of sendust magnetic powder with 10% nitric acid solution, passivation temperature is 40℃, passivation time is 10min;

[0040] 5) Insulation coating: The treated Ce2(Fe 0.8 Co 0.2 ) 17 and Sendust magnetic powder in a mass ratio of 1:9, 5 ml of acetone, 0.1 g of phosphate ester and 0.7 g of polyurethane were added to 10.0 g of the mixed magnetic powder, and ultrasonic dispersion treatment was performed for 30 min to obtain a mixed slurry;

[0041] 6) Tape casting: inject the mixed slurry into a tape casting machine, with a scraper height of 0.4 mm and a casting speed of 0.5 cm / s to obtain a magnetic powder blank;

[0042] 7) Drying and curing: Dry the green blank at room temperature with a relative humidity of 30% to a thickness of 0.4 mm, and then cure the green blank in an inert gas at a curing temperature of 100° C. for 5 hours;

[0043] 8) Hot pressing: Use a stamping die to punch the blank into a ring with an outer diameter of 12 mm and an inner diameter of 6 mm. After the rings are stacked, hot pressing is performed at a pressure of 300 MPa, a pressing temperature of 90°C, and a holding time of 10 min. Then, the rare earth soft magnetic composite material is naturally cooled and demolded to obtain.

[0044] The frequency characteristics of the rare earth soft magnetic composite material were tested, and the cut-off frequency reached 65.7MHz. The power loss at 5MHz and 10mT was 1681.3kW·m -3 .

[0045] Embodiment 2:

[0046] 1) Ingredient smelting: In this embodiment, the rare earth compound Ce2(Fe x Co 1-x ) 17 wherein x is selected as 0.5, and the magnetic metal powder is iron-nickel-molybdenum magnetic powder (17wt.% Fe, 81wt.% Ni, 2wt.% Mo); raw materials are prepared according to the above alloy component ratios, the purity of the raw materials is higher than 99.9%, and two alloy ingots are obtained by smelting in a high vacuum environment, and then sealed and stored in a vacuum quartz tube;

[0047] 2) Homogenization annealing: Place the quartz tube in a muffle furnace for homogenization annealing at a temperature of 1000°C for 7 days. After annealing, water cool the quartz tube to room temperature.

[0048] 3) Crushing and ball milling: The two alloy ingots were coarsely crushed, and then 100.0 g of zirconia balls with a diameter of 5 mm were added to the two crushed particles as ball milling media, 0.1 g of oleylamine as a surfactant, and 100 ml of ethanol as a protective solvent. The crushed particles were ball milled for 6 h, with a forward and reverse rotation interval of 6 min, and a ball milling speed of 250 r / min to obtain two metal magnetic powders;

[0049] 4) Surface treatment: Surface oxidation Ce2(Fe 0.5 Co 0.5 ) 17 Magnetic powder, oxidation temperature is 300℃, iron-nickel-molybdenum magnetic powder is passivated with phosphoric acid solution with a mass fraction of 0.6%, the passivation temperature is 60℃, and the passivation time is 30min;

[0050] 5) Insulation coating: The treated Ce2(Fe 0.5 Co 0.5 ) 17 and iron-nickel-molybdenum magnetic powders in a mass ratio of 1:5, 8 ml of acetone, 0.5 g of trioleyl glycerol and 1.0 g of phenolic resin were added to 10.0 g of the mixed magnetic powders, and ultrasonic dispersion treatment was performed for 30 min to obtain a mixed slurry;

[0051] 6) Tape casting: inject the mixed slurry into a tape casting machine with a scraper height of 0.6 mm and a casting speed of 1.0 cm / s to obtain a magnetic powder blank;

[0052] 7) Drying and curing: Dry the green blank at room temperature with a relative humidity of 45% to a thickness of 0.6 mm, and then cure the green blank in an inert gas at a curing temperature of 150° C. for 3 hours;

[0053] 8) Hot pressing: Use a stamping die to punch the blank into a ring with an outer diameter of 12 mm and an inner diameter of 6 mm. After the rings are stacked, hot pressing is performed at a pressure of 250 MPa, a pressing temperature of 80°C, and a holding time of 30 min. Then, the rare earth soft magnetic composite material is naturally cooled and demolded to obtain.

[0054] The frequency characteristics of the rare earth soft magnetic composite material were tested. The cutoff frequency was 57.6MHz, and the power loss at 5MHz and 10mT was 2105.6kW·m -3 .

[0055] Embodiment 3:

[0056] 1) Ingredient smelting: In this embodiment, the rare earth compound Ce2(Fe x Co 1-x ) 17 wherein x is selected as 0.7, and the magnetic metal powder is iron-silicon-nickel magnetic powder (85wt.% Fe, 5wt.% Si, 10wt.% Ni); raw materials are prepared according to the above alloy component ratios, the purity of the raw materials is higher than 99.9%, and two alloy ingots are obtained by smelting in a high vacuum environment, and then sealed and stored in a vacuum quartz tube;

[0057] 2) Homogenization annealing: Place the quartz tube in a muffle furnace for homogenization annealing at a temperature of 1000°C for 7 days. After annealing, water cool the quartz tube to room temperature.

[0058] 3) Crushing and ball milling: The two alloy ingots were coarsely crushed, and then 100.0 g of a stainless steel ball with a diameter of 10 mm was added to the two crushed particles as a ball milling medium, 0.1 g of dimethyl silicone oil as a surfactant, and 100 ml of n-heptane as a protective solvent, and the crushed particles were ball milled for 4.5 h, with a forward and reverse rotation interval of 6 min, and a ball milling speed of 250 r / min to obtain two metal magnetic powders;

[0059] 4) Surface treatment: Surface oxidation Ce2(Fe 0.7 Co 0.3 ) 17 Magnetic powder, oxidation temperature is 250℃, passivation of Fe-Si-Ni magnetic powder with 10% sodium nitrate solution, passivation temperature is 40℃, and passivation time is 10min;

[0060] 5) Insulation coating: The treated Ce2(Fe 0.7 Co 0.3 ) 17and iron silicon nickel magnetic powder in a mass ratio of 1:1, 4 ml of xylene, 0.1 g of phosphate and 0.7 g of polyurethane were added to 10.0 g of the mixed magnetic powder, and ultrasonic dispersion treatment was performed for 20 min to obtain a mixed slurry;

[0061] 6) Tape casting: the mixed slurry is injected into a tape casting machine, the scraper height is 0.4 mm, and the casting speed is 0.6 cm / s to obtain a magnetic powder blank;

[0062] 7) Drying and curing: Dry the green blank at room temperature with a relative humidity of 40% to a thickness of 0.4 mm, and then cure the green blank in an inert gas at a curing temperature of 150° C. for 3 hours;

[0063] 8) Hot pressing: Use a stamping die to punch the blank into a ring with an outer diameter of 12 mm and an inner diameter of 6 mm. After the rings are stacked, hot pressing is performed at a pressure of 300 MPa, a pressing temperature of 80°C, and a holding time of 25 min. Then, the rare earth soft magnetic composite material is naturally cooled and demolded to obtain.

[0064] The frequency characteristics of the rare earth soft magnetic composite material were tested. The cut-off frequency was 263.4MHz, and the power loss was 2872.4kW·m at 5MHz and 10mT. -3 .

[0065] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. For ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A high-frequency, low-loss rare earth soft magnetic composite material, characterized in that: The composite material is a rare earth compound Ce2(Fe x Co 1-x ) 17 A composite of powder, magnetic metal powder and adhesive, wherein 0<x≤1, the magnetic metal powder is one or more of reduced iron powder, carbonyl iron powder, iron-silicon-aluminum alloy powder, iron-nickel alloy powder, iron-nickel-molybdenum alloy powder, iron-silicon-boron amorphous powder, iron-silicon alloy powder or iron-silicon-nickel alloy powder, and the adhesive is one or more of polyurethane, epoxy resin, W-6C magnetic powder glue, phenolic resin, polyvinyl alcohol, polyvinyl butyral or glass powder.

2. The high-frequency, low-loss rare earth soft magnetic composite material according to claim 1, characterized in that: The composite material has high-frequency, low-loss soft magnetic properties, a cut-off frequency of more than 50 MHz, and a power loss of less than 3000 kW·m at 5 MHz and 10 mT. -3 .

3. The high-frequency, low-loss rare earth soft magnetic composite material according to claim 1, characterized in that: In composite materials, rare earth intermetallic compounds Ce2(Fe x Co 1-x ) 17 The mass percentage content of the powder is 5%-45%, the mass percentage content of the magnetic metal powder is 45%-85%, and the mass percentage content of the adhesive is 5%-10%.

4. The method for preparing a high-frequency, low-loss rare earth soft magnetic composite material according to any one of claims 1 to 3, characterized in that: The following steps are involved: 1) Ingredient smelting: According to the rare earth compound Ce2(Fe x Co 1-x ) 17 , and the alloy components of the magnetic metals are respectively prepared with raw materials, and are smelted separately in a high vacuum environment to obtain two alloy ingots, which are then sealed and stored in a vacuum quartz tube; 2) Homogenization annealing: Place the quartz tube in a muffle furnace for homogenization annealing at a temperature of 1000°C. After annealing, water cool the quartz tube to room temperature. 3) Crushing and ball milling: Coarsely crush the two alloy ingots, then add ball milling media, surfactants and protective solvents to each, and ball mill the crushed particles for 4 to 6 hours, with a 6-minute interval between positive and negative rotations, and a ball milling speed of 250 r / min to obtain two kinds of metal magnetic powders; 4) Surface treatment: high temperature oxidation or chemical passivation of two kinds of metal magnetic powder to form a high resistance coating layer on the surface, the oxidation temperature is 150-350℃, the passivation temperature is 25-100℃, and the heat preservation or passivation time is 10-30min; 5) Insulation coating: the two treated metal magnetic powders are mixed, and then an organic solvent, a dispersant and the binder are added, and ultrasonic dispersion treatment is performed for 10 to 30 minutes to obtain a mixed slurry; 6) Tape casting: inject the mixed slurry into a tape casting machine, with a scraper height of 0.4-2 mm and a tape casting speed of 0.2-2 cm / s to obtain a magnetic powder blank; 7) Drying and curing: Dry the green blank at room temperature with a relative humidity of 30% to 50% to a thickness of 0.1 to 1 mm, and then cure the green blank in an inert gas at a curing temperature of 80-250° C. for 1 to 5 hours; 8) Hot pressing: Use a stamping die to punch the blank into a ring with an outer diameter of 12 mm and an inner diameter of 6 mm. After the rings are stacked, hot pressing is performed at a pressure of 200 to 300 MPa, a pressing temperature of 50 to 100°C, and a holding time of 10 to 30 min. Then, the rare earth soft magnetic composite material is naturally cooled and demolded to obtain.

5. The preparation method according to claim 4, characterized in that: The ball milling medium is a stainless steel ball, a zirconium oxide ball or an agate ball with a diameter of 1 to 10 mm; the mass ratio of the ball milling medium to the ball milling material is 10:1 to 25:

1.

6. The preparation method according to claim 4, characterized in that: The surfactant in step 3) is dimethyl silicone oil, polyethylene glycol ester-20, oleic acid or oleylamine, and the protective solvent is n-hexane, ethanol or n-heptane; the volume ratio of the surfactant to the protective solvent is 1:20 to 1:50, and the mass ratio of the two to the ball-milled material is 10:1 to 25:

1.

7. The preparation method according to claim 4, characterized in that: In step 5), Ce2(Fe x Co 1-x ) 17 The powder and the magnetic metal powder are mixed in a mass ratio of 1:1 to 1:

17.

8. The preparation method according to claim 4, characterized in that: The chemical passivation is nitric acid passivation, sodium nitrate passivation or phosphoric acid passivation, and the mass fraction of the passivation solution is 0.1% to 10%.

9. The preparation method according to claim 4, characterized in that: The organic solvent is ethanol, methyl ethyl ketone, butanone, acetone, trichloroethylene and xylene, and the volume fraction of the organic solvent is 30% to 80% of the mixed slurry.

10. The preparation method according to claim 4, characterized in that: The dispersant is herring oil, phosphate, trioleylglycerol or triethanolamine, and the volume fraction of the dispersant is 0.2% to 5% of the mixed slurry.

Citation Information

Patent Citations

  • Tape-casting temperature isostatic pressing composite molding preparation method of metal soft magnetic composite material

    CN104036906A

  • Diphasic nanocrystalline high-frequency soft magnetic material and preparation method thereof

    CN104319050A

  • Preparation method of soft magnetic composite material with high saturation magnetic flux density and high magnetic conductivity

    CN104934180A

Cited By

  • 2 / 17 type rare earth soft magnetic composite material based on high-abundance rare earth resources and preparation method of 2 / 17 type rare earth soft magnetic composite material

    CN121204551A

  • 2:17 type rare earth soft magnetic composite material based on high-abundance rare earth resources and preparation method thereof

    CN121204551B

  • High-plane-orientation rare earth soft magnetic nanocrystal and preparation method thereof

    CN121394093A