Narrow gap laser wire-filling welding equipment and method thereof
By using angle-adjustable protective air pipes, carbide slag cleaning brushes and high-power lasers in narrow gap laser wire filler welding equipment, the problem of welding slag influence in medium-thick plate welding has been solved, and welding quality and efficiency have been improved. It avoids unfusion and pore defects between layers and improves welding efficiency.
Patent Information
- Application Number
- CN202110306217.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-23
AI Technical Summary
Existing technology In the welding of medium-thick plates, the grooves of narrow-gap laser filler welding equipment are narrow, resulting in strict welding requirements. The welding slag attached to the weld bead and side walls after welding affects the quality of re-welding, and traditional methods are difficult to be effective. Remove welding slag, which causes defects such as lack of fusion between layers and pores.
Narrow gap laser wire filling welding equipment including a laser head, protective air pipe, wire feeding mechanism, slag cleaning brush and air knife tube is used. The mixed gas is delivered through the angle-adjustable protective air tube, and the slag cleaning brush and air knife driven by a carbide motor are used. The pipe is cleaned of welding slag, and the wire feeding mechanism adopts a front wire feeding method, combined with high-power laser and optimized gas protection to ensure welding quality and efficiency.
It improves the smoothness and welding quality of the workpiece after welding, effectively prevents welding slag from destroying the welding pool, solves the problem of non-fusion between layers and pores, improves the welding efficiency and the slag removal rate of multi-layer welding, and ensures welding High-quality joining of panels.
Smart Images

Figure CN112935549B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a welding device and a method thereof, in particular to a narrow gap laser wire-filling welding device and a method thereof. Background Art
[0002] In the field of welding of metal materials, especially in the manufacturing of equipment such as mining machinery, aerospace, nuclear power, shipbuilding, and automobile manufacturing, there is welding of large medium and thick wall components.
[0003] At present, the main methods for welding medium and thick plates are manual welding, submerged arc welding and gas shielded welding, but they often produce coarse grains in the weld area and heat-affected zone. Compared with traditional arc welding, narrow gap laser wire welding technology has the characteristics of small heat-affected zone, small welding deformation, high welding efficiency, and can even further refine the grains to improve the mechanical properties of the joint. The advantages are more obvious in the welding of thick plates. However, when welding medium and thick plates, due to the narrow groove of narrow gap laser wire welding, the welding requirements are more stringent. The welding slag attached to the weld and side wall after welding seriously affects the welding quality when welding again. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the defects of the prior art and provide a narrow gap laser wire filling welding device and a method thereof.
[0005] In order to solve the above technical problems, the present invention provides narrow gap laser wire-filling welding equipment, including a laser head, a protective air pipe fixed on the laser head, a wire feeding mechanism, a slag cleaning brush and an air knife tube.
[0006] As an improvement, the shielding gas pipe is equipped with an angle adjuster; the shielding gas pipe conveys one or more mixed gases of Ar, CO2 and He; during the welding process, under certain conditions such as voltage and wire feeding speed, when the shielding gas composition changes, that is, with the increase of helium content, the side wall fusion depth increases, the welded workpiece has a smooth morphology and good welding quality. 25% He + 75% CO2 (volume ratio) has the largest depth of penetration and width, and the best welding effect.
[0007] As an improvement, the slag cleaning brush is made of hard alloy and is driven by a motor to rotate for slag cleaning; the direction of the slag cleaning brush and the air knife tube is opposite to the welding direction, which effectively prevents the blown-away welding slag from damaging the welding molten pool.
[0008] As an improvement, the wire feeding mechanism is provided with an adjuster; the angle between the wire feeding mechanism and the welding direction is acute, and the front wire feeding method is used for narrow gap laser wire filling welding. In the process of narrow gap laser wire filling welding. The laser direction, the wire filling direction and the direction of the shielding gas introduction form different combinations. Front wire feeding and rear wire feeding are the two basic wire feeding methods for laser wire filling welding. Front wire feeding is to feed the front of the welding wire molten pool into the molten pool at an acute angle to the welding direction; rear wire feeding is to feed the welding wire from the rear of the molten pool and into the molten pool at an obtuse angle to the welding direction; side wire feeding is to feed the welding wire into the molten pool from both sides of the molten pool or both sides of the welding direction. The wire feeding method affects the heating principle of the welding wire and plays a decisive role in the melting and filling process of the welding wire. In post-wire welding, the energy cannot achieve rapid and sufficient melting of the welding wire, so the reaction between the welding wire and the matrix is insufficient, resulting in an unstable welding process and unsatisfactory weld formation. In front-wire welding, when the welding wire is far away from the laser beam, it mainly relies on the energy of metal vapor and photoplasma and the energy of the molten pool to melt. When it is close to the laser beam, the welding wire is directly irradiated by part of the laser and is further heated and melted. The melting is sufficient, the melting process of the welding wire is continuous and stable, and the welding wire first melts into the front molten pool and flows to the rear with the molten liquid. The welding wire can be evenly melted into the weld.
[0009] As an improvement, the laser beam emitted by the laser head and the welding wire of the wire feeding mechanism form an angle α, and the angle value is between 20 and 80°. Due to the small size of the groove, the welding wire needs to be extended into the bottom of the groove for welding. For deep grooves, since the diameter of the wire feeding nozzle is larger than the width of the upper surface of the groove, the welding wire can only be extended into the deep groove, and the welding wire needs to be extended by about 40mm. This places extremely high demands on the correction of the welding wire. If the welding wire swings during the welding process, the laser beam will not be able to irradiate the welding wire, resulting in unfused defects, which will directly affect the welding effect. Before welding, the wire feeding mechanism is arbitrarily adjusted in the direction of the wire feeding weld through the regulator, and the α angle is adjusted within a certain range. The optimal angle can be selected for wire feeding to ensure welding quality.
[0010] As an improvement, the welding equipment uses an IPG 4kW laser, the fiber core diameter is 200μm, the focusing lens diameter is 247mm, and the spot diameter at zero defocus is 160μm; during the welding process, the laser beam is prevented from directly hitting the workpiece, causing beam reflection and damage to the focusing lens. The laser beam is at an oblique angle to the workpiece surface, and the angle value is between 2 and 5°.
[0011] As an improvement, the air knife tube conveys a mixture of alcohol-water solution and Ar gas, which enables the welding slag to be cleaned while effectively protecting the weld.
[0012] As an improvement, it also includes a back plate protection gas pipe; the back plate protection gas pipe conveys N2 gas. There are two types of shielding gas, the first welding pool shielding gas and the back plate shielding gas. At present, 99.99% Ar is used for protection of the welding pool, and He+CO2 (volume ratio is 1:3) mixed gas can also be used for protection. During the welding process, the shielding gas is directly blown into the welding pool for protection. The back plate shielding gas is only turned on during the first blunt edge self-fusion welding to provide ventilation protection for the back of the welding plate. The shielding gas is 99.99% N2 gas. The angle β between the shielding gas pipe of the welding pool and the laser beam is adjustable between 20 and 80°. In the direction of the weld, it can be adjusted arbitrarily by the regulator.
[0013] At zero defocus, the spot diameter is 0.16mm, and the spot diameter is adjusted by a galvanometer, with a maximum diameter of 5mm. The galvanometer adjusts the spot diameter by adjusting the light path through the wobble of the laser head to achieve a straight line swing during the welding process, thereby improving the adaptability of the groove, eliminating pores through optical stirring, and promoting side wall fusion.
[0014] The present invention also provides a narrow gap laser wire-filling welding method, comprising the following steps:
[0015] Step (1): Assemble the workpiece to be welded, spot weld the back of the workpiece, and fix the workpiece to be welded;
[0016] Step (2): The laser head is moved to the starting point of the workpiece to be welded for alignment, so that the center of the light spot falls on the gap of the unwelded workpiece, and this spatial point is recorded to mark the end point of the welding;
[0017] Step (3): The front end of the welding wire is fed to the center of the light spot by a wire feeder so that the light spot falls on the front end of the welding wire; during welding, the gas feeding, wire feeding and light feeding systems are turned on simultaneously;
[0018] Step (4): The back protection air pipe is opened when the first laser self-melting welding starts and remains closed during the laser wire filling welding process.
[0019] As an improvement, the laser-wire synchronization coordination means that the welding wire fed by the wire feeder can be completely melted by the laser. Feeding the wire too fast will result in the welding wire not being melted, and feeding the wire too slowly will result in a smaller filling thickness. Feeding the wire too slowly will result in a smaller filling thickness and unfused side walls. When the wire is fed too fast, the laser cannot completely melt the welding wire due to its energy output per unit time, resulting in unfused welding wire at the weld. In addition, due to the accumulation of welding wire, the welding wire deviates from the laser beam during the welding process, resulting in the welding wire not being melted and deviating and rushing out of the weld, causing welding failure.
[0020] The research found that under the conditions of P (laser welding power) = 3.6kW, V (welding speed) = 9mm / s, the wire feeding speed was changed for comparison. The research found that: when Vf (wire feeding speed) = 4.6m / min, the welding wire was fully melted and the weld filling degree was good; when Vf (wire feeding speed) = 6m / min, the welding wire was not melted and the weld was broken; when Vf (wire feeding speed) = 2m / min, the filling thickness was small and the side wall was not melted. The main reason for the non-melting was that the wire feeding amount was too small, and the welding wire was not enough to melt and flow to fill the weld at the same height.
[0021] As an improvement, increase the wire feed rate, reduce the welding speed, and adjust the laser output power. The wire feed rate depends on the direct formation of the weld and directly determines the metal accumulation morphology in the groove. In the study of the interaction of process parameters in ultra-narrow gap laser welding of high-strength steel by Wei Guo et al., it was found that the number of filling passes decreased with increasing wire feed speed and could decrease with decreasing welding speed. The increase in wire feed rate and the decrease in welding speed lead to an increase in the volume of filler material deposited per unit length, and therefore an increase in the average height of each filling channel. This means that a weld of a given thickness will be completed in fewer passes. Increasing the wire deposition rate will also result in a shortened joint completion time.
[0022] Laser output power is a key technical condition that affects narrow gap laser wire welding. It determines the role of welding heat input, affects the depth of a weld, the size of the molten pool, the filling amount, and the poor fusion through the side wall. Increasing the power of the laser improves defects such as poor side wall fusion. However, this process is not always a positive proportional function. When the power increases to a threshold, the rate of increase in the depth of weld and the size of the molten pool will become slow. It has been found that when P = 3.7kW, Vf (wire feed speed) = 4.7m / min, V (welding speed) = 8.5m / min, and the shielding gas pipe outputs 25% He + 75% CO2 (volume ratio), the increase in power makes the interlayer fusion better, the welding effect is optimal, the depth of penetration and the depth of width are the largest, the maximum penetration depth can reach 5.37mm, the width is 3.85mm, and the width of the single-sided heat-affected zone is 0.4mm.
[0023] The beneficial effects of the present invention are as follows: (1) In the conventional narrow gap laser welding with wire filling, the present invention acts on the weld bead through a slag cleaning brush and an air knife tube, wherein the slag cleaning brush directly acts on the weld bead and the side wall, so as to cause the weld slag attached to the weld bead and the side wall to peel off; in addition, since the peeled weld slag cannot be separated from the weld bead, a high-pressure airflow or a mixed solution is used to blow the weld slag away from the weld bead, and with the help of a pneumatic pressure system, according to the law and characteristics of laser welding plates, a high-pressure gas or a mixed solution is transported through a controllable pipeline system fixed on the laser to the weld bead to avoid the problem of interlayer unfusion during multi-layer welding, and solves the problem that it is difficult to clean slag after narrow gap laser welding with wire filling, and defects such as interlayer unfusion, pores, and side wall unfusion are easily generated during the next welding, thereby improving the welding quality of the interlayer and side wall. (2) The slag cleaning brush and the air knife tube can perform slag cleaning operations while performing narrow gap laser welding, and the post-weld slag cleaning after welding is combined into one step, which greatly improves the welding efficiency, can reduce the slag cleaning time of the welded plate, and improve the multi-layer welding efficiency, and the slag cleaning rate can reach more than 90%. (3) The present invention uses high-power laser to irradiate the filler wire to melt it and fuse it with the base material, thereby overcoming the shortcomings of traditional laser self-melting welding, such as small tolerance of workpiece assembly gap and thin welding plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic structural diagram of the narrow gap laser wire-filling welding equipment of the present invention;
[0025] In the figure: 1. Laser head; 2. Laser beam; 3. Protective air pipe; 4. Wire feeding mechanism; 5. Welding pool; 6. Rotary switch; 7. Slag cleaning brush; 8. Air valve switch; 9. Air knife tube; 10. Restraint buckle 1; 11. Base material; 12. Welding alloy; 13. Restraint buckle 2; 14. Back plate protective air pipe; 15. Fixed reinforcement plate. DETAILED DESCRIPTION
[0026] The present invention will be described in detail below with reference to the accompanying drawings.
[0027] like Figure 1As shown, the laser and the laser head 1 are connected by an optical fiber cable, and the optical fiber cable plays the role of transmitting the laser generated by the laser generator. The laser head 1 is fixed to the robot arm by bolts. The wire feeding mechanism 4 and the protective gas pipe 3 are respectively fixed on the extended fixed reinforcement plate 15, and the fixed reinforcement plate 15 is fixed on the laser head 1. The clamping tool is used as a support for the workpiece and as a separate workpiece. Constraint buckle 1, constraint buckle 2 and back plate protective gas pipe are independent of each other. Constraint buckle 1 fixes the slag brush 7 and the air knife tube 9 together, and the air knife tube 9 and the slag brush 7 are at an angle of 10°. Constraint buckle 2 mainly fixes the multi-tube gas channel together so that the 25% He+75% CO2 mixed gas in the gas pipe is transported in the same direction. The gas transported by the multi-tube gas channel can fully wrap the molten pool to achieve a better molten pool protection effect. The back plate protective gas pipe mainly transports Ar gas. This gas channel is opened separately, mainly considering the protection of the back weld formation during the first laser self-melting welding.
[0028] Before welding, the laser, wire feeding and gas feeding systems are debugged, and the protective gas pipe 3, wire feeding mechanism 4, slag brush 7 and air knife tube 9 are fixed on the laser head 1 through the reinforcing plate. After debugging, use acetone to clean the base material 11 of the workpiece to be welded. To ensure the alignment of the welded workpiece, the back of the workpiece is spot welded after manual assembly. The workpiece to be welded is supported by manual or hoisting methods. During the welding operation, the laser beam 2, protective gas pipe 3, wire feeding mechanism 4, rotary switch 6 and air valve switch 8 are turned on at the same time. The laser beam 2 is turned on to act on the welding molten pool 5 to the left for welding, and the light emitted by the laser beam 2 acts on the welding wire extending through the wire feeding mechanism 4 to form a weld alloy 12. The rotary switch 6 controls the rotation speed of the slag brush 7. While welding, the slag brush 7 rotates clockwise and removes slag as the laser head 1 moves to the left. The air valve switch 8 blows away the cleaned welding slag after the slag brush 7 acts.
[0029] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.
Claims
1. A narrow gap laser wire welding device, comprising a laser head (1), Features: It also includes a protective air pipe (3), a wire feeding mechanism (4), a slag cleaning brush (7) and an air knife pipe (9) which are respectively fixed on the laser head (1); The protective gas pipe (3) transports Ar, CO 2 A gas or a mixture of gases containing He; The protective air pipe (3) and / or the wire feeding mechanism (4) are provided with an angle adjuster; The slag cleaning brush is made of hard alloy and is driven by a motor to rotate for slag cleaning; The angle between the wire feeding mechanism (4) and the welding direction is acute, and welding is performed by using a front wire feeding method; The included angle between the wire feeding mechanism (4) and the laser beam (2) emitted by the laser head (1) is between 20 and 80 degrees; the included angle between the laser beam (2) and the protective air pipe (3) is between 20 and 80 degrees; The laser beam (2) forms an oblique angle with the workpiece surface, and the angle value is between 2 and 5 degrees; Also included is a back plate to protect the air pipe (14).
2. A narrow gap laser wire welding method, It is characterized in that The narrow gap laser wire welding device according to claim 1 comprises the following steps: Step (1): Assemble the workpiece to be welded, spot weld the back of the workpiece, and fix the workpiece to be welded; Step (2): the laser head (1) is moved to the starting point of the workpiece to be welded for alignment, so that the center of the light spot falls on the gap of the unwelded workpiece, and this spatial point is recorded to mark the end point of the welding; Step (3): The front end of the welding wire is delivered to the center of the light spot through the wire feeding mechanism (4), so that the light spot falls on the front end of the welding wire; during welding, the laser head (1), the protective air pipe (3), the wire feeding mechanism (4), the slag cleaning brush (7) and the air knife (9) are turned on simultaneously.
3. The narrow gap laser welding method according to claim 2, Features: In step (3), the mixed gas transported by the protective gas pipe (3) is He, CO 2 , the volume ratio is 1:3, the laser welding power is 3.7kW, the wire feeding speed is 4.7m / min, and the welding speed is 8.5m / min.