Alloy material for overhead conductor and preparation method thereof

By adjusting the alloy material formula and process flow, we can prepare alloy materials with high tensile strength, good elongation and low linear expansion coefficient, which solves the problems of performance stability and high cost of existing aluminum-clad nickel-molybdenum steel core materials and achieves High performance and low cost overhead conductor core material.

CN112962020BActive Publication Date: 2024-10-22GLOBAL ENERGY INTERCONNECTION RES INST CO LTD +3
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN201911275204.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-12
Publication Date
2024-10-22
Estimated Expiration
2039-12-12

AI Technical Summary

Technical Problem

The preparation process of existing aluminum-clad nickel-molybdenum steel core materials for overhead conductors requires high content and expensive nickel and cobalt alloy elements, which results in difficulty in controlling performance stability and high production costs, limiting its large-scale promotion and application.

Method used

Using new alloy material formulas, including C, Si, Mn, P, S, Ni, Mo, V, Co, Nb and other elements, it is prepared through smelting, electroslag refining, remelting, high-temperature calcination and drawing processes. An alloy material with high tensile strength, good elongation and low linear expansion coefficient.

Benefits of technology

The strength and toughness of alloy steel are improved, the tensile strength reaches ≥1400MPa, the elongation is ≥1.5%, and the linear expansion coefficient is ≤3.6×10-6/℃. It also simplifies the process and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides an alloy material for overhead wires, which comprises the following components by mass: C: 0.1-0.3wt%, Si: 0.05-0.2wt%, Mn: 0.05-0.3wt%, P≤0.01wt%, S≤0.01wt%, Ni: 32-36wt%, Mo: 0.1-1wt%, V: 0.1-3wt%, Co: 0.05-2wt%, Nb: 0.05-2wt%, and the balance is Fe and other inevitable impurities. The alloy material for overhead wires provided by the invention changes the raw material formula and proportion of alloy steel materials, refines the grains, improves the strength and toughness of alloy steel, tensile strength ≥1400MPa, elongation ≥1.5%, linear expansion coefficient ≤3.6×10 ‑6 / ℃ (20~200℃). The method for preparing the alloy material for overhead conductor provided by the present invention simplifies the process flow and saves the cost of the preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of core wire materials for conductors, and in particular to an alloy material for overhead conductors and a preparation method thereof. Background Art

[0002] Ordinary steel core materials used for overhead conductors have high thermal expansion coefficients and large sags, and cannot operate for a long time at high temperatures, resulting in the limitation of the allowable range of continuous working temperature of conventional steel core aluminum stranded wires. Invar material, which has the advantages of small thermal expansion coefficient, low thermal conductivity, and good toughness and plasticity, is an ideal core wire material for overhead conductors with low sag and high temperature resistance. The aluminum-clad Invar core heat-resistant aluminum alloy conductor, which is made of aluminum-clad Invar core and heat-resistant aluminum alloy wire, has low sag and high heat resistance. It can operate at high temperatures for a long time and has the characteristics of "same diameter, same arc, double capacity", which is one of the effective ways to increase transmission capacity.

[0003] Traditional Invar (Invar alloy) materials have low strength, and their performance is generally improved by adding alloying elements. At present, the Invar core used for overhead conductors is mainly Fe-Ni-Mo series Invar material, so it is also called nickel-molybdenum alloy steel. In recent years, with the development of aluminum-clad nickel-molybdenum steel core technology, aluminum-clad nickel-molybdenum steel core heat-resistant aluminum alloy conductor products have received more and more attention and application. However, the nickel-molybdenum alloy steel used for aluminum-clad nickel-molybdenum steel core currently produced and used at home and abroad requires the addition of high-content and expensive nickel and cobalt alloy elements to improve performance during the preparation process. At the same time, the preparation process is relatively complicated, resulting in the performance stability of nickel-molybdenum alloy steel wire rods and their core wire products being difficult to control well, and the production and manufacturing costs are relatively high, which to a certain extent restricts their large-scale promotion and application.

[0004] Although Chinese Patent No. 201610851813.0 entitled "Fe-Ni Invar Alloy Welding Wire and Manufacturing Method Thereof" ensures a lower expansion coefficient, the tensile strength of the alloy produced is relatively low.

[0005] Therefore, it is necessary to provide a high-performance, low-cost alloy steel material and its core wire products to meet the needs of transmission line capacity expansion and transformation and the development of large-capacity transmission technology. Summary of the invention

[0006] The object of the present invention is to provide an alloy material for overhead conductors having high tensile strength, good elongation and low linear expansion coefficient.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] An alloy material for overhead conductors, comprising the following components by mass:

[0009] C: 0.1~0.3wt%, Si: 0.05~0.2wt%, Mn: 0.05~0.3wt%, P≤0.01wt%, S≤0.01wt%, Ni: 32~36wt%, Mo: 0.1~1wt%, V: 0.1~3wt%, Co: 0.05~2wt%, Nb: 0.05~2wt%, and the balance is Fe and other inevitable impurities.

[0010] Preferably, the alloy material includes the following components in parts by mass: C: 0.15-0.3wt%, Si: 0.1-0.2wt%, Mn: 0.1-0.3wt%, P≤0.01wt%, S≤0.01wt%, Ni: 33-35wt%, Mo: 0.1-0.5wt%, V: 0.5-3wt%, Co: 0.1-2wt%, Nb: 0.1-2wt%, and the balance is Fe and other inevitable impurities.

[0011] Preferably, the alloy material includes the following components in percentage by mass: C: 0.2wt%, Si: 0.12wt%, Mn: 0.25wt%, P: 0.005wt%, S: 0.005wt%, Ni: 35.0wt%, Mo: 0.5wt%, V: 1.5wt%, Co: 1.0wt%, Nb: 0.8wt%, the balance is Fe, and the rest are inevitable trace impurities.

[0012] A method for preparing an alloy material as described in any one of the above items, the method comprising the following steps:

[0013] (1) Smelting raw materials;

[0014] (2) Electroslag refining and remelting;

[0015] (3) High temperature calcination and hot rolling into φ8mm round disc;

[0016] (4) Drawing process.

[0017] Preferably, the step (1) comprises vacuum melting and smelting the raw material after drying treatment and the nickel material after dehydrogenation annealing.

[0018] Preferably, the electroslag refining in step (2) includes refining at 1400° C. to 1600° C. for 0.5 to 1.5 h.

[0019] Preferably, the electroslag remelting in step (2) includes furnace charging, arc striking and slag forming, smelting, shrinkage feeding, cooling treatment and forming steel billets.

[0020] Preferably, in the step (3), the initial forging temperature of the high-temperature calcination is 1100-1250°C, and the final forging temperature is 900-1100°C.

[0021] Preferably, in step (3), the temperature is kept at 1100-1200° C. for 0.5-2 h before calcination.

[0022] Preferably, the step (3) comprises: keeping the temperature at 1050-1150°C for 0.5-2h and then hot rolling, with the initial rolling temperature being 1050-1150°C and the final rolling temperature being 900-1000°C.

[0023] Preferably, the drawing process in step (4) comprises the following steps:

[0024] (1) After solution treatment at 1000-1100°C, cold drawing is performed to φ6.0 mm;

[0025] (2) After heat treatment at 500-650℃ for 2-5h, the steel is cold drawn to φ3.5mm.

[0026] Compared with the closest prior art, the technical solution provided by the present invention has the following beneficial effects:

[0027] The alloy material for overhead conductors provided by the present invention changes the raw material formula and proportion of alloy steel materials, refines the crystal grains, and improves the strength and toughness of the alloy steel.

[0028] The alloy material for overhead wires provided by the present invention has a tensile strength of ≥1400MPa, an elongation of ≥1.5%, and a linear expansion coefficient of ≤3.6×10 -6 / ℃(20~200℃).

[0029] The method for preparing the alloy material for overhead conductors provided by the present invention simplifies the process flow and saves the cost of the preparation process. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is clearly and completely described below in the form of specific embodiments.

[0031] Example 1

[0032] An alloy steel core wire material for an overhead conductor comprises the following components by weight: C: 0.25wt%, Si: 0.1wt%, Mn: 0.28wt%, P: 0.008wt%, S: 0.01wt%, Ni: 33.0wt%, Mo: 0.4wt%, V: 2wt%, Co: 1.5wt%, Nb: 0.5wt%, the balance is Fe, and the rest are inevitable trace impurities.

[0033] The preparation and processing technology of the above alloy steel comprises the following steps:

[0034] (1) Raw material preparation: dehydrogenation annealing of nickel plate and drying of all raw materials;

[0035] (2) Vacuum smelting: After the iron is melted, other alloying elements are added and all of them are melted;

[0036] (3) Electroslag refining: Refining at 1450℃ for 0.5h and casting into electroslag ingots;

[0037] (3) Electroslag remelting: Electroslag remelting is carried out to obtain steel ingots through furnace loading, arc slag making, smelting, shrinkage feeding, and cooling;

[0038] (4) High temperature forging: forging after keeping at 1150℃ for 2h, initial forging temperature 1100℃, final forging temperature 900℃;

[0039] (5) Hot rolling: keep the temperature at 1100℃ for 2h, and hot roll the square billet into φ8mm round disc, with the initial rolling temperature of 1050℃ and the final rolling temperature of 900℃;

[0040] (6) Drawing treatment: After the coil is peeled, it is solution treated at 1000℃ under argon protection, and then cold drawn to φ6.0mm through 6 passes; it is heat treated at 550℃ for 5h under argon protection to keep it bright, and then cold drawn to φ3.5mm.

[0041] Example 2

[0042] An alloy steel core wire material for an overhead conductor comprises the following components by weight: C: 0.2wt%, Si: 0.12wt%, Mn: 0.25wt%, P: 0.01wt%, S: 0.005wt%, Ni: 34.0wt%, Mo: 0.4wt%, V: 1.5wt%, Co: 0.8wt%, Nb: 1.0wt%, the balance is Fe, and the rest are inevitable trace impurities.

[0043] The preparation and processing technology of the above alloy steel comprises the following steps:

[0044] (1) Raw material preparation: dehydrogenation annealing of nickel plate and drying of all raw materials;

[0045] (2) Vacuum smelting: After the iron is melted, other alloying elements are added and all of them are melted;

[0046] (3) Electroslag refining: Refining at 1450℃ for 1h and casting into electroslag ingots;

[0047] (3) Electroslag remelting: Electroslag remelting is carried out to obtain steel ingots through furnace loading, arc slag making, smelting, shrinkage feeding, and cooling;

[0048] (4) High temperature forging: forging after keeping at 1170℃ for 2h, initial forging temperature 1100℃, final forging temperature 900℃;

[0049] (5) Hot rolling: keep the temperature at 1100℃ for 2h, and hot roll the square billet into φ8mm round disc, with the initial rolling temperature of 1070℃ and the final rolling temperature of 900℃;

[0050] (6) Drawing treatment: After the coil is peeled, it is solution treated at 1000℃ under argon protection, and then cold drawn to φ6.0mm through 6 passes; it is heat treated at 580℃ for 5h under argon protection to keep it bright, and then cold drawn to φ3.5mm.

[0051] Example 3

[0052] An alloy steel core wire material for an overhead conductor comprises the following components by weight: C: 0.2wt%, Si: 0.12wt%, Mn: 0.25wt%, P: 0.005wt%, S: 0.005wt%, Ni: 35.0wt%, Mo: 0.5wt%, V: 1.5wt%, Co: 1.0wt%, Nb: 0.8wt%, the balance is Fe, and the rest are inevitable trace impurities.

[0053] The preparation and processing technology of the above alloy steel comprises the following steps:

[0054] (1) Raw material preparation: dehydrogenation annealing of nickel plate and drying of all raw materials;

[0055] (2) Vacuum smelting: After the iron is melted, other alloying elements are added and all of them are melted;

[0056] (3) Electroslag refining: Refining at 1470℃ for 1h and casting into electroslag ingots;

[0057] (3) Electroslag remelting: Electroslag remelting is carried out to obtain steel ingots through furnace loading, arc slag making, smelting, shrinkage feeding, and cooling;

[0058] (4) High temperature forging: forging after keeping at 1170℃ for 2h, initial forging temperature 1100℃, final forging temperature 900℃;

[0059] (5) Hot rolling: keep the temperature at 1100℃ for 2h, and hot roll the square billet into φ8mm round disc, with the initial rolling temperature of 1060℃ and the final rolling temperature of 900℃;

[0060] (6) Drawing treatment: After the coil is peeled, it is solution treated at 1000℃ under argon protection, and then cold drawn to φ6.0mm through 6 passes; it is heat treated at 580℃ for 5h under argon protection to keep it bright, and then cold drawn to φ3.5mm.

[0061] Example 4

[0062] An alloy steel core wire material for an overhead conductor comprises the following components by weight: C: 0.2wt%, Si: 0.1wt%, Mn: 0.26wt%, P: 0.005wt%, S: 0.01wt%, Ni: 35.0wt%, Mo: 0.5wt%, V: 1wt%, Co: 1.0wt%, Nb: 0.8wt%, the balance is Fe, and the rest are inevitable trace impurities.

[0063] The preparation and processing technology of the above alloy steel comprises the following steps:

[0064] (1) Raw material preparation: dehydrogenation annealing of nickel plate and drying of all raw materials;

[0065] (2) Vacuum smelting: After the iron is melted, other alloying elements are added and all of them are melted;

[0066] (3) Electroslag refining: Refining at 1470℃ for 0.5h and casting into electroslag ingots;

[0067] (3) Electroslag remelting: Electroslag remelting is carried out to obtain steel ingots through furnace loading, arc slag making, smelting, shrinkage feeding, and cooling;

[0068] (4) High temperature forging: forging after keeping at 1170℃ for 2h, initial forging temperature 1100℃, final forging temperature 900℃;

[0069] (5) Hot rolling: keep the temperature at 1100℃ for 2h, and hot roll the square billet into φ8mm round disc, with the initial rolling temperature of 1050℃ and the final rolling temperature of 900℃;

[0070] (6) Drawing treatment: After the coil is peeled, it is solution treated at 1000℃ under argon protection, and then cold drawn to φ6.0mm through 6 passes; it is heat treated at 600℃ for 4h under argon protection to keep it bright, and then cold drawn to φ3.5mm.

[0071] Example 5

[0072] An alloy steel core wire material for an overhead conductor comprises the following components by weight: C: 0.25wt%, Si: 0.1wt%, Mn: 0.2wt%, P: 0.005wt%, S: 0.01wt%, Ni: 34wt%, Mo: 0.5wt%, V: 1.5wt%, Co: 1.0wt%, Nb: 0.6wt%, the balance is Fe, and the rest are inevitable trace impurities.

[0073] The preparation and processing technology of the above alloy steel comprises the following steps:

[0074] (1) Raw material preparation: dehydrogenation annealing of nickel plate and drying of all raw materials;

[0075] (2) Vacuum smelting: After the iron is melted, other alloying elements are added and all of them are melted;

[0076] (3) Electroslag refining: Refining at 1450℃ for 1h and casting into electroslag ingots;

[0077] (3) Electroslag remelting: Electroslag remelting is carried out to obtain steel ingots through furnace loading, arc slag making, smelting, shrinkage feeding, and cooling;

[0078] (4) High temperature forging: forging after keeping at 1150℃ for 2h, initial forging temperature 1100℃, final forging temperature 900℃;

[0079] (5) Hot rolling: keep the temperature at 1120℃ for 2h, and hot roll the square billet into φ8mm round disc, with the initial rolling temperature of 1050℃ and the final rolling temperature of 900℃;

[0080] (6) Drawing treatment: After the coil is peeled, it is solution treated at 1000℃ under argon protection, and then cold drawn to φ6.0mm through 6 passes; it is heat treated at 580℃ for 4h under argon protection to keep it bright, and then cold drawn to φ3.5mm.

[0081] The performance of the alloy materials prepared in each embodiment was tested, and the test results are shown in Table 1 below.

[0082] Table 1: Performance test results

[0083] Tensile strength / MPa Elongation / % <![CDATA[Coefficient of expansion / °C -1 (20 to 200 °C)]]> Example 1 1420 1.66 <![CDATA[3.58×10 -6 ]]> Example 2 1460 1.62 <![CDATA[3.52×10 -6 ]]> Example 3 1520 1.52 <![CDATA[3.48×10 -6 ]]> Example 4 1480 1.58 <![CDATA[3.50×10 -6 ]]> Example 5 1470 1.63 <![CDATA[3.53×10 -6 ]]>

[0084] As can be seen from the above table, the alloy material for overhead wire provided by the present invention has excellent properties, tensile strength ≥ 1400MPa, elongation ≥ 1.5%, (20-200℃) expansion coefficient ≤ 3.6×10 -6 / ℃.

[0085] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Those skilled in the art should understand that the specific implementation modes of the present invention may be modified or replaced by equivalents with reference to the above embodiments. Any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention are within the scope of protection of the pending claims.

Claims

1. An alloy material for overhead conductors, characterized in that: The alloy material includes the following components in percentage by mass: C: 0.2wt%, Si: 0.12wt%, Mn: 0.25wt%, P: 0.005wt%, S: 0.005wt%, Ni: 35.0wt%, Mo: 0.5wt%, V: 1.5wt%, Co: 1.0wt%, Nb: 0.8wt%, the balance is Fe, and the rest are inevitable trace impurities.

2. The method for preparing the alloy material according to claim 1, characterized in that: The method comprises the following steps: (1) Smelting raw materials; (2) Electroslag refining and remelting; (3) High temperature calcination and hot rolling into φ8mm round disc; (4) Drawing treatment.

3. The preparation method according to claim 2, characterized in that: The step (1) comprises vacuum melting and smelting the raw material after drying treatment and the nickel material after dehydrogenation annealing.

4. The preparation method according to claim 2, characterized in that: The electroslag refining in step (2) includes refining at 1400° C. to 1600° C. for 0.5 to 1.5 hours.

5. The preparation method according to claim 2, characterized in that: The electroslag remelting in step (2) includes furnace charging, arc striking and slag making, smelting, shrinkage feeding, cooling treatment and forming steel billets.

6. The preparation method according to claim 2, characterized in that: In the step (3), the initial forging temperature of the high temperature calcination is 1100-1250°C, and the final forging temperature is 900-1100°C.

7. The preparation method according to claim 2, characterized in that: In the step (3), the temperature is kept at 1100-1200° C. for 0.5-2 h before calcination.

8. The preparation method according to claim 2, characterized in that: The step (3) comprises: keeping the temperature at 1050-1150°C for 0.5-2h and then hot rolling, wherein the initial rolling temperature during hot rolling is 1050-1150°C and the final rolling temperature is 900-1000°C.

9. The preparation method according to claim 2, characterized in that: The drawing process in step (4) comprises the following steps: (1) After solution treatment at 1000~1100℃, cold drawing to φ6.0mm; (2) After heat treatment at 500~650℃ for 2~5h, cold draw to φ3.5mm.

Citation Information

Cited By

  • Nanophase carbon-nitrogen composite particle reinforced invar alloy wire and preparation method thereof

    CN114086086A

  • High-strength iron-nickel-molybdenum alloy wire and low-cost preparation method thereof

    CN114107834A

  • Production method of invar steel wire with high surface quality

    CN114130849A