Etching method of inclined through hole
Through the etching method of cyclically adjusting the chamber pressure and excitation power, the problem of small inclination angle of the back through hole wall of the third-generation semiconductor material is solved, forming through holes with a large inclination angle, simplifying the metal filling process.
Patent Information
- Application Number
- CN202110399927.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-04-14
AI Technical Summary
In the existing semiconductor manufacturing process, the thermal conductivity of the third-generation semiconductor material is poor, resulting in a small inclination angle of the hole wall when the back through hole is installed on the film layer, which increases the difficulty of subsequent metal filling.
The etching method performed cyclically is adopted to gradually increase the chamber pressure and reduce the excitation power by depositing the protective layer, bombardment and etching steps, and control the etching force and quantity of the plasma to form a through hole with a specified inclination angle.
It is realized that through holes with a large inclination angle on wide bandgap semiconductor materials are formed, which simplifies the subsequent metal filling process and meets different process needs.
Smart Images

Figure CN113140455B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor manufacturing, and in particular to an etching method for an inclined through hole. Background Art
[0002] At present, the third-generation semiconductor materials are widely used in the field of semiconductor manufacturing because of their advantages such as large bandgap width, large breakdown electric field strength and large saturated electron drift velocity. However, due to the poor thermal conductivity of some third-generation semiconductor materials (for example, gallium nitride materials), when using third-generation semiconductor materials with poor thermal conductivity to make transistors, it is necessary to set back vias on the film layer of the transistor to assist in heat dissipation, wherein the back vias are surface holes opened on the surface of the film layer and connected to the source and drain. The back vias are usually filled with a metal layer, which can be grounded as a lead to achieve overall grounding of the transistor.
[0003] The existing back via etching process generally directly adopts physical etching or chemical etching, or a process of alternating physical etching and chemical etching. However, this etching method will form a straight hole or a hole with a very small hole wall inclination angle. The small hole wall inclination angle or no inclination will increase the difficulty of filling metal in the back via in the subsequent process. Summary of the invention
[0004] The embodiment of the present invention aims to solve at least one of the technical problems existing in the prior art, and proposes an etching method for an inclined through hole, which can form a through hole with a hole wall with a specified inclination angle on a wide bandgap semiconductor material, thereby meeting different process requirements.
[0005] In order to achieve the purpose of the present invention, a method for etching an inclined through hole is provided, which is used to etch an inclined through hole on a film layer made of a wide bandgap semiconductor material. The etching method comprises the following steps which are performed cyclically:
[0006] S1, depositing a protective layer on the hole wall of the through hole;
[0007] S2, bombarding the protective layer located on the bottom surface of the through hole until the bottom surface of the through hole is exposed;
[0008] S3, etching the bottom surface of the through hole to a preset depth;
[0009] S4, determine whether the current number of cycles reaches the preset total number of cycles, if not, add 1 to the current number of cycles, and proceed to step S5; if yes, the process ends;
[0010] S5, increasing the chamber pressure value by a preset first unit adjustment amount, and reducing the excitation power value by a preset second unit adjustment amount, and returning to step S1.
[0011] Optionally, the first unit adjustment amount satisfies the following formula:
[0012] P1=(P final -P initial ) / n total
[0013] Wherein, P1 represents the first unit adjustment amount, P initial Indicates the preset initial chamber pressure value, P final Indicates the preset terminal chamber pressure value, n total Indicates the preset total number of cycles.
[0014] Optionally, the second unit adjustment amount satisfies the following formula:
[0015] p2=(p initial -p final ) / n total
[0016] Wherein, p2 represents the adjustment amount of the second unit, p initial Indicates the preset initial excitation power value, p final Indicates the preset final excitation power value, n total Indicates the preset total number of cycles.
[0017] Optionally, the step S1 includes:
[0018] S11, introducing deposition gas into the process chamber;
[0019] S12, turning on an excitation power supply to output a first excitation power value to the process chamber to excite the deposition gas to form a plasma of a material capable of forming the protective layer, so as to deposit the protective layer.
[0020] Optionally, the deposition gas is a gas containing fluorine and carbon elements.
[0021] Optionally, step S2 includes:
[0022] S21, introducing bombardment gas into the process chamber;
[0023] S22, turning on the excitation power supply to output a second excitation power value to the process chamber to excite the bombardment gas to form a bombardment plasma;
[0024] S23, turning on the bias power supply, outputting a first bias power value to the lower electrode, so that the bombardment plasma physically bombards the protective layer located on the bottom surface of the through hole to etch the protective layer on the bottom surface of the through hole.
[0025] Optionally, step S3 includes:
[0026] S31, introducing etching gas into the process chamber;
[0027] S32, turning on the excitation power supply to output a third excitation power value to the process chamber to excite the etching gas to form an etching plasma;
[0028] S33, turning on the bias power supply, outputting a second bias power value to the lower electrode, so that the etching plasma chemically etches the bottom surface of the through hole.
[0029] Optionally, the wide bandgap semiconductor material includes silicon carbide or gallium nitride.
[0030] Optionally, the chamber pressure value ranges from 5 mTorr to 500 mTorr.
[0031] Optionally, the excitation power value ranges from 500W to 3000W.
[0032] The embodiments of the present invention have the following beneficial effects:
[0033] The etching method of the inclined through hole provided by the embodiment of the present invention is to perform the deposition step, the bombardment step and the etching step on the surface of the through hole in a cycle, and to increase the chamber pressure and reduce the excitation power after each cycle. Since the greater the chamber pressure, the shorter the mean free path of the plasma, the etching force of the plasma on the through hole gradually weakens as the number of cycles increases, so that the etching amount of the etching step can be gradually reduced as the number of cycles increases; at the same time, since the smaller the excitation power value, the smaller the ionization rate of the process gas, the number of plasmas used for etching gradually decreases as the number of cycles increases, so that the etching amount of the etching step can also be reduced as the number of cycles increases, and finally the hole wall of the through hole can be tilted at a specified angle, so as to meet different process requirements. For example, when the etching method provided by the present invention is applied to etching holes on wide bandgap semiconductor materials, a hole with a large inclination can be obtained to facilitate metal filling. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 A flow chart of an etching method for an inclined through hole provided in Embodiment 1 of the present invention;
[0035] Figure 2 A flow chart of an etching method applied to a silicon carbide film layer provided in Example 2 of the present invention;
[0036] Figure 3 A morphology image of a through hole wall obtained by using the etching method provided in Example 2 of the present invention;
[0037] Figure 4 This is a flow chart of an etching method applied to a gallium nitride film layer provided in Example 3 of the present invention. DETAILED DESCRIPTION
[0038] The present invention is described in detail below, and examples of embodiments of the present invention are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar components or components with the same or similar functions. In addition, if the detailed description of the known technology is unnecessary for the features of the present invention shown, it will be omitted. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention.
[0039] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical terms and scientific terms) used in the present embodiment have the same meaning as the general understanding of those skilled in the art in the field to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as the meaning in the context of the prior art, and unless specifically defined as here, will not be interpreted with an idealized or overly formal meaning.
[0040] In order to enable those skilled in the art to better understand the technical solution of the present invention, the etching method of the inclined through hole provided by the embodiment of the present invention is described in detail below with reference to the accompanying drawings.
[0041] Example 1
[0042] This embodiment provides an etching method for an inclined through hole, which is used to etch a through hole with an inclined hole wall on a film layer made of a wide bandgap semiconductor material, wherein the wide bandgap semiconductor material includes silicon carbide or gallium nitride, which are representatives of third-generation semiconductor materials. However, this embodiment is not limited thereto, and the above etching method can also be used to etch holes on the surface of a film layer made of a third-generation semiconductor material such as zinc oxide or diamond.
[0043] The above-mentioned wide bandgap semiconductor materials generally have the characteristics of high hardness, high brittleness and high melting point. Such characteristics make it difficult to process holes with inclined angles in the wide bandgap semiconductor material film layer. The current etching method can only form a straight hole or a hole with a very small inclination angle of the hole wall. The small inclination angle of the hole wall or no inclination will increase the difficulty of filling metal in the back through hole in the subsequent process.
[0044] In order to solve the above problems, Figure 1 As shown, the etching method of the inclined through hole provided in this embodiment includes the following steps which are performed cyclically:
[0045] S1, depositing a protective layer on the hole wall of the through hole;
[0046] It should be noted that when step S1 is performed for the first time, the protective layer is only formed on the unprocessed flat surface of the film layer.
[0047] Specifically, the protective layer is used to protect the hole wall surface of the through hole from being etched in the subsequent bombardment step and etching step.
[0048] S2, bombarding the protective layer on the bottom surface of the through hole until the bottom surface of the through hole is exposed;
[0049] S3, etching the bottom surface of the through hole to a preset depth;
[0050] Specifically, this step can adopt an isotropic etching method to perform etching in the longitudinal and transverse directions simultaneously. Since the bottom surface of the through hole is exposed due to the removal of the protective layer in the above step S2, and the side of the through hole is still protected by the protective layer, the etching amount can be increased only in the longitudinal direction, that is, the etching depth of the through hole is increased.
[0051] Specifically, a mask plate can be covered on the surface of the film layer to be processed, and the portion of the film layer surface where the orifice is to be formed is exposed in the process chamber, so that plasma bombards or etches the portion of the film layer surface where the orifice is to be formed, thereby defining the position and orifice size of the through hole.
[0052] S4, determine whether the current number of cycles reaches the preset total number of cycles, if not, add 1 to the current number of cycles, and proceed to step S5; if yes, the process ends;
[0053] Specifically, the preset total number of cycles can be set according to the total target depth of the through hole.
[0054] S5, increasing the chamber pressure value by a preset first unit adjustment amount, and increasing the excitation power value by a preset second unit adjustment amount, and returning to step S1.
[0055] Since the mean free path of plasma decreases with increasing chamber pressure, as the current chamber pressure gradually increases, the kinetic energy of plasma in the etching step can be gradually reduced, so that the etching amount can be gradually reduced as the number of cycles increases; at the same time, since the ionization rate of the process gas decreases as the excitation power value decreases, as the current excitation power value gradually decreases, the amount of plasma used for etching can be gradually reduced, and the etching amount can also be gradually reduced as the number of cycles increases; therefore, gradually increasing the aforementioned current chamber pressure value and reducing the current excitation power value can gradually reduce the etching amount in each cycle, and ultimately the hole wall of the through hole can be tilted at a specified angle, thereby meeting different process requirements.
[0056] In some embodiments, the above etching method can be applied to the through-hole etching process of the third-generation wide bandgap semiconductor material. For example, in the process of manufacturing a thin film transistor, it is necessary to form a back through hole in all film layers containing the third-generation wide bandgap semiconductor material film layer on one side of the source and drain layers, so that the source and drain layers can be exposed through the back through hole and connected to the outside. The etching method provided in the embodiment of the present invention can be applied to etching the above-mentioned back through hole to increase its inclination, so as to facilitate filling of metal in the subsequent process.
[0057] The first unit adjustment amount is a single adjustment amount of the chamber pressure each time step S5 is performed. The adjustment amount can be set in a variety of ways. For example, in some embodiments, the first unit adjustment amount satisfies the following formula:
[0058] P1=(P final -P initial ) / n total
[0059] Among them, P1 represents the adjustment amount of the first unit, P initial Indicates the preset initial chamber pressure value, P final Indicates the preset terminal chamber pressure value, n total Indicates the total number of preset cycles.
[0060] In some embodiments, the current chamber pressure value P may be reset to: P = P before the next step S1 begins. initial +(P final -P initial )×n / n total
[0061] Where n is the current cycle number.
[0062] In some embodiments, the range of the chamber pressure value is 5mTorr to 500mTorr, and the initial value and the final value of the chamber pressure value need to be set according to the process requirements to ensure that the kinetic energy of the plasma in the aforementioned steps S2 and S3 is not too large, so as to avoid the single etching amount being too large and causing the depth of the through hole to be difficult to control; at the same time, it can ensure that the kinetic energy of the plasma in the aforementioned steps S2 and S3 is not too small, so as to avoid the single etching amount being too small so that the protective layer cannot be bombarded or cause waste of process steps.
[0063] Specifically, the aforementioned multiple parameters can be preset before the cycle starts, wherein the preset initial chamber pressure value P initial Less than the preset terminal chamber pressure value P final, the difference in chamber pressure at the beginning and the end is divided into n parts, so that the first unit adjustment amount in each cycle is equal, so that the chamber pressure can be uniformly increased in each cycle, so that the etching amount can be uniformly reduced, so that the inclined hole wall surface morphology can be relatively flat. However, this embodiment is not limited to this, and in actual production, the first unit adjustment amount can be adjusted according to production requirements.
[0064] The second unit adjustment amount refers to a single adjustment amount of the excitation power each time step S5 is performed. The size of the adjustment amount can be set in a variety of ways. For example, in some embodiments, the second unit adjustment amount satisfies the following formula:
[0065] p2=(p initial -p final ) / n total
[0066] Among them, p2 represents the adjustment amount of the second unit, p initial Indicates the preset initial excitation power value, p final Indicates the preset final excitation power value, n total In some embodiments, the current excitation power value p can be reset to p=p before the next step S1 starts. initial +(p final -p initial )×n / n total , where n is the current loop number.
[0067] In some embodiments, the range of the excitation power value is 500W to 3000W. Similarly, the initial value and the final value of the excitation power value also need to be set according to the process requirements to ensure that the amount of plasma in the aforementioned steps S2 and S3 is not too small, so as to avoid a single etching amount that is too small so that the protective layer cannot be bombarded open or cause a waste of process steps; at the same time, it can ensure that the amount of plasma in the aforementioned steps S2 and S3 is not too much, so as to avoid a single etching amount that is too large and the depth of the through hole is difficult to control.
[0068] Specifically, the aforementioned multiple parameters can be pre-set before the cycle starts, wherein the preset initial excitation power value p initial must be greater than the preset final excitation power value p final, the difference between the initial and final excitation powers is divided into n parts, so that the second unit adjustment amount in each cycle is equal; since the smaller the excitation power, the smaller the ionization rate of the process gas, reducing the excitation power can reduce the amount of plasma used for etching, which helps to form an inclined hole wall. Therefore, in each cycle, the excitation power value is reduced by a certain value, so that the etching amount can be evenly reduced, so that the surface morphology of the inclined hole wall can be smoother. However, this embodiment is not limited to this. In actual production, the second unit adjustment amount can be adjusted according to production requirements.
[0069] In some embodiments, the aforementioned step S1 includes:
[0070] S11, introducing deposition gas into the process chamber;
[0071] Specifically, the type of deposition gas should be selected according to the type of film material. For example, octafluorocyclobutane gas can be used as the deposition gas for silicon carbide material. Specifically, the flow rate of octafluorocyclobutane gas can be in the range of 10 sccm to 1000 sccm.
[0072] S12, turning on an excitation power supply to output a first excitation power value to the process chamber to excite the deposition gas to form a plasma of a material capable of forming a protective layer.
[0073] In some embodiments, the deposition gas is a gas containing fluorine and carbon. Specifically, octafluorocyclobutane gas can be used, which generates plasma containing fluorine ions and carbon ions after ionization, and under high temperature and high pressure catalysis, the fluorine ions and carbon ions react to produce fluorocarbon polymers; due to the stable properties of fluorocarbon polymers, the fluorocarbon polymers deposited on the hole walls of the through holes can well protect the hole wall surface of the hole to be etched.
[0074] In some embodiments, the aforementioned step S2 includes:
[0075] S21, introducing bombardment gas into the process chamber;
[0076] Specifically, the type of bombardment gas should be selected according to the type of film material. For example, sulfur hexafluoride gas can be used as the bombardment gas for silicon carbide material. Specifically, the flow rate of sulfur hexafluoride gas can range from 10 sccm to 1000 sccm.
[0077] S22, turning on the excitation power supply to output a second excitation power value to the process chamber to excite the bombardment gas to form a bombardment plasma;
[0078] S23, turn on the bias power supply, and output the first bias power value to the lower electrode, so that the bombarding plasma can physically bombard the protective layer on the bottom surface of the through hole. Specifically, the lower electrode to which the first bias power is applied can exert an attraction perpendicular to the surface of the lower electrode on the plasma to attract the plasma to rush toward the film layer; and the first bias power value is relatively high, so the attraction exerted on the plasma is relatively high. At this time, other forces except the attraction on the plasma can be ignored, so that the plasma can rush vertically toward the film layer to bombard the protective layer on the bottom surface of the through hole. In other words, the bombardment process in step S23 can be understood as an anisotropic etching process with a relatively large etching force.
[0079] Step S23 is used to remove the protective layer on the bottom surface of the through hole, exposing the film layer at the bottom of the through hole to prepare for the subsequent etching step.
[0080] In some embodiments, the aforementioned step S3 includes:
[0081] S31, introducing etching gas into the process chamber;
[0082] Specifically, the type of etching gas should be selected according to the type of film material. For example, for silicon carbide material, a mixed gas of sulfur hexafluoride and oxygen can be used as the etching gas. Specifically, the flow rate value of the mixed gas can range from 10 sccm to 1000 sccm.
[0083] S32, turning on the excitation power supply to output a third excitation power value to the process chamber to excite the etching gas to form an etching plasma;
[0084] S33, turn on the bias power supply, and output a second bias power value to the lower electrode, which can attract the etching plasma to move toward the surface of the film layer, so that the etching plasma chemically etches the bottom surface of the through hole. Specifically, the second bias power value applied to the lower electrode is low, so the attraction it exerts on the plasma is small. At this time, the movement direction of the plasma is not only limited by the attraction, so that it can rush to the film layer at a variety of incident angles, so as to etch the surface of the film layer from a variety of angles to the surface of the film layer. In other words, the chemical etching process in step S33 can be understood as an isotropic etching process.
[0085] It should be noted that the purpose of the chemical etching process in the aforementioned step S33 is to expand the hole at the bottom surface of the through hole in the longitudinal and transverse directions. However, in the actual chemical etching process, there is also a certain amount of etching on the through hole wall. However, in step S12, a protective layer that is not easily chemically etched is deposited on the through hole wall, so the aforementioned etching amount is extremely small and will not affect the shape of the through hole, so it is ignored here.
[0086] Example 2
[0087] Based on Example 1, this embodiment provides an etching method for an inclined through hole applied to a silicon carbide film layer, which specifically includes:
[0088] S41, preset the initial chamber pressure value P initial , preset terminal chamber pressure value P final , preset initial excitation power value p initial , preset final excitation power value p final , preset total number of cycles n total Make settings;
[0089] S42, introducing octafluorocyclobutane gas into the process chamber, and turning on an excitation power supply to excite the octafluorocyclobutane gas to form plasma, wherein the plasma contains carbon ions and fluorine ions, which can undergo polymerization reaction under the catalysis of high temperature and high pressure to generate fluorocarbon polymers, so that the fluorocarbon polymers are deposited on the surface of the film layer to form a protective layer;
[0090] Specifically, when performing the above step S42, the octafluorocyclobutane gas is simultaneously introduced from the central gas inlet and the edge gas inlet at the top of the process chamber, wherein the octafluorocyclobutane gas flow rate at the central gas inlet at the top of the process chamber is the central flow rate of the octafluorocyclobutane gas, and the octafluorocyclobutane gas flow rate at the central gas inlet at the top of the process chamber is the edge flow rate of the octafluorocyclobutane gas; specifically, the central flow rate value of the octafluorocyclobutane gas may range from 10 sccm to 1000 sccm, preferably 350 sccm; the edge flow rate of the octafluorocyclobutane gas may range from 10 sccm to 1000 sccm, preferably 150 sccm;
[0091] When performing the above-mentioned step S42, the excitation power supply applies excitation power to the central area and edge area of the upper electrode respectively, wherein the excitation power applied to the central area of the upper electrode is the central power, and the excitation power applied to the edge area of the upper electrode is the edge power; specifically, the central power applied by the excitation power supply to the process chamber is in the range of 500W to 5000W, preferably 2000W; the edge power applied to the process chamber is in the range of 500W to 3000W, preferably 1000W.
[0092] Because in the plasma reaction, the polymer produced by the reaction of carbon ions and fluorine ions is often more likely to form at the edge of the surface to be processed, resulting in excessive deposition of protective film material on the side walls of the through hole and too little deposition of protective film material on the bottom surface of the through hole. Therefore, in order to make the protective layer evenly formed on the surface of the film layer, the preferred value of the aforementioned gas flow rate is that the center flow value is greater than the edge flow value, and the preferred value of the power value applied by the aforementioned excitation power supply to the upper electrode is also that the center power value is greater than the edge power value, so as to reduce the amount of plasma in the edge area of the film layer, thereby reducing the deposition amount of carbon fluoropolymer in the edge area of the film layer.
[0093] S43, introducing sulfur hexafluoride gas into the process chamber, and turning on an excitation power supply to excite the sulfur hexafluoride gas to form plasma;
[0094] Specifically, when performing the above step S43, the sulfur hexafluoride gas is simultaneously introduced from the central gas inlet and the edge gas inlet at the top of the process chamber; specifically, the central flow rate value of the sulfur hexafluoride gas may range from 10 sccm to 1000 sccm, preferably 500 sccm; the edge flow rate value of the sulfur hexafluoride gas may range from 10 sccm to 1000 sccm, preferably 300 sccm;
[0095] S44, turning on the bias power supply and outputting a first bias power value to the lower electrode to attract plasma to bombard the protective layer; specifically, the first bias power value is in the range of 5W to 500W, preferably 100W;
[0096] S45, introducing a mixed gas containing sulfur hexafluoride and oxygen into the process chamber, and turning on an excitation power supply to ignite the mixed gas; specifically, the oxygen flow rate value may range from 10 sccm to 1000 sccm, preferably 500 sccm; the sulfur hexafluoride gas center flow rate value may range from 10 sccm to 1000 sccm, preferably 500 sccm; the sulfur hexafluoride gas edge flow rate value may range from 10 sccm to 1000 sccm, preferably 300 sccm;
[0097] S46, turning on the bias power supply to output a second bias power value to the lower electrode, which can attract the plasma containing sulfur ions and oxygen ions toward the film layer;
[0098] Specifically, fluorine ions and oxygen ions can react with silicon carbide to generate silicon tetrafluoride and carbon dioxide, specifically converting carbon atoms and silicon atoms in the silicon carbide material into silicon tetrafluoride gas and carbon dioxide gas, thereby completing the chemical etching of the silicon carbide film layer. At the same time, since both silicon tetrafluoride gas and carbon dioxide gas are gases, they can be extracted from the chamber during the process to avoid remaining in the through hole. Specifically, the second bias power value ranges from 5W to 500W, preferably 25W.
[0099] It should be noted that the above-mentioned second bias power value should be smaller than the above-mentioned first bias power value. The reason for such setting is that, when performing step S44, by adopting a larger first bias power value, it is beneficial to give the plasma a larger kinetic energy, thereby helping to attract the plasma to bombard the protective layer; and when performing step S45, a smaller second bias power value is adopted to attract the plasma to the surface of the film layer so that it reacts with the film layer material, without giving the plasma a larger kinetic energy.
[0100] S47, determine whether the current number of cycles reaches the preset total number of cycles, if yes, the process ends; if no, add 1 to the current number of cycles and proceed to step S48;
[0101] Specifically, the greater the total number of cycles, the greater the corresponding total etching depth, so the preset total number of cycles can be set according to the total target depth of the through hole;
[0102] S48, reset the current chamber pressure P so that the current chamber pressure P satisfies:
[0103] P=P initial +(P final -P initial )×n / n total ;
[0104] At the same time, reset the current excitation power value p so that the current excitation power value p satisfies:
[0105] p=p initial +(p final -p initial )×n / n total ; and return to step S41 to proceed to the next cycle.
[0106] Specifically, the preset initial chamber pressure value P initial Less than the preset terminal chamber pressure value P finalTherefore, as the number of cycles n increases, the current chamber pressure P will increase uniformly. Since the mean free path of the plasma will decrease with the chamber pressure, the cyclic increase of the current chamber pressure can gradually reduce the kinetic energy of the plasma in the etching step, so that as the number of cycles increases, the etching amount becomes smaller and smaller, thereby being able to etch a hole with an inclined hole wall on the silicon carbide film layer; the preset initial excitation power value p initial Greater than the preset final excitation power value p final Therefore, as the number of cycles n increases, the current excitation power value p will decrease evenly. Since the smaller the excitation power, the smaller the ionization rate of the process gas, reducing the excitation power can reduce the amount of plasma used for etching, which helps to form an inclined hole wall.
[0107] This embodiment also provides an etching process recipe, which is specifically: when performing the above step S42 (deposition step), the chamber pressure of the process chamber is 35mTorr, the center power of the upper electrode is 1800W-500W, the edge power of the upper electrode is 500W, the power of the lower electrode is 1W, the center flow rate of octafluorocyclobutane is 350sccm, the edge flow rate of octafluorocyclobutane is 150sccm, and the process time of step S42 is 2s;
[0108] When performing the above step S43 and step S44 (bombardment step), the chamber pressure range of the process chamber is 35mTorr to 65mTorr, the center power of the upper electrode is 2000W to 500W, the edge power of the upper electrode is 500W, the power of the lower electrode is 100W, the center flow rate of sulfur hexafluoride is 500sccm, the edge flow rate of sulfur hexafluoride is 300sccm, the flow rate of oxygen is 500sccm, and the process duration of step S44 is 1s;
[0109] When performing the above-mentioned step S45 and step S46 (etching step), the chamber pressure range of the process chamber is 35mTorr~65mTorr, the center power of the upper electrode is 2000W~500W, the edge power of the upper electrode is 500W, the lower electrode power is 25W, the center flow rate of sulfur hexafluoride is 500sccm, the edge flow rate of sulfur hexafluoride is 300sccm, the flow rate of oxygen is 500sccm, and the process time of step S46 is 4s.
[0110] Figure 3 The figure shows the hole wall morphology of the through hole obtained by the etching method applied to the silicon carbide film layer provided in this embodiment. Figure 3 It can be seen that by adopting the hole etching method applied to the silicon carbide film layer provided in this embodiment, a through hole with an inclined hole wall can be etched on the silicon carbide film layer.
[0111] Example 3
[0112] Based on Example 1, this embodiment provides a through-hole etching method applied to a gallium nitride film layer, such as Figure 4 As shown, it specifically includes:
[0113] S51, preset the initial chamber pressure value P initial , preset terminal chamber pressure value P final , preset initial excitation power value p initial , preset final excitation power value p final , preset total number of cycles n total Make settings;
[0114] S52, introducing boron trichloride gas into the process chamber, turning on an excitation power supply to excite the boron trichloride gas to form a plasma, wherein the plasma contains boron ions and chloride ions, wherein the boron ions undergo a replacement reaction with the gallium nitride film layer under the catalysis of high temperature and high pressure, and form a dense gallium boride compound in the gallium nitride film layer, so that the gallium boride compound is deposited on the surface of the film layer to form a protective layer;
[0115] Specifically, when performing the above step S52, the boron trichloride gas is simultaneously introduced through the central air inlet and the edge air inlet at the top of the process chamber, wherein the boron trichloride gas flow rate at the central air inlet at the top of the process chamber is the central flow rate of the boron trichloride gas, and the boron trichloride gas flow rate at the central air inlet at the top of the process chamber is the edge flow rate of the boron trichloride gas; specifically, the central flow rate value of the boron trichloride gas may range from 10 sccm to 1000 sccm, preferably 350 sccm; the edge flow rate of the boron trichloride gas may range from 10 sccm to 1000 sccm, preferably 150 sccm;
[0116] When performing the above step S52, the excitation power supply applies excitation power to the central area and the edge area of the upper electrode respectively, wherein the excitation power applied to the central area of the upper electrode is the central power, and the excitation power applied to the edge area of the upper electrode is the edge power; specifically, the central power applied by the excitation power supply to the process chamber has a value range of 500W to 5000W, preferably 2000W; the edge power applied to the upper electrode of the process chamber has a value range of 500W to 3000W, preferably 1000W;
[0117] S53, introducing chlorine gas into the process chamber, and turning on the excitation power supply to make the chlorine gas glow; specifically, the value range of the central flow value of the chlorine gas can be 10 sccm to 1000 sccm, preferably 500 sccm; the value range of the edge flow value of the chlorine gas can be 10 sccm to 1000 sccm, preferably 300 sccm;
[0118] S54, turning on the bias power supply and outputting a first bias power value to the lower electrode to attract plasma to bombard the protective layer; specifically, the value range of the chlorine gas center flow value can be 10 sccm to 1000 sccm, preferably 500 sccm; the value range of the chlorine gas edge flow value can be 10 sccm to 1000 sccm, preferably 300 sccm;
[0119] S55, introducing chlorine gas into the process chamber, and turning on an excitation power supply to cause the chlorine gas to glow;
[0120] S56, turning on the bias power supply, outputting a second bias power value to the lower electrode, which can attract the plasma containing chloride ions to the film layer. Specifically, the chloride ions can react with the gallium nitride film layer to generate gallium trichloride gas, which can be extracted from the chamber to chemically etch the gallium nitride film layer; specifically, the second bias power value ranges from 5W to 500W, preferably 25W;
[0121] S57, determine whether the current number of cycles reaches the preset total number of cycles, if yes, the process ends; if no, add 1 to the current number of cycles and proceed to step S58;
[0122] Specifically, the greater the total number of cycles, the greater the corresponding total etching depth, so the preset total number of cycles can be set according to the total target depth of the through hole;
[0123] S58: Reset the current chamber pressure P so that the current chamber pressure P satisfies:
[0124] P=P initial +(P final -P initial )×n / n total ;
[0125] At the same time, reset the current excitation power value p so that the current excitation power value p satisfies:
[0126] p=p initial +(p final -p initial )×n / n total ; and return to step S51 to perform the next cycle; specifically, the preset initial chamber pressure value P initial Less than the preset terminal chamber pressure value P final Therefore, as the number of cycles n increases, the current chamber pressure P will increase uniformly. Since the mean free path of the plasma will decrease with the chamber pressure, the cyclic increase of the current chamber pressure can gradually reduce the kinetic energy of the plasma in the etching step, so that as the number of cycles increases, the etching amount becomes smaller and smaller, thereby being able to etch a hole with an inclined hole wall on the gallium nitride film layer; the preset initial excitation power value p initialGreater than the preset final excitation power value p final Therefore, as the number of cycles n increases, the current excitation power value p will decrease evenly. Since the smaller the excitation power, the smaller the ionization rate of the process gas, reducing the excitation power can reduce the amount of plasma used for etching, which helps to form an inclined hole wall.
[0127] The above-mentioned embodiments provide an etching method for an inclined through hole, which cyclically performs a deposition step, a bombardment step, and an etching step on the surface of the through hole, and increases the chamber pressure and reduces the excitation power after each cycle. Since the greater the chamber pressure, the shorter the mean free path of the plasma, the etching intensity of the plasma on the through hole gradually weakens as the number of cycles increases, thereby making the etching amount of the etching step gradually decrease as the number of cycles increases; at the same time, since the smaller the excitation power value, the smaller the ionization rate of the process gas, the amount of plasma used for etching gradually decreases as the number of cycles increases, thereby also making the etching amount of the etching step decrease as the number of cycles increases, and finally making the hole wall of the through hole tilted at a specified angle, thereby meeting different process requirements.
[0128] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A method for etching an inclined through hole, characterized in that: The method is used for etching a through hole with inclined hole wall on a film layer made of a wide bandgap semiconductor material, wherein the wide bandgap semiconductor material comprises gallium nitride, and the etching method comprises the following steps which are performed cyclically: S1, depositing a protective layer on the hole wall of the through hole; wherein the deposition gas used in step S1 is boron trichloride; S2, etching the protective layer on the bottom surface of the through hole until the bottom surface of the through hole is exposed; S3, etching the bottom surface of the through hole to a preset depth; S4, determine whether the current number of cycles reaches the preset total number of cycles, if not, add 1 to the current number of cycles, and proceed to step S5; if yes, the process ends; S5, increasing the chamber pressure value by a preset first unit adjustment amount, and reducing the excitation power value by a preset second unit adjustment amount to reduce the etching amount, and returning to step S1, wherein the excitation power is the upper electrode power.
2. The etching method according to claim 1, characterized in that: The first unit adjustment amount satisfies the following formula: P1=(P final -P initial ) / n total Wherein, P1 represents the first unit adjustment amount, P initial Indicates the preset initial chamber pressure value, P final Indicates the preset terminal chamber pressure value, n total Indicates the preset total number of cycles.
3. The etching method according to claim 1, characterized in that: The second unit adjustment amount satisfies the following formula: p2=(p initial -p final ) / n total Wherein, p2 represents the adjustment amount of the second unit, p initial Indicates the preset initial excitation power value, p final Indicates the preset final excitation power value, n total Indicates the preset total number of cycles.
4. The etching method according to claim 1, characterized in that: The step S1 comprises: S11, introducing deposition gas into the process chamber; S12, turning on an excitation power supply to output a first excitation power value to the process chamber to excite the deposition gas to form a plasma of a material capable of forming the protective layer, so as to deposit the protective layer.
5. The etching method according to claim 1, characterized in that: The step S2 comprises: S21, introducing bombardment gas into the process chamber; S22, turning on the excitation power supply to output a second excitation power value to the process chamber to excite the bombardment gas to form a bombardment plasma; S23, turning on the bias power supply, outputting a first bias power value to the lower electrode, so that the bombardment plasma physically bombards the protective layer located on the bottom surface of the through hole to etch the protective layer on the bottom surface of the through hole.
6. The etching method according to claim 1, characterized in that: The step S3 comprises: S31, introducing etching gas into the process chamber; S32, turning on the excitation power supply to output a third excitation power value to the process chamber to excite the etching gas to form an etching plasma; S33, turning on the bias power supply, outputting a second bias power value to the lower electrode, so that the etching plasma chemically etches the bottom surface of the through hole.
7. The etching method according to claim 1, characterized in that: The chamber pressure value ranges from 5 mTorr to 500 mTorr.
8. The etching method according to claim 1, characterized in that: The excitation power value ranges from 500W to 3000W.