Thermosetting resin composition
By introducing a self-crosslinking copolymer and a triazine-based ultraviolet absorber into the polymer material, a resin composition with high refractive index and light resistance is solved, and the problem of the fused ring hydrocarbon-based material being easily deteriorated is achieved, and high Optical member materials with refractive index and light resistance.
Patent Information
- Application Number
- CN201980076609.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-11-21
- Filing Date
- 2019-11-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2039-11-07
AI Technical Summary
When the conventional polymer materials are introduced into the condensed ring hydrocarbon group to increase the refractive index, it is easy to deteriorate ultraviolet light, making it difficult to take into account both high refractive index and high light resistance.
Using a thermosetting resin composition containing a self-crosslinking copolymer, a triazine-based ultraviolet absorber and an organic solvent, a cured film with high refractive index and light resistance is formed by introducing a triazine ring structure and a carboxy group protection into a fused ring hydrocarbon group. and microlens.
It has achieved high refractive index, excellent transparency, heat resistance, solvent resistance and flatness, and has a dry etching rate equal to that of the resist, which is suitable for the production of optical components.
Smart Images

Figure CN113166324B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thermosetting resin composition comprising a self-crosslinking copolymer, an ultraviolet absorber having at least one triazine ring in one molecule, and an organic solvent, and can be used for the production of a high-refractive-index planarizing film and a high-refractive-index microlens. Background Art
[0002] In recent years, in the field of electronic devices such as liquid crystal displays, organic EL displays, light-emitting diodes, solar cells, CCD / CMOS image sensors, etc., for optical components such as protective films, flattening films, insulating films, anti-reflection films, refractive index control films, microlenses, intra-layer lenses, optical waveguides, and film substrates, resin compositions of polymer materials with excellent transparency in the visible light region are often used. Such optical components require not only transparency, but also excellent heat resistance and light resistance. Furthermore, in order to improve the efficiency of light extraction and the improvement of light focusing, the optical component also often requires a high refractive index.
[0003] Generally speaking, as a method for increasing the refractive index of a polymer material, a method of, for example, introducing an aromatic ring, a halogen atom other than a fluorine atom, a sulfur atom, a metal atom, or a hydrogen bond into the molecule of the polymer material is used. Regarding the introduction of an aromatic ring, the introduction of a condensed cyclic hydrocarbon group such as a naphthalene ring or anthracene ring is an effective means for increasing the refractive index of a polymer material compared to a monocyclic hydrocarbon group such as a phenyl group (Patent Documents 1 and 2).
[0004] In addition, as one of the manufacturing methods for microlenses for CCD / CMOS image sensors, the etch-back method is known (Patent Document 3 and Patent Document 4). That is, a resist pattern is formed on a microlens resin layer formed on a color filter layer, and the resist pattern is reflowed by heat treatment to form a lens pattern. Using the lens pattern formed by reflowing the resist pattern as an etching mask, the underlying microlens resin layer is etched back, and the lens pattern shape is transferred to the microlens resin layer, thereby manufacturing a microlens. For the etch-back method, when the lens pattern shape is faithfully transferred to the underlying microlens resin layer, the dry etching rate X of the resist pattern is required to be equal to the dry etching rate Y of the microlens resin layer (X:Y=1:0.8~1.2) (Patent Document 5).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 8-53517
[0008] Patent Document 2: International Publication No. 2008 / 143095
[0009] Patent Document 3: Japanese Patent Application Laid-Open No. 1-10666
[0010] Patent Document 4: Japanese Patent Application Laid-Open No. 6-112459
[0011] Patent Document 5: International Publication No. 2013 / 005619 Summary of the invention
[0012] Problems to be solved by the invention
[0013] If a condensed cyclic hydrocarbon group is introduced into the molecule of a polymer material, the wavelength of light absorption is increased, and the polymer material is easily degraded by light such as ultraviolet rays. Therefore, an optical component produced using a resin composition using a polymer material into which a condensed cyclic hydrocarbon group is introduced has a problem that it is difficult to have both a high refractive index and high light resistance because it is easy to cause quality degradation such as discoloration.
[0014] The present invention is proposed based on the above situation, and its purpose is to provide a thermosetting resin composition that can form a cured film having a high refractive index and excellent transparency, heat resistance, light resistance, solvent resistance, flatness, and a dry etching rate equivalent to that of a resist. In addition, another purpose of the present invention is to provide a planarized film and a microlens having a high refractive index and excellent transparency, heat resistance, light resistance, and solvent resistance.
[0015] Methods for solving problems
[0016] The inventors of the present invention have conducted intensive research to solve the above problems and have completed the present invention. That is, the present invention is a thermosetting resin composition comprising: a self-crosslinking copolymer having a structural unit represented by the following formula (1), a structural unit represented by the following formula (2), and a structural unit represented by the following formula (3); a triazine-based ultraviolet absorber; and an organic solvent, wherein the triazine-based ultraviolet absorber is contained in a ratio of 3% to 20% by mass relative to the content of the self-crosslinking copolymer.
[0017]
[0018] [In formula (1) to formula (3), Ar represents a condensed hydrocarbon group, R 1 and R 2 Each independently represents a hydrogen atom or a methyl group, R 3 represents a single bond or an alkylene group, A 1 represents a group having an oxirane ring, R 4 represents an alkyl group, A 2 represents an alkoxy group.]
[0019] The condensed ring hydrocarbon group is, for example, a naphthyl group, and the group having an oxirane ring is, for example, an epoxy group.
[0020] The self-crosslinking copolymer contains, for example, at least 70 mol % of the structural unit represented by the formula (1). The self-crosslinking copolymer has, for example, a weight average molecular weight of 6,000 to 25,000.
[0021] The triazine-based ultraviolet absorber is a compound comprising a triazine ring and three phenyl groups bonded to carbon atoms of the triazine ring, wherein the phenyl group may have a substituent, and at least one of the three phenyl groups is a group represented by the following formula (4).
[0022]
[0023] (wherein, * represents a bond to the carbon atom of the triazine ring, A 3 and A 4 Each independently represents a hydrogen atom or an organic group. )
[0024] The thermosetting resin composition of the present invention may further contain a surfactant.
[0025] The thermosetting resin composition of the present invention is, for example, a resin composition for a planarizing film or a resin composition for a microlens.
[0026] Effects of the Invention
[0027] The thermosetting resin composition of the present invention is self-crosslinking type because the copolymer included in the composition does not need to necessarily add a crosslinking agent, and has thermosetting properties. In addition, the thermosetting resin composition of the present invention is excellent in storage stability because the carboxyl group is blocked (protected) in the structural unit shown in the formula (3) of the above-mentioned copolymer. Further, the cured film formed by the thermosetting resin composition of the present invention has a high refractive index (more than 1.65), excellent transparency, heat resistance, solvent resistance, flatness and an etching rate equivalent to that of a resist pattern. Therefore, the thermosetting resin composition of the present invention is suitable as a material for forming a microlens and a flattened film. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram showing a cured film formed by applying the resin composition of the present invention on a stepped substrate and baking the coating. DETAILED DESCRIPTION
[0029] Hereinafter, each component of the thermosetting resin composition of the present invention is described in detail. In the thermosetting resin composition of the present invention, the content of the solid component defined as all the components after removing the solvent from the composition is usually 1% by mass to 50% by mass. In addition, in this specification, even if it is a liquid component, it is also treated as a "solid component" for convenience.
[0030] <Self-crosslinking copolymer>
[0031] The self-crosslinking copolymer contained in the thermosetting resin composition of the present invention is a copolymer having structural units represented by the above formula (1), formula (2) and formula (3).
[0032] Specific examples of the compound (monomer) forming the structural unit represented by the above formula (1) include 1-vinylnaphthalene, 2-vinylnaphthalene, 6-methyl-2-vinylnaphthalene, 5,8-dimethyl-2-vinylnaphthalene, 6-methoxy-2-vinylnaphthalene, 5,8-dimethoxy-2-vinylnaphthalene, 6-hydroxy-2-vinylnaphthalene, 5,8-dihydroxy-2-vinylnaphthalene, 6-bromo-2-vinylnaphthalene, 5,8-dibromo-2-vinylnaphthalene, 1-vinylanthracene, 2-vinylanthracene, 9-vinylanthracene, and N-vinylcarbazole. These compounds may be used alone or in combination of two or more.
[0033] Specific examples of the compound (monomer) forming the structural unit represented by the above formula (2) include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclopentyl methyl (meth)acrylate, 3,4-epoxycyclohexyl methyl (meth)acrylate, 5,6-epoxy-2-bicyclo[2.2.1]heptyl methyl (meth)acrylate, 3,4-epoxytricyclo[5.2.1.0 2,6 ]Decan-8-yl (meth)acrylate. These monomers can be used alone or in combination of two or more. In addition, in this specification, the descriptions of (meth)acrylate and (meth)acrylic acid represent both methacrylate and acrylate, and methacrylic acid and acrylic acid.
[0034] The compound (monomer) forming the structural unit represented by the above formula (3) is obtained as an acrylic acid ester or a methacrylic acid ester having a protected carboxyl group by reacting acrylic acid or methacrylic acid with an alkenyl ether compound. Instead of the above method, the structural unit represented by the above formula (3) can also be formed by a method in which an alkenyl ether compound is reacted with a structural unit obtained by (co)polymerizing acrylic acid or methacrylic acid.
[0035] The alkenyl ether compound is represented by the following formula (5).
[0036]
[0037] (Where R 5 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, R 6 represents an alkyl group having 1 to 10 carbon atoms or a cyclic hydrocarbon group having 6 to 10 carbon atoms.
[0038] The reaction of the compound having a carboxyl group and the alkenyl ether compound can be carried out by stirring at 70° C. using monooctyl phosphate, which is one of phosphoric acid esters, as a catalyst as described in, for example, Japanese Patent No. 3042033.
[0039] Examples of the alkenyl ether compound represented by the formula (5) include methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, tert-butyl vinyl ether, n-hexyl vinyl ether, cyclohexyl vinyl ether and 2-ethylhexyl vinyl ether.
[0040] The structural unit represented by the above formula (3) is represented by, for example, the following formula (3-1).
[0041]
[0042] (Where R 2 represents a hydrogen atom or a methyl group, R 6 represents an alkyl group having 1 to 10 carbon atoms or a cyclic hydrocarbon group having 6 to 10 carbon atoms.
[0043] Specific examples of the compound (monomer) forming the structural unit represented by the above formula (3) include 1-methoxyethyl (meth) acrylate, 1-ethoxyethyl (meth) acrylate, 1-propoxyethyl (meth) acrylate, 1-isopropoxyethyl (meth) acrylate, 1-n-butoxyethyl (meth) acrylate, 1-tert-butoxyethyl (meth) acrylate, 1-n-hexyloxyethyl (meth) acrylate, and 1-cyclohexyloxyethyl (meth) acrylate. In addition, these monomers may be used alone or in combination of two or more.
[0044] In the self-crosslinking copolymer having the structural units represented by the above formula (1), formula (2) and formula (3), the content of the structural unit represented by the above formula (1) is 60 mol% to 95 mol%, preferably 70 mol% to 90 mol%, relative to the sum of 100 mol% of the structural units represented by the above formula (1), the structural units represented by the above formula (2) and the structural units represented by the above formula (3), the content of the structural unit represented by the above formula (2) is 2 mol% to 20 mol%, preferably 5 mol% to 15 mol%, and the content of the structural unit represented by the above formula (3) is 2 mol% to 30 mol%, preferably 5 mol% to 15 mol%.
[0045] The weight average molecular weight of the self-crosslinking copolymer is usually 1,000 to 100,000, preferably 6,000 to 25,000, and more preferably 6,000 to 20,000. The weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using polystyrene as a standard sample.
[0046] The content of the self-crosslinking copolymer in the thermosetting resin composition of the present invention is usually 50 to 99% by mass, preferably 70 to 95% by mass, based on the solid content of the thermosetting resin composition.
[0047] In the present invention, the method for obtaining the self-crosslinking copolymer is not particularly limited, and the self-crosslinking copolymer is generally obtained by polymerizing the compounds (monomers) forming the structural units represented by the above formula (1), formula (2) and formula (3), and, if necessary, compounds other than the above compounds (hereinafter referred to as compound X in this specification) in a solvent in the presence of a polymerization initiator, usually at a temperature of 50° C. to 120° C. The copolymer obtained in this way is usually in a solution state dissolved in a solvent, and can be used in the thermosetting resin composition of the present invention without isolation in this state.
[0048] In addition, the solution of the self-crosslinking copolymer obtained by operating as described above is put into the diethyl ether, toluene, methanol, ethanol, isopropanol, acetonitrile or water stirred and the copolymer is reprecipitated, the precipitate generated is decanted or filtered, after washing as required, normal temperature drying or heat drying is carried out under normal pressure or reduced pressure, so that the copolymer can be made into an oily substance or powder. By such operation, the polymerization initiator and unreacted compound coexisting with the above-mentioned copolymer can be removed. In the present invention, the oily substance or powder of the above-mentioned copolymer can be directly used, or the oily substance or powder can be made to be, for example, redissolved in the solvent described later and used as the state of the solution.
[0049] Specific examples of the compound X include styrene, 4-vinylbiphenyl, 2-vinylfluorene, acenaphthene, (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, γ-butyrolactone (meth)acrylate, Esters, indene, maleimide, N-methylmaleimide, N-ethylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-benzylmaleimide, N-(4-hydroxyphenyl)maleimide, 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, 5-hydroxypentyl vinyl ether, 6-hydroxyhexyl vinyl ether, 4-hydroxycyclohexyl vinyl ether, 1,4-cyclohexanedimethanol monovinyl ether, diethylene glycol monovinyl ether and dipropylene glycol monovinyl ether.
[0050] <Triazine-based UV absorbers>
[0051] Examples of the triazine ultraviolet absorber contained in the thermosetting resin composition of the present invention include compounds represented by the following formulas (T-1) to (T-15).
[0052]
[0053] Commercially available products of the triazine-based ultraviolet absorbers include, for example, Tinuvin [registered trademark] 400, Tinuvin 405, Tinuvin 460, Tinuvin 477, Tinuvin 479, Tinuvin 1577ED, Tinuvin 1600 (all manufactured by BASF Japan Co., Ltd.), ADECAS STABB [registered trademark] LA-46, ADECAS STABB LA-F70 (all manufactured by ADEKA Co., Ltd.), and Kemisorb [registered trademark] 102 (manufactured by Chemipro Chemicals Co., Ltd.). These triazine-based ultraviolet absorbers may be used alone or in combination of two or more.
[0054] The content of the triazine ultraviolet absorber contained in the thermosetting resin composition of the present invention is preferably 3% by mass to 20% by mass, more preferably 5% by mass to 20% by mass, based on the content of the self-crosslinking copolymer.
[0055] The method for preparing the thermosetting resin composition of the present invention is not particularly limited, and examples thereof include a method in which a self-crosslinking copolymer having structural units represented by the above formula (1), formula (2) and formula (3) is dissolved in an organic solvent described later, and the above triazine-based ultraviolet absorber is mixed in a predetermined ratio in the resulting solution to prepare a uniform solution. Furthermore, a method in which other additives are further added and mixed as needed at an appropriate stage of the preparation method may be mentioned.
[0056] <Organic solvents>
[0057] The organic solvent contained in the thermosetting resin composition of the present invention is not particularly limited as long as it dissolves the self-crosslinking copolymer and triazine-based ultraviolet absorber contained in the thermosetting resin composition. Examples of such organic solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether, propylene glycol propyl ether acetate, propylene glycol monobutyl ether, propylene glycol monobutyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, and cyclohexanone. , ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, γ-butyrolactone, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone. These organic solvents can be used alone or in combination of two or more.
[0058] Among the above-mentioned organic solvents, from the viewpoint of improving the leveling property of a coating film formed by applying the thermosetting resin composition of the present invention on a substrate, preferred are propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 2-heptanone, ethyl lactate, butyl lactate, methyl pyruvate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, cyclopentanone, cyclohexanone, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and γ-butyrolactone.
[0059] <Surfactant>
[0060] Furthermore, the thermosetting resin composition of the present invention may contain a surfactant for the purpose of improving coating properties. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkyl aryl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether, polyoxyethylene / polyoxypropylene block copolymers, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate. Sugar alcohol fatty acid esters, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tristearate and other polyoxyethylene sorbitan fatty acid esters and other nonionic surfactants, Eftop EF301 (registered trademark), Eftop EF303, Eftop EF352 (all manufactured by Mitsubishi Material Electronics Co., Ltd.), Megapack (registered trademark) Standard〕F171, メガファックF173, メガファックR-30, メガファックR-40, メガファックR-40-LM (above, manufactured by DIC Co., Ltd.), Fururo FC430, Fururo FC431 (above) , manufactured by Sumitomo Solar (Co., Ltd.), アサヒガード [registered trademark] AG710, サーフロン [registered trademark] S- 382. サーフロンSC101, サーフロンSC102, サーフロンSC103, サーフロンSC10 4. Fluorine-based surfactants such as Surflon SC105, Surflon SC106 (manufactured by AGC Co., Ltd.), FTX-206D, FTX-212D, FTX-218, FTX-220D, FTX-230D, FTX-240D, FTX-212P, FTX-220P, FTX-228P, and FTX-240G (manufactured by Neos Co., Ltd.), and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). These surfactants may be used alone or in combination of two or more.
[0061] When the above-mentioned surfactant is used, the content in the thermosetting resin composition of the present invention is usually 0.0001% by mass to 3% by mass, preferably 0.001% by mass to 1% by mass, and more preferably 0.01% by mass to 0.5% by mass, based on the solid content of the resin composition.
[0062] Furthermore, the thermosetting resin composition of the present invention may contain additives such as a curing agent, a curing aid, a sensitizer, a plasticizer, an antioxidant, a light stabilizer (HALS), and an adhesion aid as necessary, unless the effects of the present invention are impaired.
[0063] Hereinafter, the use of the thermosetting resin composition of the present invention will be described.
[0064] <Method for preparing cured film>
[0065] The preparation method of the cured film using the thermosetting resin composition of the present invention is described. On a substrate (for example, a PET film, a TAC film, a semiconductor substrate, a glass substrate, a quartz substrate, a silicon wafer, and a substrate having various metal films or color filters formed on their surfaces), after the thermosetting resin composition of the present invention is applied by a suitable coating method such as a spin coater or a coater, a heating device such as a hot plate or an oven is used to bake and prepare the cured film. The baking conditions are appropriately selected from a baking temperature of 50°C to 300°C and a baking time of 0.1 minute to 360 minutes. The baking when making the above-mentioned cured film can be processed in more than 2 steps. In addition, the film thickness of the cured film formed by the thermosetting resin composition of the present invention is, for example, 0.001 μm to 1000 μm, preferably 0.01 μm to 100 μm, and more preferably 0.1 μm to 10 μm.
[0066] <Microlens production method>
[0067] The method for making a microlens using the thermosetting resin composition of the present invention is described. A resist is applied to a cured film made by the method for making the cured film, and the resist is exposed through a prescribed mask, and post-exposure heating (PEB) is performed as needed, and further alkali development, rinsing, and drying are performed to form a prescribed resist pattern on the cured film. Exposure can use, for example, g-rays, i-rays, KrF excimer lasers, and ArF excimer lasers. Next, a heat treatment is performed to reflow the resist pattern to form a lens pattern. Using the lens pattern as an etching mask, the cured film of the lower layer of the lens pattern is etched back, and the shape of the lens pattern is transferred to the cured film to make a microlens.
[0068] Example
[0069] The present invention will be described in more detail below based on Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0070] [Measurement of weight average molecular weight of copolymer obtained in the following synthesis example]
[0071] Equipment: GPC system manufactured by JASCO Corporation
[0072] Column: Shodex [registered trademark] GPC KF-804L and GPC KF-803L
[0073] Column oven: 40°C
[0074] Flow rate: 1mL / min
[0075] Eluent: Tetrahydrofuran
[0076] [Synthesis of self-crosslinking copolymer]
[0077] <Synthesis example 1>
[0078] 15.0 g of 2-vinylnaphthalene, 3.9 g of 1-n-butoxyethyl methacrylate, 3.0 g of glycidyl methacrylate, and 1.5 g of 2,2'-azobisisobutyronitrile were dissolved in 23.3 g of propylene glycol monomethyl ether acetate. The resulting solution was added dropwise to a flask containing 31.1 g of propylene glycol monomethyl ether acetate at 70°C over 4 hours. After the addition was completed, the mixture was reacted for 18 hours to obtain a copolymer solution (solid content concentration 30% by mass). The weight average molecular weight Mw of the resulting copolymer was 6,000 (polystyrene conversion).
[0079] <Synthesis example 2>
[0080] 18.0 g of 2-vinylnaphthalene, 2.7 g of 1-n-butoxyethyl methacrylate, 2.1 g of glycidyl methacrylate, and 0.7 g of 2,2'-azobisisobutyronitrile were dissolved in 23.5 g of propylene glycol monomethyl ether acetate. The resulting solution was added dropwise to a flask containing 31.4 g of propylene glycol monomethyl ether acetate at 70°C over 4 hours. After the addition was completed, the reaction was carried out for 18 hours to obtain a copolymer solution (solid content concentration 30% by mass). The weight average molecular weight Mw of the resulting copolymer was 16,000 (polystyrene conversion).
[0081] <Synthesis Example 3>
[0082] After dissolving 20.0 g of 2-vinylnaphthalene, 1.4 g of 1-n-butoxyethyl methacrylate, 1.1 g of glycidyl methacrylate, and 0.5 g of 2,2'-azobisisobutyronitrile in 23.5 g of propylene glycol monomethyl ether acetate, the resulting solution was added dropwise over 4 hours to a flask containing 31.4 g of propylene glycol monomethyl ether acetate at 70°C. After the addition was completed, the mixture was reacted for 18 hours to obtain a copolymer solution (solid content concentration 30% by mass). The weight average molecular weight Mw of the resulting copolymer was 20,000 (polystyrene conversion).
[0083] [Preparation of Thermosetting Resin Composition]
[0084] <Example 1>
[0085] 20.0 g of the solution of the copolymer obtained in Synthesis Example 1, 0.3 g of the compound represented by the above formula (T-9) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0086] <Example 2>
[0087] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the above formula (T-9) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0088] <Example 3>
[0089] 20.0 g of the solution of the copolymer obtained in Synthesis Example 3, 0.3 g of the compound represented by the above formula (T-9) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0090] <Example 4>
[0091] 20.0 g of the copolymer solution obtained in Synthesis Example 1, 0.18 g of the compound represented by the above formula (T-9) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.0 g of propylene glycol monomethyl ether acetate and 14.0 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0092] <Example 5>
[0093] 20.0 g of the solution of the copolymer obtained in Synthesis Example 1, 0.6 g of the compound represented by the above formula (T-9) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 5.3 g of propylene glycol monomethyl ether acetate and 12.9 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0094] <Example 6>
[0095] 20.0 g of the solution of the copolymer obtained in Synthesis Example 1, 1.2 g of the compound represented by the above formula (T-9) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 3.3 g of propylene glycol monomethyl ether acetate and 11.5 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0096] <Example 7>
[0097] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the above formula (T-7) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0098] <Example 8>
[0099] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the above formula (T-6) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac [registered trademark] R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0100] <Example 9>
[0101] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the above formula (T-11) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0102] <Example 10>
[0103] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the above formula (T-13) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0104] <Example 11>
[0105] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the above formula (T-5) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0106] <Example 12>
[0107] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the above formula (T-4) as a triazine-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0108] <Comparative Example 1>
[0109] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2 and 0.003 g of Megaffac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 6.4 g of propylene glycol monomethyl ether acetate and 13.6 g of cyclohexanone to obtain a solution. Then, the obtained solution was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a thermosetting resin composition. The thermosetting resin composition prepared in this comparative example does not contain an ultraviolet absorber.
[0110] <Comparative Example 2>
[0111] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BT-1) as a benzotriazole-based ultraviolet absorber, and 0.003 g of Megaphage R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0112]
[0113] <Comparative Example 3>
[0114] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BT-2) as a benzotriazole-based ultraviolet absorber, and 0.003 g of Megaphage R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0115]
[0116] <Comparative Example 4>
[0117] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BT-3) as a benzotriazole-based ultraviolet absorber, and 0.003 g of Megaphage R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0118]
[0119] <Comparative Example 5>
[0120] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BT-4) as a benzotriazole-based ultraviolet absorber, and 0.003 g of Megafac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0121]
[0122] <Comparative Example 6>
[0123] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BP-1) as a benzophenone-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0124]
[0125] <Comparative Example 7>
[0126] 20.0 g of the solution of the copolymer obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BP-2) as a benzophenone-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0127]
[0128] <Comparative Example 8>
[0129] 20.0 g of the copolymer solution obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BP-3) as a benzophenone-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0130]
[0131] <Comparative Example 9>
[0132] 20.0 g of the copolymer solution obtained in Synthesis Example 2, 0.3 g of the compound represented by the following formula (BP-4) as a benzophenone-based ultraviolet absorber, and 0.003 g of Megapac (registered trademark) R-40 (manufactured by DIC Corporation) as a surfactant were dissolved in 7.4 g of propylene glycol monomethyl ether acetate and 14.3 g of cyclohexanone to obtain a solution. The obtained solution was then filtered using a polyethylene microfilter having a pore size of 0.10 μm to prepare a thermosetting resin composition.
[0133]
[0134] [Solvent resistance test]
[0135] The thermosetting resin compositions prepared in Examples 1 to 12 and Comparative Examples 1 to 9 were applied to silicon wafers using a spin coater, baked on a hot plate at 100°C for 1 minute, and further baked at 220°C for 5 minutes to form a cured film with a thickness of 1 μm. These cured films were immersed in propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, cyclohexanone, 2-propanol, and a 2.38 mass % aqueous solution of tetramethylammonium hydroxide (hereinafter referred to as TMAH) at a temperature of 23°C for 5 minutes, and then dried by baking at 100°C for 1 minute. The film thickness of each of the above cured films was measured before and after dipping and drying, and the film thickness change was calculated. The solvent resistance was evaluated by marking "×" when the film thickness after drying increased or decreased by 5% or more relative to the film thickness before immersion even for one of the solvents used for the immersion, and "○" when the film thickness after drying increased or decreased by less than 5% relative to the film thickness before immersion for all the solvents used for the immersion. The evaluation results are shown in Table 1.
[0136] [Refractive index measurement]
[0137] The thermosetting resin compositions prepared in Examples 1 to 12 and Comparative Examples 1 to 9 were applied to silicon wafers using a spin coater, baked on a hot plate at 100°C for 1 minute, and further baked at 220°C for 5 minutes to form a cured film with a film thickness of 1 μm. The refractive index at a wavelength of 550 nm was measured using a spectroscopic ellipsometer M-2000 (Japan (Strain)) for these cured films. The evaluation results are shown in Table 1.
[0138] [Heat resistance test]
[0139] The thermosetting resin compositions prepared in Examples 1 to 12 and Comparative Examples 1 to 9 were applied to a quartz substrate using a spin coater, baked on a hot plate at 100°C for 1 minute, and further baked at 220°C for 5 minutes to form a cured film with a film thickness of 1 μm. With respect to these cured films, the transmittance was measured in the range of 400nm to 800nm using an ultraviolet visible spectrophotometer UV-2600 (manufactured by Shimadzu Corporation). Further, after these cured films were baked at 260°C for 5 minutes, the transmittance was measured again in the range of 400nm to 800nm. The minimum transmittance measured in the range of 400nm to 800nm after baking at 220°C for 5 minutes and at 260°C for 5 minutes, respectively, was 90% or more, and was set as "0", and the case of less than 90% was set as "×" to evaluate the heat resistance. The evaluation results are shown in Table 1.
[0140] [Light resistance test]
[0141] The thermosetting resin compositions prepared in Examples 1 to 12 and Comparative Examples 1 to 9 were applied to a quartz substrate using a spin coater, baked on a hot plate at 100°C for 1 minute, and further baked at 220°C for 5 minutes to form a cured film with a film thickness of 1 μm. With respect to these cured films, the transmittance was measured in the range of 400nm to 800nm using an ultraviolet visible spectrophotometer UV-2600 (manufactured by Shimadzu Corporation) . Further, after the light resistance test was carried out on these cured films under the following conditions, the transmittance was measured again in the range of 400nm to 800nm. The light resistance was evaluated by setting the minimum transmittance measured in the range of 400nm to 800nm before and after the light resistance test as 90% or more as "0", and setting the case of less than 90% as "×". The evaluation results are shown in Table 1.
[0142] 〔Lightfastness test conditions〕
[0143] Equipment: Xenon accelerated weathering tester Q-Sun Xe-1-B (manufactured by Q-Lab Corporation)
[0144] Light source: Xenon arc lamp
[0145] Optical filter: Window-B / SL
[0146] Illuminance: 60W / m 2 (Wavelength 300nm~400nm)
[0147] Black disk temperature: 63℃
[0148] Test time: 20 hours
[0149] [Leveling properties]
[0150] The thermosetting resin compositions prepared in Examples 1 to 12 were applied using a spin coater onto a step substrate (refer to Figure 1 ) was placed on a hot plate and baked at 100°C for 1 minute and further at 220°C for 5 minutes to form a film with a thickness of 1 μm. Figure 1 The flattening rate was calculated using the formula (1-(h2 / h1))×100 from the values of h1 (height difference of the height difference substrate) and h2 (height difference of the cured film, i.e., the height difference between the height of the cured film on the line and the height of the cured film on the gap) shown in the height difference substrate 1. The flattening rate was evaluated by setting the flattening rate to "0" for a flattening rate of 80% or more, "△" for a flattening rate of 50% or more and less than 80%, and "×" for a flattening rate of less than 50%. The evaluation results are shown in Table 1.
[0151] [Determination of dry etching rate]
[0152] The thermosetting resin compositions prepared in Examples 1 to 12 were applied to silicon wafers using a spin coater, and baked on a hot plate at 100° C. for 1 minute and further at 220° C. for 5 minutes to form a cured film with a film thickness of 1 μm. These cured films were dry-etched using a dry etching apparatus RIE-10NR (manufactured by Samco Co., Ltd.) (etching gas: CF4), and the dry etching rate was measured. Similarly, a resist solution (THMR-iP1800 (manufactured by Tokyo Ohka Industry Co., Ltd.) was applied to a silicon wafer using a spin coater, and baked on a hot plate at 90°C for 1.5 minutes, at 110°C for 1.5 minutes, and further at 180°C for 1 minute to form a resist film having a film thickness of 1 μm, and the dry etching rate was measured. Furthermore, the dry etching rate ratio of the cured film obtained from the thermosetting resin composition prepared in Examples 1 to 12 to the above-mentioned resist film was determined. The evaluation results are shown in Table 1.
[0153] [Table 1]
[0154] Table 1
[0155]
[0156] According to the results in Table 1, the cured film formed by the thermosetting resin composition of the present invention has high solvent resistance, high refractive index, high transparency, and the minimum transmittance in the wavelength range of 400nm to 800nm after heating at 260°C and after the light resistance test is 90% or more, and has high heat resistance and high light resistance. Furthermore, the cured films formed by the thermosetting resin composition of the present invention have excellent high-low difference flattening with a flattening rate of more than 80%. In addition, for the etch-back method, when the lens pattern shape is faithfully transferred to the underlying microlens resin layer, the dry etching rate X of the resist is required to be equal to the dry etching rate Y of the microlens resin layer (X:Y=1:0.8~1.2), but the cured film formed by the thermosetting resin composition of the present invention is the result of satisfying this condition.
[0157] On the other hand, although the cured films formed from the thermosetting resin compositions prepared in Comparative Examples 1 to 9 have high solvent resistance, high refractive index and high heat resistance, when subjected to a light resistance test, the minimum transmittance in the wavelength range of 400 nm to 800 nm decreases to less than 90%, resulting in a lack of light resistance.
[0158] Based on the above, the thermosetting resin composition of the present invention is useful as a resin composition for forming optical members such as protective films, planarizing films, insulating films, antireflection films, refractive index control films, microlenses, in-layer lenses, optical waveguides, and film substrates.
[0159] Explanation of symbols
[0160] 1: Height difference substrate
[0161] 2: Cured film
[0162] 3: Line width
[0163] 4: Gap between lines
[0164] h1: Height difference of the substrate
[0165] h2: height difference of the cured film.
Claims
1. A thermosetting resin composition comprising: A self-crosslinking copolymer having a structural unit represented by the following formula (1), a structural unit represented by the following formula (2), and a structural unit represented by the following formula (3-1); Triazine-based UV absorbers; and Organic solvents, The triazine-based ultraviolet absorber is contained in a ratio of 3% by mass to 20% by mass relative to the content of the self-crosslinking copolymer, In formula (1) to formula (3-1), Ar represents a condensed hydrocarbon group, and R 1 and R 2 Each independently represents a hydrogen atom or a methyl group, R 3 represents a single bond or an alkylene group, A 1 represents a group having an oxirane ring, R 6 represents an alkyl group having 1 to 10 carbon atoms or a cyclic hydrocarbon group having 6 to 10 carbon atoms, and The compound forming the structural unit represented by the formula (1) is selected from 1-vinylnaphthalene, 2-vinylnaphthalene, 6-methyl-2-vinylnaphthalene, 5,8-dimethyl-2-vinylnaphthalene, 6-methoxy-2-vinylnaphthalene, 5,8-dimethoxy-2-vinylnaphthalene, 6-hydroxy-2-vinylnaphthalene, 5,8-dihydroxy-2-vinylnaphthalene, 6-bromo-2-vinylnaphthalene, 5,8-dibromo-2-vinylnaphthalene, 1-vinylanthracene, 2-vinylanthracene, 9-vinylanthracene and N-vinylcarbazole, The compound forming the structural unit represented by the formula (2) is selected from glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclopentyl methyl (meth)acrylate, 3,4-epoxycyclohexyl methyl (meth)acrylate, 5,6-epoxy-2-bicyclo[2.2.1]heptyl methyl (meth)acrylate and 3,4-epoxytricyclo[5.2.1.0 2,6 ]Decan-8-yl (meth)acrylate, The triazine-based ultraviolet absorber is a compound comprising a triazine ring and three phenyl groups bonded to carbon atoms of the triazine ring, wherein the phenyl group may have a substituent, and at least one of the three phenyl groups is a group represented by the following formula (4): In formula (4), * represents a bond to a carbon atom of the triazine ring, and A 3 and A 4 Each independently represents a hydrogen atom or an organic group. 2 . The thermosetting resin composition according to claim 1 , wherein the condensed hydrocarbon group is a naphthyl group. 3 . The thermosetting resin composition according to claim 1 , wherein the self-crosslinking copolymer comprises at least 70 mol % of the structural unit represented by the formula (1). 4 . The thermosetting resin composition according to claim 1 , wherein the self-crosslinking copolymer has a weight average molecular weight of 6,000 to 25,000. 5 . The thermosetting resin composition according to claim 1 , further comprising a surfactant. The thermosetting resin composition according to claim 1 or 2, which is used for a planarization film.
7. The thermosetting resin composition according to claim 1 or 2, which is used for a microlens.
8. According to the thermosetting resin composition according to claim 1 or 2, the compound forming the structural unit represented by the formula (3-1) is selected from 1-methoxyethyl (meth)acrylate, 1-ethoxyethyl (meth)acrylate, 1-propoxyethyl (meth)acrylate, 1-isopropoxyethyl (meth)acrylate, 1-n-butoxyethyl (meth)acrylate, 1-tert-butoxyethyl (meth)acrylate, 1-n-hexyloxyethyl (meth)acrylate and 1-cyclohexyloxyethyl (meth)acrylate.
9. The thermosetting resin composition according to claim 1 or 2, wherein the triazine-based ultraviolet absorber is selected from the compounds represented by the following formula (T-1) to formula (T-15),