Electronic component and method of manufacturing the same
By coating and heating a paste containing copper particles and inorganic oxide particles on an inorganic substrate, the problem of insufficient adhesion between the copper electrode and the ceramic substrate was solved, achieving a strong connection between the copper electrode and the substrate and low resistance characteristics.
Patent Information
- Application Number
- CN202080007067.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-01-10
- Filing Date
- 2020-01-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-01-09
AI Technical Summary
In the existing technology, the adhesion between the copper electrode and the ceramic substrate is insufficient, and they are prone to peeling off under stress load. In particular, the problem of substrate damage caused by thermal stress during the high-temperature sintering and cooling process has not been effectively solved.
A paste containing copper particles, copper oxide particles and/or nickel oxide particles, as well as inorganic oxide particles with softening points, is coated on an inorganic substrate. The substrate is then heated in an inactive atmosphere at a temperature below the softening point of the inorganic oxides and above the sintering temperature of the copper particles. Subsequently, the substrate is heated at a temperature above the softening point of the inorganic oxides to form a copper sintered body and improve its adhesion.
This achieves a strong and tight bond between the copper electrode and the inorganic substrate, improving the mechanical reliability and conductivity of electronic components while reducing resistivity.
Smart Images

Figure CN113196471B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electronic component and a method for producing the same, and more particularly, to an electronic component having a copper electrode having strong adhesion to an inorganic substrate, a low-resistance and an inexpensive electrode, and a method for producing the same. Background Art
[0002] In the past, representative substrate materials used for electronic components include ceramic substrates such as oxide substrates (glass, crystal, aluminum oxide, gallium oxide, barium titanate, lead zirconate titanate, ferrite oxide, etc.), nitride substrates (aluminum nitride, silicon nitride, gallium nitride, etc.), and carbide substrates (silicon carbide, etc.). Such ceramic substrates are used in electronic components for a wide range of applications, such as wireless communication equipment and power conversion equipment.
[0003] In the case of electronic components, a planar electrode is formed on the surface of such a ceramic substrate to form a substrate for the electronic component.
[0004] As a method for forming an electrode on a ceramic substrate, a method of printing and sintering a conductive paste can be cited. Such a method can provide an inexpensive electronic component. In addition, by using a copper paste as the conductive paste, an even cheaper electronic component can be provided.
[0005] However, copper has insufficient adhesion to ceramics, so there is a situation where the copper electrode is peeled off from the ceramic substrate due to stress loads in the manufacturing process of electronic components or stress loads generated by temperature cycles during use as electronic components. In order to prevent such peeling, various studies have been conducted.
[0006] For example, Patent Document 1 describes that when a copper internal electrode is formed at the interface of two ferroelectric oxides having different dielectric constants, peeling can be prevented by including a component common to an additive component of at least one of the oxides in the internal electrode.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2011-119343 Summary of the invention
[0010] Problems to be solved by the invention
[0011] In the above-mentioned Patent Document 1, in order to add the additive component of the oxide adjacent to the electrode to the electrode and ensure the interface adhesion strength, sintering is performed at a high temperature of 800 to 1000°C. However, in the process of cooling from the sintering temperature to room temperature, there is a possibility that the thermal stress generated corresponding to the large temperature difference becomes larger and the ceramic substrate is easily damaged, so the adhesion between the copper electrode and the ceramic substrate is insufficient. In order to improve the adhesion between the copper electrode and the ceramic substrate, there is still room for improvement.
[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an electronic component in which a copper electrode and an inorganic substrate have strong adhesion.
[0013] Means for solving problems
[0014] The inventors of the present application have found that, in an electronic component produced by the following process, even when a cheap copper electrode is mainly used, the metal electrode has strong adhesion with an inorganic substrate, thereby completing the present invention. The above process is: after applying a paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate, heating at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper, and then performing a softening process of heating at a temperature higher than the softening point of the inorganic oxide particles in an inert gas atmosphere. Specifically, the present invention provides the following scheme.
[0015] (1) A method for manufacturing an electronic component, comprising the following steps: a coating step of coating a paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate; a sintering step of heating at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper; and a softening step of heating at a temperature higher than the softening point of the inorganic oxide particles in an inert gas atmosphere.
[0016] (2) The method for producing an electronic component according to (1), wherein a content of the oxide particles in the paste is 0.1% by mass or more and 10% by mass or less relative to the copper particles.
[0017] (3) A method for manufacturing an electronic component, comprising the following steps: a first coating step of coating a first paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate; a second coating step of coating a second paste containing copper particles and oxide particles containing copper and / or nickel and not containing an inorganic oxide component having a softening point, or the second paste containing copper particles and oxide particles containing copper and / or nickel and having an inorganic oxide component having a softening point in an amount of less than 0.1% by mass; a sintering step of heating in an inert gas atmosphere at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles to form a sintered body containing at least copper; and a softening step of heating in an inert gas atmosphere at a temperature higher than the softening point of the inorganic oxide particles.
[0018] (4) A method for manufacturing an electronic component, comprising the following steps: a first coating step of coating a first paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate; a first sintering step of heating at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper; a softening step of heating at a temperature higher than the softening point of the inorganic oxide particles in an inert gas atmosphere; a second coating step of coating a second paste containing copper particles and the oxide particles and not containing an inorganic oxide component having a softening point, or containing copper particles and oxide particles containing copper and / or nickel and having an inorganic oxide component having a softening point in an amount of less than 0.1% by mass; and a second sintering step of heating at a temperature higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper.
[0019] (5) The method for producing an electronic component according to any one of (1) to (4), wherein the inorganic oxide particles have a softening point of 550° C. or higher and 750° C. or lower.
[0020] (6) The method for manufacturing an electronic component according to any one of (1) to (5), wherein the inorganic oxide particles contain three or more metal elements selected from the group consisting of B, Al, Si, Zn, Ba, Bi, Ca, Mg, Sr, Hf, K, Zr, Ti and Na.
[0021] (7) An electronic component comprising: a bonding electrode portion containing an inorganic oxide in gaps in a porous body containing copper; and an inorganic substrate, wherein the content of the inorganic oxide in the half of the bonding electrode portion that is in contact with the inorganic substrate is greater than the content of the inorganic oxide in the remaining half.
[0022] (8) An electronic component comprising: an electrode portion comprising copper; a bonding electrode portion comprising an inorganic oxide in gaps in a porous body comprising copper; and an inorganic substrate, wherein the content of the inorganic oxide in the half of the bonding electrode portion that is in contact with the inorganic substrate is greater than the content of the inorganic oxide in the remaining half.
[0023] (9) An electronic component according to (7) or (8), wherein the inorganic oxide contains three or more metal elements selected from the group consisting of B, Al, Si, Zn, Ba, Bi, Ca, Mg, Sr, Hf, K, Zr, Ti and Na.
[0024] Effects of the Invention
[0025] According to the present invention, an electronic component can be obtained in which a copper electrode and an inorganic substrate have strong adhesion. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic cross-sectional view of the electronic component according to the first embodiment.
[0027] Figure 2 It is a schematic cross-sectional view of an electronic component according to a second embodiment. DETAILED DESCRIPTION
[0028] Hereinafter, specific embodiments of the present invention will be described in detail. The present invention is not limited to the following embodiments at all, and can be implemented with appropriate changes within the scope of the purpose of the present invention.
[0029] <Manufacturing method of the first aspect>
[0030] The manufacturing method of the first embodiment includes the following steps: a coating step, coating a paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate; a sintering step, heating at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper; and a softening step, heating at a temperature higher than the softening point of the inorganic oxide particles in an inert gas atmosphere.
[0031] It should be noted that, in this specification, "copper electrode" refers to an electrode containing copper as a main component (60% by mass or more), and does not exclude the inclusion of other metals and the like as long as it functions as an electrode.
[0032] 〔Coating process〕
[0033] The coating step is a step of coating a paste containing copper particles, copper oxide particles and / or nickel oxide particles, and inorganic oxide particles having a softening point on an inorganic substrate.
[0034] In addition, the presence or absence and temperature of the "softening point" can be determined using DTA.
[0035] [Inorganic substrate]
[0036] The inorganic substrate is, for example, a semiconductor substrate and has an oxide at least on its surface. By having an oxide on the surface of the inorganic substrate, the inorganic oxide particles are softened in the softening step described later, and the inorganic substrate reacts with the components derived from the inorganic oxide particles (referring to the components in which the inorganic oxide particles are softened and filled in the pores of the porous copper sintered body). The components derived from the inorganic oxide particles are contained in the voids of the porous body (electrode) generated by sintering the copper particles and the copper oxide particles and / or the nickel oxide particles, and therefore, by reacting with the inorganic substrate as described above, the adhesion between the inorganic substrate and the electrode as a porous body can be improved.
[0037] The oxide present on the surface of the inorganic substrate 13 is not particularly limited, and examples thereof include insulators such as aluminum oxide and silicon dioxide, and ferroelectrics such as lithium niobium oxide and titanium barium oxide.
[0038] The substrate 13 other than the surface may be made of an insulating material, and examples thereof include silicon nitride, aluminum nitride, and silicon carbide.
[0039] [Paste]
[0040] The paste contains at least copper particles, copper oxide particles and / or nickel oxide particles, and inorganic oxide particles having a softening point. The copper particles, copper oxide particles and / or nickel oxide particles become porous bodies of conductive metals by sintering and function as electrodes of the obtained electronic component.
[0041] An example of such a paste includes copper particles, copper oxide particles and / or nickel oxide particles, a binder resin, and a solvent. In addition, an organic component mainly composed of a binder resin and a solvent is hereinafter referred to as an "organic vehicle".
[0042] (Copper particles)
[0043] The copper particles are not particularly limited, and are preferably particles produced by, for example, a gas atomization method, a water atomization method, or a liquid phase reduction precipitation method, and have a 50% particle size of 70 nm or more and 10 μm or less.
[0044] The particle size of the copper particles is not particularly limited, and is preferably, for example, 0.3 μm or more, more preferably 0.5 μm or more. By making the average particle size of the copper particles 0.3 μm or more, gaps can be formed between the copper particles after sintering. If it is less than 0.3 μm, the gaps between the copper particles sintered densely in the sintering process become smaller, and in the subsequent softening process, the inorganic oxide does not reach the interface and the adhesion is poor. If it is 0.5 μm or more, the adhesion strength is further increased. It should be noted that the average particle size of the copper particles is a value measured using a laser diffraction particle size distribution meter such as Microtrac.
[0045] (Copper oxide particles and / or nickel oxide particles)
[0046] The copper oxide particles contain at least one of cuprous oxide and cupric oxide. In addition, the nickel oxide particles contain nickel oxide. These oxide particles are easily reduced to become conductive metals because the standard free energy of oxide formation is small.
[0047] As described above, the paste contains a resin as a binder. Here, if the binder remains in the electrode after sintering, the conductivity of the electrode may be reduced. Therefore, such a binder needs to be removed. However, in the manufacturing method of the present embodiment, heating needs to be performed under an inert atmosphere. Therefore, oxygen supply is required outside the gas atmosphere. Here, if copper oxide particles and nickel oxide particles are added to the paste and the paste is sintered, even in an inert gas atmosphere, oxygen can be supplied from the oxide particles to the resin by heating and the resin can be decomposed and removed. As a result, a good sintered body of copper particles can be obtained.
[0048] The content of copper oxide particles and / or nickel oxide particles in the paste (the total of two metal oxide particles) is not particularly limited, for example, preferably 0.1% by mass or more relative to the mass of copper particles, more preferably 0.2% by mass or more, and more preferably 0.5% by mass or more. By making the content of copper oxide particles and / or nickel oxide particles 0.1% by mass or more, the amount of oxygen supplied to the resin can be sufficient to further promote the decomposition of the resin. On the other hand, as the content of copper oxide particles and / or nickel oxide particles, it is preferably 10% by mass or less, more preferably 9% by mass or less, more preferably 8% by mass or less, and particularly preferably 7% by mass or less. By making the content of copper oxide particles and / or nickel oxide particles 10% by mass or less, the copper oxide particles and / or nickel oxide particles can be completely reduced, and the resistance of the porous body (electrode) can be further reduced. It should be noted that when weighing the required amount of oxide particles, the resin content in the paste is a trace amount, so the oxide particles can be weighed based on the mass of the copper particles as the main component in the paste, and the appropriate amount of oxide particles can be contained with high precision.
[0049] The average particle size of the copper oxide particles and / or nickel oxide particles is not particularly limited, and may be, for example, a 50% average particle size (D 50 ) is preferably 0.1 μm or more, more preferably 0.2 μm or more, and further preferably 0.3 μm or more. By making the average particle size of the copper oxide particles and / or nickel oxide particles be 0.1 μm or more, it is possible to prevent the copper oxide particles and / or nickel oxide particles from aggregating with each other, which helps to decompose more copper oxide particles and / or nickel oxide particles. In addition, the average particle size of the copper oxide particles and / or nickel oxide particles is preferably 10 μm or less, more preferably 9 μm or less, further preferably 8 μm or less, and particularly preferably 7 μm or less. By making the average particle size of the copper oxide particles and / or nickel oxide particles be 10 μm or less, the printability of the copper paste can be further improved.
[0050] (Inorganic oxide particles)
[0051] The inorganic oxide particles are particles having a softening point. By making the inorganic oxide have a softening point, the inorganic oxide can be softened in a softening step described later and can move from the inside of the porous sintered body to the vicinity of the inorganic substrate through the pores.
[0052] The inorganic oxide particles preferably contain three or more metal elements selected from the group consisting of B, Al, Si, Zn, Ba, Bi, Ca, Mg, Sr, Hf, K, Zr, Ti and Na. By containing oxides of multiple metal elements, a softening point is easily generated.
[0053] The softening point of the inorganic oxide particles is not particularly limited, and is preferably 550°C or more, more preferably 570°C or more, more preferably 590°C or more, and particularly preferably 600°C or more. By setting it to 550°C or more, a difference with the sintering temperature of the copper particles is formed, and softening can be suppressed in the sintering process. On the other hand, as a softening point, it is preferably 750°C or less, more preferably 740°C or less, further preferably 720°C or less, and particularly preferably 700°C or less. By setting it to 750°C or less, it is possible to prevent the components derived from the inorganic oxide particles from reacting with the inorganic substrate to release gas and form bubble-like voids on the interface, thereby further improving the adhesion strength between the porous copper body generated by the sintering of the copper particles and the inorganic substrate.
[0054] The content of the inorganic oxide particles in the paste is not particularly limited, for example, preferably 0.4% by mass or more relative to the mass of the copper particles, more preferably 1.0% by mass or more. By making the content of the inorganic oxide particles 0.4% by mass or more, the amount of inorganic oxide that moves to the interface with the inorganic substrate in the softening process can be increased, ensuring the adhesion strength with the inorganic substrate. In addition, by making the content of the inorganic oxide particles 1.0% by mass or more, the adhesion strength can be further improved. On the other hand, as the content of the inorganic oxide particles, it is preferably 20% by mass or less, more preferably 10% by weight or less, further preferably 4.8% by mass or less, and particularly preferably 4% by mass or less. By making the content of the inorganic oxide particles 20% by mass or less, the adhesion strength can be ensured. In addition, in particular, by making the content of the inorganic oxide particles 4.8% by mass or less, the resistance can be reduced while maintaining the adhesion strength.
[0055] The average particle size of the inorganic oxide particles is not particularly limited, and is, for example, a 50% particle size (D 50 ) is preferably 0.5 μm or more, more preferably 0.7 μm or more, further preferably 1 μm or more, and particularly preferably 1.5 μm or more. By making the average particle size of the inorganic oxide particles be 0.5 μm or more, it is possible to prevent the particles from aggregating to improve the printability of the paste. In addition, it is possible to prevent the formation of spherical voids in the sintered body to improve the mechanical strength of the electronic component. On the other hand, the average particle size of the inorganic oxide particles is preferably 10 μm or less, more preferably 8 μm or less, further preferably 7 μm or less, and particularly preferably 5 μm or less. By making the average particle size of the inorganic oxide particles be 7 μm or less, it is possible to uniformly and sufficiently apply heat to the glass, and it is possible to suppress the inorganic oxide particles that do not soften in the softening step described later. Moreover, the adhesion strength between the inorganic substrate and the porous body generated by sintering of copper can be improved thereby.
[0056] (Binder resin)
[0057] The content of the binder resin in the organic vehicle is preferably 0.05% by mass or more and 17% by mass or less in mass %. The binder resin is not particularly limited, and may be a resin decomposed by heating, for example, cellulose resins such as methyl cellulose, ethyl cellulose, and carboxymethyl cellulose, acrylic resins, butyral resins, alkyd resins, epoxy resins, phenolic resins, etc. Among them, it is preferred to use a cellulose resin that has a tendency to easily disappear from the paste by reacting with oxygen and carbon monoxide, and among the cellulose resins, ethyl cellulose is more preferably used.
[0058] By heating together with the conductive metal oxide in an inert atmosphere, the binder resin reacts with the conductive metal oxide, and the amount of resin remaining in the wiring after sintering can be minimized, thereby suppressing the increase in wiring resistance caused by the resin residue. However, even so, there is still the possibility that the binder resin component remains in the wiring, the sintering property deteriorates, and the wiring resistance increases. Therefore, by making the content of the binder resin in the organic vehicle less than 17.0% by mass, the effect of the binder resin component remaining in the wiring after sintering on the wiring resistance can be ignored. On the other hand, if the content of the binder resin in the organic vehicle is less than 0.05% by mass, there is the possibility that the viscosity of the paste decreases and the printability deteriorates.
[0059] (Solvent)
[0060] The solvent contained in the conductive paste is not particularly limited, and may have a suitable boiling point, vapor pressure, and viscosity, and examples thereof include hydrocarbon solvents, chlorinated hydrocarbon solvents, cyclic ether solvents, amide solvents, sulfoxide solvents, ketone solvents, alcohol compounds, polyol ester solvents, polyol ether solvents, terpene solvents, and mixtures thereof. Among them, TEXANOL, butyl carbitol, butyl carbitol acetate, and terpineol having a boiling point of approximately 200° C. are preferably used.
[0061] (Ingredients in other organic carriers)
[0062] Organic carrier is a liquid formed by mixing binder resin, solvent and other organic substances added as required. In the case of sintering in the atmosphere of the present invention, an organic carrier prepared by mixing binder resin with solvent can be used, and metal salt and polyol can be mixed and used as required. As an example of metal salt, when Cu is used as the first metal element, copper acetate (II), copper benzoate (II), bis (acetylacetone) copper (II) etc. can be cited. In addition, as polyol, ethylene glycol, diethylene glycol, trimethylene glycol, propylene glycol, tetraethylene glycol can be cited. By adding the above substances, polyols reduce metal salts during sintering, and the metal after reduction is precipitated into the gap between particles, so there is an effect of improving the conductivity between particles.
[0063] The content of the organic vehicle contained in the paste is not particularly limited, but is, for example, preferably 3% by mass or more and 19% by mass or less, and more preferably 8% by mass or more and 15% by mass or less.
[0064] By making the content of the organic vehicle contained in the paste 3 mass % or more and 19 mass % or less, the wiring shape can be well maintained. If the content of the organic vehicle exceeds 19 mass %, the viscosity of the paste is weakened, so there is a possibility that the wiring shape after printing may sag. On the other hand, if the content of the organic vehicle is less than 3 mass %, the viscosity of the paste is too high, so there is a possibility that a wiring with a uniform shape cannot be formed.
[0065] [Method for producing paste]
[0066] The paste can be prepared by mixing the binder resin and a solvent, further adding copper particles, copper oxide particles and / or nickel oxide particles, and kneading them using a planetary mixer, etc. In addition, a three-roll mill can be used to improve the dispersibility of these particles as needed.
[0067] The method for applying the paste is not particularly limited, and for example, an inkjet method, a dispenser method, a screen printing method, or the like can be used.
[0068] In addition, the inorganic substrate after the paste is applied is preferably dried at room temperature or high temperature as appropriate to remove a predetermined amount of the solvent.
[0069] 〔Sintering process〕
[0070] The sintering step is a step of heating the inorganic substrate coated with the paste prepared in the coating step at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper.
[0071] When the paste is sintered in this way, the copper particles and the copper oxide particles and / or the nickel oxide are sintered, and the surfaces of these particles are connected to form a porous body. That is, the porous body thus obtained is formed of copper (when nickel oxide is not used) or formed of copper and nickel (when nickel oxide is used) (hereinafter, for convenience, the case where nickel is also included is referred to as a "copper porous body".). It should be noted that at this time, oxygen is supplied from the copper oxide particles and / or the nickel oxide to the resin existing from the paste by heating, so that the resin is decomposed. On the other hand, since the heating is performed at a temperature below the softening point, the inorganic oxide particles do not change at this time.
[0072] The heating temperature in the sintering step is not particularly limited, and may be lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles, and is, for example, preferably 400° C. or higher, more preferably 450° C. or higher, further preferably 470° C. or higher, and particularly preferably 500° C. or higher. On the other hand, the heating temperature is preferably lower than 750° C., more preferably 700° C. or lower, further preferably 650° C. or lower, and particularly preferably 620° C. or lower.
[0073] In addition, the heating temperature in the sintering step is not particularly limited, but is preferably 30° C. or more lower than the softening point of the inorganic oxide particles, more preferably 50° C. or more lower, further preferably 70° C. or more lower, and particularly preferably 100° C. or more lower. By setting the heating temperature to be 30° C. or more lower than the softening point of the inorganic oxide particles, it is possible to more reliably prevent the softening of the inorganic oxide particles during the sintering step.
[0074] The heating time in the sintering process is not particularly limited, and is preferably, for example, more than 5 minutes, more preferably more than 15 minutes. In addition, the heating time is preferably less than 60 minutes, more preferably less than 45 minutes. By making the heating time in the above range, the copper particles can be fully sintered.
[0075] As the inert atmosphere, any atmosphere substantially free of oxidizing gas and reducing gas may be used, for example, nitrogen atmosphere, helium atmosphere, argon atmosphere, etc. Among them, nitrogen atmosphere is preferred from the viewpoint of cost. It should be noted that, although it is an inert atmosphere, since the device used for implementation has limitations in excluding oxidizing gas and reducing gas, for example, it is allowed to contain oxidizing gas and reducing gas below 100 ppm respectively.
[0076] It should be noted that, for the inorganic oxide particles, inorganic oxide particles of one composition can be used alone or inorganic oxide particles of multiple compositions can be mixed and used. When multiple inorganic oxides are used, the so-called "lower than the softening point of the inorganic oxide particles" is based on the material with the lowest softening point among the multiple inorganic oxides.
[0077] 〔Softening process〕
[0078] The softening step is a step of heating at a temperature not lower than the softening point of the inorganic oxide particles in an inert gas atmosphere.
[0079] When heated in this way, the inorganic oxide particles are softened and move to the vicinity of the inorganic substrate through the pores of the copper porous body. Furthermore, components derived from the inorganic oxide particles react with the inorganic substrate to integrate, thereby improving the adhesion strength between the copper porous body and the inorganic substrate.
[0080] As the inert atmosphere, similar to the above-mentioned sintering step, it is sufficient to be an atmosphere that does not substantially contain oxidizing gas and reducing gas, and for example, nitrogen atmosphere, helium atmosphere, argon atmosphere, etc. can be used. Among them, from the perspective of cost, nitrogen atmosphere is preferred. It should be noted that although it is an inert atmosphere, since the device used for implementation has limitations in excluding oxidizing gas and reducing gas, it is impossible to exclude, for example, oxidizing gas and reducing gas that contain less than 100 ppm respectively.
[0081] The heating temperature in the softening process is not particularly limited, and it can be a temperature above the softening point of the inorganic oxide particles, for example, preferably above 600°C, more preferably above 620°C, and further preferably above 650°C. By setting the heating temperature to above 600°C, the inorganic substrate and the components derived from the inorganic oxide particles can be integrated, and the adhesion between the inorganic substrate and the copper sintered body can be further improved. In addition, as the heating temperature, it is preferably below 900°C, more preferably below 870°C, and further preferably below 850°C. By setting the heating temperature to below 900°C, the generation of bubbles due to the evaporation of the metal component and the decrease in the adhesion between the inorganic substrate and the copper sintered body can be suppressed.
[0082] The heating temperature in the softening step is preferably 30° C. or higher than the softening point of the inorganic oxide particles, more preferably 50° C. or higher, and even more preferably 70° C. or higher. By setting the heating temperature 30° C. or higher than the softening point of the inorganic oxide particles, the inorganic oxide particles can be easily softened.
[0083] The heating time in the softening process is not particularly limited, and is preferably, for example, more than 5 minutes, more preferably more than 15 minutes. In addition, as the heating time, it is preferably less than 60 minutes, more preferably less than 45 minutes. By making the heating time be in the above range, the inorganic oxide particles after softening can be fully moved to the vicinity of the inorganic substrate.
[0084] It should be noted that, regarding the inorganic oxide particles, one or more inorganic oxides may be used, or when multiple inorganic oxides are used, the term "above the softening point of the inorganic oxide particles" refers to the one having the highest softening point among the multiple inorganic oxides.
[0085] <Production method of the second aspect>
[0086] The manufacturing method of the second embodiment includes the following steps: a first coating step, coating a first paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate; a second coating step, coating a second paste, wherein the second paste contains copper particles and oxide particles containing copper and / or nickel and does not contain an inorganic oxide component having a softening point, or contains copper particles and oxide particles containing copper and / or nickel and the content of the inorganic oxide component having a softening point is less than 0.1% by mass; a sintering step, heating at a temperature lower than the softening point of the inorganic oxide particles and above the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper; and a softening step, heating at a temperature above the softening point of the inorganic oxide particles in an inert gas atmosphere.
[0087] That is, the production method of the second aspect includes a second coating step, as compared with the production method of the first aspect.
[0088] [First coating step]
[0089] The first coating step is a step of coating a first paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate. The first coating step is the same as the coating step in the manufacturing method of the first embodiment, so a detailed description is omitted here. It should be noted that in this case, the "paste" in the manufacturing method of the first embodiment is replaced by the "first paste".
[0090] [Second coating step]
[0091] In the second coating step, a second paste is coated, the second paste containing copper particles and oxide particles containing copper and / or nickel and not containing an inorganic oxide component having a softening point, or containing copper particles and oxide particles containing copper and / or nickel and having an inorganic oxide component having a softening point in an amount of less than 0.1% by mass. The second coating step is different from the coating step in the manufacturing method of the first embodiment only in that the second paste (corresponding to the "paste" in the manufacturing method of the first embodiment) does not contain an inorganic oxide component having a softening point, or the content of the inorganic oxide component is less than 0.1% by mass relative to the second paste, and therefore detailed descriptions other than the second paste are omitted here.
[0092] The electrode portion (copper electrode) formed by the second paste is arranged for the purpose of electrically connecting a plurality of wirings to be electrically connected. Therefore, the higher the conductivity, the better. As the second paste, a paste containing no inorganic oxide component having a softening point or containing an inorganic oxide component having a softening point in an amount of less than 0.1% by mass (only a small amount) is used.
[0093] The concept of "inorganic oxide components" that are not contained in the second paste or whose content is less than 0.1% by mass relative to the second paste includes all inorganic oxide particles having a softening point, and is not limited to the components constituting the "inorganic oxide particles having a softening point" used in the first coating step. It should be noted that oxide particles containing copper and / or nickel do not have a softening point and are therefore excluded from the inorganic oxide components.
[0094] 〔Sintering process〕
[0095] The sintering step is a step of heating the inorganic oxide particles at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper. This sintering step is the same as the sintering step in the manufacturing method of the first embodiment, so a detailed description is omitted here.
[0096] 〔Softening process〕
[0097] The softening step is a step of heating the inorganic oxide particles at a temperature higher than the softening point in an inert gas atmosphere. This softening step is the same as the softening step in the production method of the first embodiment, and therefore detailed description thereof is omitted here.
[0098] As described above, the manufacturing method of the second embodiment further includes a second coating step in addition to the manufacturing method of the first embodiment. In addition, in the second step, when a paste containing copper particles and copper and / or nickel oxide particles and containing no or only a small amount of an inorganic oxide component having a softening point is applied, a copper skeleton containing no inorganic oxide component having a softening point is formed. This portion can further improve the conductivity of the electronic component to be formed.
[0099] <Third aspect of the manufacturing method>
[0100] The same electronic component as the manufacturing method of the second embodiment, that is, an electronic component having a copper skeleton that does not contain an inorganic oxide component having a softening point, can also be manufactured using the following method. Specifically, the manufacturing method of the third embodiment includes the following steps: a first coating step, coating a first paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point on an inorganic substrate; a first sintering step, heating at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper; a softening step, heating at a temperature higher than the softening point of the inorganic oxide particles in an inert gas atmosphere; a second coating step, coating a second paste, the second paste containing copper particles and oxide particles and not containing an inorganic oxide component having a softening point, or containing copper particles and oxide particles containing copper and / or nickel and having an inorganic oxide component having a softening point of less than 0.1% by mass; and a second sintering step, heating at a temperature higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper.
[0101] That is, in the manufacturing method of the third embodiment, the first paste is applied and then sintered, and then the second paste is applied and then sintered, and the pastes are sintered twice in this manufacturing method. In contrast, the manufacturing method of the second embodiment described above does not sinter after applying the first paste, but applies the second paste and simultaneously sinters the first and second pastes.
[0102] [First coating step]
[0103] In the first coating step, a first paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point is coated on an inorganic substrate. This first coating step is the same as the first coating step in the manufacturing method of the second embodiment, so detailed description is omitted here.
[0104] [First sintering step]
[0105] In the first sintering step, the inorganic oxide particles are heated at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper. The first sintering step is the same as the sintering step in the manufacturing method of the first embodiment, so a detailed description is omitted here.
[0106] [Second coating step]
[0107] In the second coating step, a first paste containing copper particles, copper oxide particles and / or nickel oxide particles and inorganic oxide particles having a softening point is coated on the substrate. The first coating step is the same as the second coating step in the manufacturing method of the second embodiment, so detailed description is omitted here.
[0108] 〔Softening process〕
[0109] The softening step is a step of heating the inorganic oxide particles at a temperature higher than the softening point in an inert gas atmosphere. This softening step is the same as the softening step in the production method of the first embodiment, and therefore detailed description thereof is omitted here.
[0110] [Second sintering step]
[0111] In the second sintering step, heating is performed at a temperature higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper. The second sintering step is the same as the sintering step in the first embodiment except for the heating temperature.
[0112] The heating temperature in the second sintering step is not particularly limited, and it can be a temperature above the sintering temperature of the copper particles. In addition, it is not necessary to be a temperature lower than the softening point of the inorganic oxide particles as in the first sintering step. However, the heating temperature in the second heating and sintering step can be the same as the sintering step in the manufacturing method of the first embodiment, for example, preferably 400°C or more, more preferably 450°C or more, more preferably 470°C or more, and particularly preferably 500°C or more. In addition, as a heating temperature, it is preferably 700°C or less, more preferably 670°C or less, more preferably 650°C or less, and particularly preferably 620°C or less.
[0113] <Electronic component according to the first aspect>
[0114] Features of an electronic component produced using the production method of the first embodiment (hereinafter referred to as “the electronic component of the first embodiment”) will be described. Figure 1 1 is a schematic cross-sectional view of an electronic component of the first embodiment. The electronic component 1 of the first embodiment includes an inorganic substrate 13 and a bonding electrode portion 12 containing an inorganic oxide in a gap of a porous body containing copper. In such an electronic component 1, the bonding electrode portion 12 is stacked with the organic substrate 13. In addition, in the bonding electrode portion 12, the content of the inorganic oxide in the half on the side in contact with the inorganic substrate 13 is greater than the content of the inorganic oxide in the other half.
[0115] 〔Jointing electrode part〕
[0116] The bonding electrode portion 12 contains an inorganic oxide in the gaps of the porous body containing copper. In addition, in the bonding electrode portion 12, the content of the inorganic oxide in the half of the side in contact with the inorganic substrate 13 described later is greater than the content of the inorganic oxide in the half of the side in contact with the electrode portion. It should be noted that "bonding" here means being connected to and attached to the inorganic substrate, and does not require, for example, a bonding strength above a specific value.
[0117] The porous body is a skeleton body containing at least copper. The porous body can contain nickel as another element. That is, the porous body is composed of copper or copper and nickel. It should be noted that "composed of copper" or "composed of copper and nickel" also includes substances containing impurities of up to about 5% by mass or oxygen bonded by oxidation. In addition, the porous body can also be a sintered body composed of, for example, particle-shaped metal surfaces connected to each other.
[0118] The elements constituting the inorganic oxide are not particularly limited, and preferably contain three or more metal elements selected from the group consisting of B, Al, Si, Zn, Ba, Bi, Ca, Mg, Sr, Hf, K, Zr, Ti and Na. These elements form oxides respectively, and by forming oxides containing three or more metal elements among them, the softening point can be adjusted to a range of 550° C. to 750° C., thereby improving the adhesion strength.
[0119] The metal element constituting the inorganic oxide preferably reacts with the inorganic substrate 13 described later as an oxide to form an integral body. By thus integrating the metal element constituting the inorganic oxide with the inorganic substrate 13, the adhesion strength between the bonding electrode portion 12 and the inorganic substrate 13 can be improved.
[0120] The content of inorganic oxide is not particularly limited. Preferably, the content of inorganic oxide particles contained in the electronic component 1 is 10% or less in terms of area occupancy relative to the total cross-sectional area of the electrode, and more preferably 5% or less. By forming it to be less than 10%, the mechanical reliability of the electrode can be improved and the resistivity of the electrode can be reduced. In addition, by forming it to be less than 5%, the resistivity is further reduced. Here, the area occupancy of the inorganic oxide can be obtained as follows: prepare a sample cut and ground at the midpoint of the length direction of the electrode perpendicular to the length direction of the electrode, observe the cross section using a scanning electron microscope and obtain a composition distribution map using an X-ray spectrometer, set the area of the entire electrode cross section as the total cross-sectional area of the electrode, and measure the area of the portion where the inorganic oxide exists relative to the total cross-sectional area.
[0121] The thickness of the bonding electrode portion 12 is not particularly limited, but is preferably 10 μm or more, for example. The thickness of the bonding electrode portion 12 is 10 μm or more, which is much larger than the D 50Therefore, the surface irregularities caused by the shape of the copper particles are relatively small compared to the electrode thickness, and wiring with a good shape can be obtained.
[0122] 〔Inorganic substrate〕
[0123] The substrate 13 is a substrate containing oxide at least on the surface. It should be noted that, here, "surface" refers to the entire surface at least on the side in contact with the bonding electrode portion 12. As for the details, the same substrate as above can be used, so the description is omitted here.
[0124] <Electronic component according to the second aspect>
[0125] Features of electronic components produced using the manufacturing methods of the second and third aspects (hereinafter collectively referred to as “electronic components of the second aspect”) will be described. Figure 2 2 is a schematic cross-sectional view of an electronic component of the second embodiment. The electronic component 2 of the second embodiment comprises an inorganic substrate 23, an electrode portion 21 comprising copper, and a bonding electrode portion 22 comprising an inorganic oxide in gaps in a porous body comprising copper, wherein the content of the inorganic oxide in the half of the bonding electrode portion 22 on the side in contact with the inorganic substrate 23 is greater than the content of the inorganic oxide in the other half (the side in contact with the electrode portion 21).
[0126] That is, the electronic component of the second embodiment has a structure in which an electrode portion is further provided on the bonding electrode portion 12 of the electronic component of the first embodiment. Therefore, the bonding electrode portion 22 in the electronic component of the second embodiment is the same as the bonding electrode 12 in the electronic component of the first embodiment described above. In addition, the inorganic substrate 23 in the electronic component of the second embodiment is the same as the inorganic substrate 13 in the electronic component of the first embodiment. Therefore, the description of the bonding electrode portion 22 and the inorganic substrate 23 is omitted here.
[0127] 〔Electrode section〕
[0128] The electrode portion 21 is a member that electrically connects a plurality of wirings electrically connected to the electrode portion 21 .
[0129] The electrode portion 21 contains at least copper and may contain nickel as another element. That is, the electrode portion 21 is made of copper or copper and nickel.
[0130] The electrode portion 21 may also be a porous body (skeleton) having a porous structure. In addition, the porous body may also be a sintered body formed by interconnecting the surfaces of, for example, metal particles. By making the electrode portion 21 have a porous structure in this way, a certain degree of stress applied to the electronic component 2 can be absorbed, and the overall resistance of the electronic component 2 to peeling can be further improved.
[0131] When the electrode portion 21 has a porous structure, the volume percentage of the voids is not particularly limited, and is preferably, for example, 2% by volume or more, more preferably 5% by volume or more, and further preferably 10% by volume or more. In addition, the volume percentage of the voids is preferably 40% by volume or less, and more preferably 35% or less.
[0132] It is preferred that the electrode portion 21 does not contain inorganic oxides other than copper and nickel oxides. If the electrode portion 21 contains inorganic oxide particles, the conductivity decreases. It should be noted that the electrode portion 21 contains at least copper as a metal and may also contain nickel, but the copper and nickel may also be oxidized in the atmosphere in a metallic state. Therefore, the oxides of copper and nickel are allowed to be within a range that can ensure conductivity (for example, less than 5% by mass).
[0133] The thickness of the electrode portion 21 is not particularly limited, but is preferably thicker than the thickness of the bonding electrode portion 12 described later. By making the thickness of the electrode portion 21 thicker than the thickness of the bonding electrode portion 22, stress relaxation caused by the electrode portion 21 having a porous structure becomes significant, and the overall adhesion strength of the electronic component can be improved.
[0134] The electronic component described above can be used for, for example, a high-current substrate for a power module, an insulating heat dissipation substrate for an LED, and the like.
[0135] Example
[0136] The present invention is further described in detail with reference to the following examples, but the present invention is not limited to these examples.
[0137] 100 mass% D 50 The copper particles are spherical in shape of 1.0 μm and 2% by mass of D 50 The Cu2O particles are 0.3 μm and the specified amount of D 50Inorganic oxide particles with a softening point of 3 μm are mixed with a carrier to prepare a copper paste. The copper paste is printed on an alumina substrate to a thickness of about 150 μm using a screen printing method, and an electrode is made by a sintering process and a softening process in a nitrogen atmosphere after an atmospheric drying process at 110°C for 10 minutes. Using the prepared sample, a tensile fixture is joined to the upper surface of the electrode using a solder alloy, the fixture is stretched, and the peel strength between the electrode and the substrate is measured. In addition, the resistivity is measured using a DC four-probe method. Table 1 shows the elements contained in the inorganic oxide particles (excluding oxygen), the amount of inorganic oxide particles added (mass %), the softening point of the inorganic oxide particles (°C), the heating temperature of the sintering process (°C), the heating temperature of the softening process (°C), the peel strength (MPa) and the resistivity (μΩ·cm) of the prepared electrode. It should be noted that the heating time of the sintering process is 10 minutes, and the heating time of the softening process is 30 minutes. In addition, due to the relationship between the softening point and the heating temperature in the softening step, there are samples that are not actually softened, and for convenience, it is referred to as a "softening step."
[0138] [Table 1]
[0139]
[0140] Description of Reference Numerals
[0141] 1.2 Electronic components
[0142] 12, 22 Bonding electrode part
[0143] 13.23 Inorganic substrate
[0144] 21 Electrode
Claims
1. A method for manufacturing an electronic component, comprising the following steps: A coating step of coating a paste containing copper particles, copper oxide particles and / or nickel oxide particles, and inorganic oxide particles having a softening point on an inorganic substrate; A sintering step of heating the inorganic oxide particles at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper, in, The temperature is a temperature between 400°C and 620°C; and Next, a softening step of heating the inorganic oxide particles at a temperature not lower than the softening point of the inorganic oxide particles is performed in an inert gas atmosphere, wherein the temperature is not lower than 650° C. and not higher than 870° C.
2. The method for manufacturing an electronic component according to claim 1, in, The content of the copper oxide particles and / or nickel oxide particles in the paste is 0.1% by mass or more and 10% by mass or less relative to the copper particles.
3. A method for manufacturing an electronic component, comprising the following steps: A first coating step of coating a first paste containing copper particles, copper oxide particles and / or nickel oxide particles, and inorganic oxide particles having a softening point on an inorganic substrate; a second coating step of applying a second paste, in, The second paste contains copper particles and oxide particles containing copper and / or nickel and does not contain an inorganic oxide component having a softening point, or the second paste contains copper particles and oxide particles containing copper and / or nickel and the content of the inorganic oxide component having a softening point is 0.1 wt % or less; A sintering step of heating the inorganic oxide particles at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper, wherein the temperature is 400° C. to 620° C.; and Next, a softening step of heating the inorganic oxide particles at a temperature not lower than the softening point of the inorganic oxide particles is performed in an inert gas atmosphere, wherein the temperature is not lower than 650° C. and not higher than 870° C.
4. A method for manufacturing an electronic component, comprising the following steps: A first coating step of coating a first paste containing copper particles, copper oxide particles and / or nickel oxide particles, and inorganic oxide particles having a softening point on an inorganic substrate; A first sintering step of heating the inorganic oxide particles at a temperature lower than the softening point of the inorganic oxide particles and higher than the sintering temperature of the copper particles in an inert gas atmosphere to form a sintered body containing at least copper, in, The temperature is a temperature between 400°C and 620°C; Next, a softening step of heating the inorganic oxide particles at a temperature above the softening point of the inorganic oxide particles is performed under an inert gas atmosphere, wherein the temperature is 650° C. to 870° C.; a second coating step of coating a second paste, wherein the second paste contains copper particles and oxide particles containing copper and / or nickel and does not contain an inorganic oxide component having a softening point, or the second paste contains copper particles and oxide particles containing copper and / or nickel and the content of the inorganic oxide component having a softening point is less than 0.1% by mass; and A second sintering step is performed in an inert gas atmosphere, wherein heating is performed at a temperature equal to or higher than a sintering temperature of the copper particles to form a sintered body containing at least copper.
5. The method for producing an electronic component according to any one of claims 1 to 4, in, The inorganic oxide particles have a softening point of 550° C. or higher and 750° C. or lower.
6. The method for producing an electronic component according to any one of claims 1 to 4, in, The inorganic oxide particles contain three or more metal elements selected from the group consisting of B, Al, Si, Zn, Ba, Bi, Ca, Mg, Sr, Hf, K, Zr, Ti and Na.
7. Electronic components having: a bonding electrode portion including an inorganic oxide in gaps in a porous body including copper; and Inorganic substrates, The content of the inorganic oxide in the half of the bonding electrode portion that is in contact with the inorganic substrate is greater than the content of the inorganic oxide in the remaining half. The porous body is connected to and attached to the inorganic substrate.
8. Electronic components having: an electrode portion including copper; a bonding electrode portion including an inorganic oxide in gaps in a porous body including copper; and Inorganic substrates, The content of the inorganic oxide in the half of the bonding electrode portion that is in contact with the inorganic substrate is greater than the content of the inorganic oxide in the remaining half. The porous body is connected to and attached to the inorganic substrate.
9. The electronic component according to claim 7 or 8, in, The inorganic oxide contains three or more metal elements selected from the group consisting of B, Al, Si, Zn, Ba, Bi, Ca, Mg, Sr, Hf, K, Zr, Ti and Na.
Citation Information
Patent Citations
Element mounting substrate and light-emitting apparatus
JP2011119343A
Electronic component and method for manufacturing same
CN106664805A
Copper conductor paste and substrate printed therewith
JP1998233119A
Copper conductor paste for aluminum nitride board, and aluminum nitride board
JP1998283840A
Circuit board and its manufacturing method
JP2002151810A