Tellurium semiconductor thin film and its preparation method, equipment and application
The preparation of tellurium semiconductor thin films by vapor phase transport deposition solves the problems of complex equipment and poor film uniformity in existing technologies, and realizes simple, low-cost and efficient film preparation, which is suitable for photodetector applications.
Patent Information
- Application Number
- CN202110359561.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-04-02
AI Technical Summary
In existing technologies, thermal evaporation and magnetron sputtering methods involve large equipment size, complex operation, high vacuum requirements, and poor uniformity of the resulting Te films.
Tellurium semiconductor thin films were prepared using vapor transport deposition (VTD). By heating a Te source under conditions of 0.003–25 torr and depositing vapor Te on a substrate, the uniformity and crystallinity of the thin films were optimized by controlling the angle between the substrate and the horizontal direction.
It enables simple and low-cost thin film preparation, producing films with regular morphology and uniform thickness. The vacuum level can be rapidly reached 10⁻¹ Pa, making it suitable for thin film growth under different atmospheres and allowing real-time observation of the film growth process.
Smart Images

Figure HDA0003004962890000011 
Figure HDA0003004962890000012 
Figure HDA0003004962890000013
Abstract
Description
Technical Field
[0001] The present application relates to a tellurium semiconductor film and a preparation method, equipment, and application thereof, and belongs to the technical field of semiconductor thin films. Background Art
[0002] The melting point of tellurium is 450℃, which can be grown at low temperature; the band gap is 0.33eV, and the absorption band edge is 3.75μm, which can be used for infrared detection. The methods reported in the literature for growing tellurium thin films include thermal evaporation and magnetron sputtering.
[0003] However, thermal evaporation and magnetron sputtering methods require large equipment volume, complex operation, and high vacuum degree (10 - 3 Pa, it is necessary to start the molecular pump, and it takes a long time to evacuate the film), and the uniformity of the obtained Te film is poor. Summary of the invention
[0004] According to one aspect of the present application, in order to provide a method for quickly preparing a smooth and flat Te film, the present application provides a method for preparing a tellurium semiconductor film. Compared with thermal evaporation and magnetron sputtering methods, the vapor transport deposition method has the advantages of easy operation, simple equipment, low growth cost, and real-time observation (based on the flip-top design of the VTD device).
[0005] A method for preparing a tellurium semiconductor thin film, the method comprising: subjecting a Te source to vapor phase transport deposition to obtain the tellurium semiconductor thin film.
[0006] Specifically, the Te source includes Te powder.
[0007] Optionally, the preparation method comprises:
[0008] S100, heating a solid-phase Te source placed in a heating zone of a vapor transport deposition tube under a condition of 0.003 to 25 torr to obtain gas-phase Te;
[0009] S200, depositing the gas-phase Te on a substrate located in a non-heating area of a vapor transport deposition tube to obtain the tellurium semiconductor thin film.
[0010] Specifically, gas-phase Te can be obtained under certain pressure (0.003-25 torr) and high temperature (450-470°C).
[0011] During the deposition of gas phase Te on the substrate, the pressure in the tube is maintained in the range of 0.003 to 25 torr by vacuuming, thus ensuring the continuous generation of Te gas phase. That is, vacuuming and deposition are carried out simultaneously.
[0012] The solid-phase Te source includes Te powder.
[0013] The vapor transport deposition tube (VTD tube) is already available in the existing vapor transport deposition equipment (VTD equipment).
[0014] Optionally, the angle between the substrate and the horizontal direction is α, and the value range of α is 0°≤α≤90°.
[0015] Specifically, the horizontal direction in the present application refers to the horizontal direction along the axis of the vapor transport deposition tube. On the one hand, the smaller the angle between the substrate and the horizontal direction, the closer the substrate is to the horizontal, so that one end of the substrate is close to the heating zone and the other end of the substrate is far away from the heating zone. The crystallinity of the grains deposited near the heating zone is higher, and the crystallinity of the grains deposited away from the heating zone is lower, making the overall uniformity of the film poor. On the other hand, the larger the angle between the substrate and the horizontal direction, the closer the substrate is to the vertical. Although this can overcome the influence of temperature difference, it will also affect the uniformity of the film due to the effect of gravity.
[0016] Specifically, in step S100, the upper limit of the pressure is selected from 0.023 torr, 0.23 torr, 0.8 torr, 1.5 torr, 2.3 torr, and 2.5 torr; the lower limit of the pressure is selected from 0.02 torr, 0.023 torr, 0.8 torr, 1.5 torr, 0.23 torr, and 2.3 torr.
[0017] Preferably, the value range of α is 70°≤α≤80°.
[0018] Specifically, when the angle between the substrate and the horizontal direction is 70°≤α≤80°, the uniformity of the thin film is very good.
[0019] Optionally, the substrate is placed on a heat conductor; and the heat conductor is placed in a non-heating area of the vapor transport deposition tube.
[0020] Specifically, in the present application, the heat conductor transfers the heat of the heating zone to the substrate so that the substrate has a certain temperature to form a Te crystalline film. If the substrate has no temperature, an amorphous film will be formed, affecting the quality of the film.
[0021] Optionally, the contact surface between the heat conducting element and the substrate is an inclined surface; the inclination of the inclined surface is 70° to 80°.
[0022] Optionally, the heat conducting member is selected from any one of a graphite block, an aluminum plate, and a ceramic plate.
[0023] Optionally, the substrate is an inert substrate or an active substrate;
[0024] The inert substrate includes any one of a glass substrate, an ITO substrate, and a FTO substrate; the active substrate includes any one of a TiO2 substrate, a CdS substrate, and a ZnO substrate.
[0025] Optionally, the heating conditions are:
[0026] Temperature: 450~470℃;
[0027] Heating rate: 15~25℃ / min.
[0028] Preferably, the heating conditions are:
[0029] Temperature: 450~460℃;
[0030] Heating rate: 15-20℃ / min.
[0031] Preferably, gas-phase Te is obtained under the condition of 0.02 to 0.3 torr.
[0032] Specifically, under lower pressure conditions, the grain deposition rate is slower and the crystallinity is better.
[0033] Optionally, the deposition time is 6 to 10 minutes.
[0034] According to the second aspect of the present application, a tellurium semiconductor thin film is also provided, in which the growth direction of the grains in contact with the substrate is parallel to the substrate; the growth direction of the remaining grains is at an angle to the substrate and / or parallel to the substrate.
[0035] Specifically, the remaining crystal grains refer to the crystal grains in the tellurium semiconductor thin film that are not in contact with the substrate, that is, the crystal grains that are deposited on the substrate crystal grain layer during the growth process.
[0036] Preferably, among the remaining grains, the number of grains whose growth direction forms an angle with the substrate is greater than the number of grains whose growth direction is parallel to the substrate.
[0037] Specifically, Te grains initially grow laterally on the substrate. When a layer of Te grains accumulates on the entire surface of the substrate, the Te grains are in contact with an extremely thin layer of Te and will grow vertically. The substrate is essentially what affects the growth direction of Te grains. When the lattice constant of Te grains does not match that of the substrate, Te grains grow laterally first; while the lattice constant of Te grains matches that of the thin Te layer, they grow vertically first.
[0038] Te grains have a one-dimensional structure.
[0039] Specifically, the growth direction of the grains in the tellurium semiconductor film in contact with the substrate is parallel to the substrate (i.e., they grow laterally along the substrate), and they are stacked in a flower shape until they cover the entire substrate. Afterwards, since the adhesion between Te and Te is better than that between Te and the glass substrate, the Te grains tend to grow vertically.
[0040] Optionally, the tellurium semiconductor thin film is obtained by any of the preparation methods described above.
[0041] According to the third aspect of the present application, a device for preparing a tellurium semiconductor thin film is also provided, the device comprising a vapor transport deposition tube, a substrate and a source holder; the vapor transport deposition tube comprises a heating zone and a non-heating zone; the source holder is placed in the heating zone, and the source holder is used to place a solid-phase Te source; the substrate is placed in the non-heating zone, and the substrate is used to deposit vapor-phase Te to form a tellurium semiconductor thin film.
[0042] Optionally, the device further comprises a heat conductor, and the heat conductor is placed in a non-heating area of the vapor transport deposition tube;
[0043] The substrate is placed on the heat conducting member.
[0044] Optionally, the contact surface between the heat conducting member and the substrate is an inclined surface;
[0045] The inclination of the inclined surface is 70° to 80°.
[0046] Optionally, the device is used to implement any of the preparation methods described above.
[0047] According to a fourth aspect of the present application, there is also provided a tellurium semiconductor thin film obtained by any of the preparation methods described above, and an application of the tellurium semiconductor thin film described above in a photodetector.
[0048] The beneficial effects of this application include:
[0049] 1) The method for preparing tellurium semiconductor thin film provided in this application can reduce the vacuum degree of VTD equipment to 10 -1 Pa, less time (1-2min), the deposition process depends on the heating program, so there is no need for personnel to watch the whole process, but the cover must be removed immediately after the program is completed to prevent the Te powder from continuing to evaporate. The equipment is convenient for passing inert gases such as nitrogen and argon to achieve the growth of Te films under different atmospheres. At the same time, the VTD can be removed. During the evaporation process, the growth of the film can be observed at any time, which is convenient for recording and exploring the growth conditions of the film;
[0050] 2) The method for preparing the tellurium semiconductor thin film provided in the present application: (1) The operation is simple, the repeatability is high, the thin film preparation process takes less time, the efficiency is high, and the requirements for experimental equipment and environment are relatively low;
[0051] 3) The tellurium semiconductor thin film provided in this application has regular morphology and uniform thickness. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 Schematic diagram of the motion model of Te atoms in a VTD tube under high pressure (2.3 torr) for this application;
[0053] Figure 2 Schematic diagram of the motion model of Te atoms in a VTD tube under low pressure (0.023 torr) for this application;
[0054] Figure 3 (a), (b), (c) are surface morphologies of Te films prepared under different gas pressures in Example 1 of the present application;
[0055] Figure 4 (a), (b), (c) are SEM images of Te films prepared under different gas pressures in Example 1 of the present application;
[0056] Figure 5 (a), (b), (c) are XRD patterns of the Te film prepared under different gas pressures in Example 1 of the present application;
[0057] Figure 6 (a), (b), (c) are surface morphologies of Te films prepared at different deposition times in Example 2 of the present application;
[0058] 7(a), (b), and (c) are SEM images of Te films prepared at different deposition times in Example 2 of the present application;
[0059] Figure 8 is the surface morphology of the Te film obtained in the comparative example;
[0060] FIG9( a ) is a light response curve of Example 3 under a 530 nm LED light source;
[0061] FIG9( b ) is a light response curve of Example 3 under a 1450 nm LED light source;
[0062] FIG9( c ) is a light response curve of Example 3 under an LED light source of 1550 nm.
[0063] List of parts and reference numerals:
[0064] 100 vapor transport deposition tube; 200 glass substrate;
[0065] 300 graphite blocks; 400 source holders. DETAILED DESCRIPTION
[0066] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0067] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0068] The following is the motion model of Te atoms during VTD deposition:
[0069] See also Figure 1 and Figure 2 As shown, the graphite block 300 is located in the non-heating zone of the vapor transport deposition tube (VTD tube) 100, the glass substrate 200 is located on the inclined surface of the graphite block 300, the source holder 400 is located in the left heating zone of the vapor transport deposition tube 100, and Te powder is placed in the source holder 400.
[0070] Te is easy to condense, and the kinetic energy of Te atoms is insufficient. During the evaporation process at 460°C, when the air pressure is low, there is little air in the tube, and Te atoms tend to deposit on the low-temperature tube walls on both sides (that is, there is deposition in the non-heating areas at both ends of the tube wall), and very few are deposited on the substrate; when the air pressure is high, because the vacuum device is on the left side of the VTD tube 100 and there is more air in the tube, the airflow in the tube is from right to left, and the air will drive the Te atoms to move linearly to the left, so that most of the Te atoms are deposited on the substrate. In addition, the kinetic energy of Te atoms decreases during the collision with the air, which slows down the deposition rate of Te.
[0071] In the embodiments of the present application, VTD model: Hefei Kejing XTF-1200X.
[0072] Example 1
[0073] Take 0.5g of tellurium powder (99.999%, purchased from Aladdin) and put it in a quartz crucible. The quartz crucible is placed in the middle area of the left heating zone of the tube furnace (such as Figure 1 He Ru Figure 2 As shown in the figure, place the glass substrate on the inclined surface of the graphite block (the inclination is 75°), and then place the graphite block in the non-direct heating area of the quartz tube (VTD tube) 6 cm away from the heating area (the placement position will affect the substrate temperature and thus affect the film quality).
[0074] Evaporation process: adjust the gas pressure to 0.023torr, 0.23torr, and 2.3torr respectively, set the evaporation temperature to 460°C, the heating rate to 20°C / min, the evaporation time to 8min, and cool naturally.
[0075] Surface morphology test of Te films prepared under different gas pressures
[0076] The surface morphology of the prepared tellurium semiconductor film is subjected to light transmission and opacity tests. The light transmission test is to align the obtained tellurium semiconductor film with a light source for observation, and the opacity test is to place the obtained tellurium semiconductor film in a conventional position for observation.
[0077] The test results are as follows Figure 3(a) , 3(b) , as shown in 3(c).
[0078] Among them, 3(a) is the test result of the tellurium semiconductor film obtained after evaporation at 2.3torr and 460℃ for 8min. The left figure is the opaque test result, and the right figure is the transparent test result;
[0079] 3(b) is the test result of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 8min. The left picture is the opaque test result, and the right picture is the transparent test result.
[0080] 3(c) is the test result of the tellurium semiconductor film obtained after evaporation at 0.023torr and 460℃ for 8min. The left picture is the opaque test result, and the right picture is the transparent test result.
[0081] Depend on Figures 3(a) to 3(c) It can be seen that the morphologies of the Te films evaporated at pressures of 2.3 torr, 0.23 torr, and 0.023 torr are all different, and the thickness increases first and then decreases.
[0082] SEM images of Te films prepared under different gas pressures
[0083] The prepared different tellurium semiconductor films were tested by SEM. The test results are as follows: Figure 4(a) , 4(b) , as shown in 4(c).
[0084] Among them, 4(a) is the SEM test result of the tellurium semiconductor film obtained after evaporation at 2.3torr and 460℃ for 8min. The left picture is the test result at 10μm scale, and the right picture is the test result at 2μm scale.
[0085] 4(b) is the SEM test result of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 8min. The left picture is the test result at 10μm scale, and the right picture is the test result at 2μm scale.
[0086] 4(c) is the SEM test result of the tellurium semiconductor film obtained after evaporation at 0.023torr and 460℃ for 8min. The left picture is the test result at 40μm scale, and the right picture is the test result at 10μm scale.
[0087] Depend on Figures 4(a) to 4(c) It can be seen that as the evaporation pressure decreases, the Te grains increase, indicating that the crystallinity of the Te film is good under low pressure.
[0088] XRD patterns of Te films prepared under different gas pressures:
[0089] XRD tests were performed on the different tellurium semiconductor films prepared, and the test results are shown in Figures 5(a), 5(b) and 5(c).
[0090] Figure 5(a) shows the XDR test results of the tellurium semiconductor film obtained after evaporation at 2.3 torr and 460°C for 8 minutes;
[0091] Figure 5(b) shows the XDR test results of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 8min;
[0092] FIG5(c) shows the XDR test result of the tellurium semiconductor film obtained after evaporation at 0.023 torr and 460°C for 8 minutes.
[0093] It can be seen from Figures 5(a) to 5(c) that the lower the gas pressure, the higher the diffraction peak intensity and the better the crystallinity.
[0094] Example 2
[0095] The difference from Example 1 is that the evaporation process in Example 1 is adjusted as a whole to:
[0096] The gas pressure was set to 0.23 torr, the evaporation temperature was set to 460°C, the heating rate was 20°C / min, the evaporation time was adjusted to 4 min, 6 min, and 8 min respectively, and natural cooling was performed.
[0097] Surface morphology test of Te films prepared at different times
[0098] The surface morphology of the prepared tellurium semiconductor film was tested for light transmission and opacity. The test results are as follows: Figure 6(a) , 6(b) , as shown in 6(c).
[0099] Among them, 6(a) is the test result of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 4min. The left figure is the opaque test result, and the right figure is the light-transmitting test result;
[0100] 6(b) is the test result of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 6min. The left figure is the opaque test result, and the right figure is the transparent test result.
[0101] 6(c) is the test result of the tellurium semiconductor film obtained after evaporation at 0.23 torr and 460°C for 8 minutes. The left figure is the opaque test result, and the right figure is the translucent test result.
[0102] Depend on Figures 6(a) to 6(c) It can be seen that the initial deposition rate of the Te film is slow, and the evaporation time is between 6 and 8 minutes, which is the rapid growth process of the Te film under this process.
[0103] Therefore, during the film making process, the evaporation time is ≥6min.
[0104] SEM images of Te films prepared at different times
[0105] The prepared different tellurium semiconductor films were tested by SEM. The test results are as follows: Figure 7(a) , 7(b) , as shown in 7(c).
[0106] Among them, 7(a) is the SEM test result of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 4min. The left figure is the test result at 100μm scale, and the right figure is the test result at 20μm scale.
[0107] 7(b) is the SEM test result of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 6min. The left picture is the test result at 30μm scale, and the right picture is the test result at 10μm scale.
[0108] 7(c) is the SEM test result of the tellurium semiconductor film obtained after evaporation at 0.23torr and 460℃ for 8min. The left picture is the test result at 10μm scale, and the right picture is the test result at 2μm scale.
[0109] Depend on Figures 7(a) to 7(c) It can be seen that the Te grains nucleate at the site and quickly grow into a rod of a certain size, then continue to proliferate at the site, stacking into a flower shape until they cover the substrate and form a layer of Te grains. At this time, the Te grains grow horizontally. Later, because the adhesion between Te and Te is better than that between Te and the glass substrate, the Te grains tend to grow vertically.
[0110] Comparative Example 1
[0111] This comparative example corresponds to the example in Example 1 in which the evaporation pressure is 0.23 torr, and the only difference from Example 1 is that the inclination angle of the inclined surface is adjusted to 65°.
[0112] Figure 8 is the surface morphology of the comparative example. Figure 8 It can be seen that the uniformity of the prepared film is not good.
[0113] Example 3
[0114] Application in infrared detectors
[0115] Structure (photoconductive structure): glass / Te film / Ag (a silver paste electrode is brushed on the Te film. The Te film in this embodiment is the film corresponding to evaporation of 0.23 torr in Example 1)
[0116] The IT curves (i.e., light response curves, with light on every 10 seconds, and the test equipment is Agilent) under LED light sources with wavelengths of 530nm, 1450nm, and 1550nm are shown in Figures 9(a), 9(b), and 9(c):
[0117] Depend on Figure 9(a) to Figure 9(c) It can be seen that the initial attempt at Te infrared detection devices has good light response at 530nm, 1450nm and 1550nm.
[0118] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a tellurium semiconductor thin film, characterized in that: The preparation method comprises: performing vapor phase transport deposition on a Te source to obtain the tellurium semiconductor film; The preparation method comprises: S100, heating a solid-phase Te source placed in a heating zone of a vapor transport deposition tube at a temperature of 0.02 to 0.3 torr to obtain gas-phase Te; S200, depositing the gas-phase Te on a substrate located in a non-heating area of a vapor transport deposition tube to obtain the tellurium semiconductor thin film; The deposition time is 6 to 10 minutes; The angle between the substrate and the horizontal direction is α, and the value range of α is 70°≤α≤80°; The heating conditions are: Temperature: 450~470℃; Heating rate: 15~25℃ / min.
2. The preparation method according to claim 1, characterized in that: The substrate is placed on the heat conducting member; The heat conducting member is placed in the non-heating area of the vapor transport deposition tube.
3. The preparation method according to claim 2, characterized in that: The contact surface between the heat conducting member and the substrate is an inclined surface; The inclination of the inclined plane is 70°~80°.
4. The preparation method according to claim 2, characterized in that: The heat conducting member is selected from any one of a graphite block, an aluminum plate, and a ceramic plate.
5. The preparation method according to claim 1, characterized in that: The substrate is an inert substrate or an active substrate; The inert substrate includes any one of a glass substrate, an ITO substrate, and a FTO substrate; The active substrate includes any one of a TiO2 substrate, a CdS substrate, and a ZnO substrate.
6. The preparation method according to claim 1, characterized in that: The heating conditions are: Temperature: 450~460℃; Heating rate: 15~20℃ / min.
7. The preparation method according to claim 1, characterized in that: The Te source is Te powder.
8. A tellurium semiconductor thin film, characterized in that: The tellurium semiconductor thin film is obtained by the preparation method according to any one of claims 1 to 7; The growth direction of the grains in the tellurium semiconductor thin film that are in contact with the substrate is parallel to the substrate; The growth direction of the remaining grains is at an angle to the substrate and / or parallel to the substrate.
9. The tellurium semiconductor thin film according to claim 8, characterized in that: Among the remaining grains, the number of grains whose growth direction forms an angle with the substrate is greater than the number of grains whose growth direction is parallel to the substrate.
10. A device for preparing a tellurium semiconductor thin film, characterized in that: The device is used to implement the preparation method according to any one of claims 1 to 7; The apparatus includes a vapor transport deposition tube, a substrate, and a source holder; The vapor transport deposition tube includes a heating zone and a non-heating zone; The source holder is placed in the heating zone, and the source holder is used to place a solid-phase Te source; The substrate is placed in the non-heating zone, and the substrate is used to deposit gas-phase Te to form a tellurium semiconductor thin film.
11. The device according to claim 10, characterized in that The device further comprises a heat conducting member, which is placed in a non-heating area of the vapor transport deposition tube; The substrate is placed on the heat conducting member.
12. The device according to claim 11, characterized in that The contact surface between the heat conducting member and the substrate is an inclined surface; The inclination of the inclined plane is 70°~80°.
13. Application of the tellurium semiconductor thin film obtained by the preparation method according to any one of claims 1 to 7 in a photodetector.
14. Use of the tellurium semiconductor thin film according to any one of claims 8 to 9 in a photodetector.