Method for manufacturing semiconductor element mounting package substrate
In the manufacturing of the packaging substrate for semiconductor component mounting, the first pressing process of the copper-clad laminated plate is omitted, and combined with the heating and pressurization and patterning process, the problems of wrinkles and concave convexity of the metal foil are solved, and the production efficiency and yield rate are improved.
Patent Information
- Application Number
- CN201980081480.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-14
- Filing Date
- 2019-10-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-10-21
AI Technical Summary
When the conventional method of manufacturing a package substrate for semiconductor component mounting simultaneously forms a circuit substrate, it is easy to cause pleats and concaves of the metal foil, which reduces yield and manufacturing efficiency.
After the metal layer and the insulating resin layer are arranged on both sides of the core resin layer, the first substrate is formed by heating and pressurization, and the first pressing process of the copper-clad laminated plate is omitted, and only the second pressing process is performed, and then the second pressing process is performed. A pattern is formed on the 2 metal layer, and an insulating resin layer and a metal layer are arranged on the 3rd metal layer again, and the second substrate is heated and pressurized to form, and finally the metal layer is peeled off from the core resin layer to ensure that the metal layer is flat.
The production efficiency and yield of the packaging substrate for semiconductor component mounting is improved, the occurrence of poor patterning is reduced, and the manufacturing efficiency and finished product quality are improved.
Smart Images

Figure CN113243146B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a package substrate for mounting a semiconductor element. Background Art
[0002] The high functionality and miniaturization of semiconductor packages widely used in electronic equipment, communication equipment, and personal computers have been accelerating in recent years. Along with this, the printed circuit board and the semiconductor element mounting package substrate in the semiconductor package are required to be thinner. Generally, the printed circuit board and the semiconductor element mounting package substrate are made by laminating a layer (hereinafter, also referred to as "wiring conductor") that will become a circuit pattern on a supporting substrate and an insulating material.
[0003] As a method for manufacturing such a semiconductor element mounting package substrate, for example, the following method is disclosed: using a circuit forming substrate formed by providing a first insulating resin on a carrier foil surface of an extremely thin copper foil with a carrier foil, forming a first wiring conductor by pattern electrolytic copper plating, and then laminating a second insulating resin to form a second wiring conductor (for example, see Patent Document 1 below). In addition, a manufacturing technology for a printed circuit board using a laminate formed of a plate-like carrier made of resin and a metal foil releasably adhered to at least one surface of the carrier is disclosed (for example, see Patent Document 2 below).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2005-101137
[0007] Patent Document 2: International Publication No. WO2014 / 046291 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] As a method for manufacturing a package substrate for mounting semiconductor elements, the following method is known: a copper-clad laminate having metal foil on both sides of a core resin layer is used as a core, and insulating layers such as prepreg and metal foil are laminated on both sides to form a circuit-forming substrate, and the formed circuit-forming substrate is used. In the case of a circuit-forming substrate having four layers of metal foil, it is also called a "four-layer coreless shielding board". For example, a four-layer coreless shielding board is then subjected to a patterning process to become a six-layer coreless shielding board, and each substrate (laminated body) provided on both sides thereof is peeled off from the core resin layer.
[0010] Typically, in a method for manufacturing a circuit-forming substrate, after metal layers are arranged on both sides of a core resin layer, a first pressurizing step is performed by heating and pressurizing to form a copper-clad laminate, and then a second pressurizing step is performed after laminating resin layers, etc., to form the circuit-forming substrate.
[0011] On the other hand, with the development of alignment and pressurization technology, from the viewpoint of reducing the number of processes, studies have been conducted on the simultaneous formation of circuit-forming substrates. In the case of the simultaneous formation of circuit-forming substrates, the first pressurization process for forming a copper-clad laminate is omitted, and only the second pressurization process is performed to form the circuit-forming substrate.
[0012] In this way, if the circuit forming substrate is formed at the same time, a pressurizing process can be omitted, so the manufacturing efficiency of the circuit forming substrate and the semiconductor element mounting package substrate using the same can be improved. However, if the circuit substrate forming substrate is produced at the same time, when the substrates arranged on both sides thereof are peeled off from the core resin layer, wrinkles and unevenness may occur in the metal foil on the side of the peeled core resin layer. Such wrinkled and uneven metal foil may cause poor patterning, and as a result, when the circuit forming substrate is formed at the same time, the yield of the semiconductor element mounting package substrate may be reduced.
[0013] In order to solve the above-mentioned problems, an object of the present invention is to provide a method for manufacturing a semiconductor element mounting package substrate with good production efficiency and excellent yield.
[0014] Solutions for solving problems
[0015] <1> A method for manufacturing a semiconductor element mounting package substrate, comprising an insulating layer and a wiring conductor provided on the insulating layer, the method comprising the following steps:
[0016] First substrate forming step (a): forming a laminated body having a first metal layer, a first insulating resin layer and a second metal layer arranged in sequence on both sides of a core resin layer having a thickness of 1 μm to 80 μm, and heating and pressing the laminated body at the same time to form a first substrate, wherein the first metal layer has a thickness of 1 μm to 70 μm and can be peeled off from the core resin layer;
[0017] Patterning step (b): forming a pattern on the second metal layer of the first substrate;
[0018] Second substrate forming step (c): sequentially disposing a second insulating resin layer and a third metal layer on the surface of the second metal layer of the first substrate to form a laminate, and heating and pressurizing the formed laminate to form a second substrate; and,
[0019] The peeling step (d) is to peel off the third substrate from the core resin layer, wherein the third substrate includes the first metal layer, the first insulating resin layer, the second metal layer, the second insulating resin layer, and the third metal layer in this order.
[0020] <2> According to the aforementioned <1> The manufacturing method of the packaging substrate for mounting semiconductor elements, wherein, further includes the following wiring conductor forming step (e): forming a non-through hole reaching the surface of the aforementioned second metal layer on the surface of the aforementioned third substrate, performing electrolytic copper plating and / or chemical copper plating on the inner wall of the aforementioned non-through hole to connect the aforementioned second metal layer with the aforementioned first metal layer and the aforementioned third metal layer respectively, forming a fourth metal layer on the surface of the aforementioned third substrate, and forming a pattern on the aforementioned fourth metal layer, thereby forming the aforementioned wiring conductor.
[0021] <3> According to the aforementioned <1> or <2> In the method for manufacturing a semiconductor element mounting package substrate, the thickness of the third substrate is 5 μm to 100 μm.
[0022] <4> According to the aforementioned <1> ~ <3> The method for manufacturing a semiconductor element mounting package substrate according to any one of the preceding claims, wherein the first metal layer includes a release layer, and the first metal layer is arranged in the laminated body such that the release layer is in contact with the core resin layer.
[0023] <5> According to the aforementioned <1> ~ <4> The method for manufacturing a semiconductor element mounting package substrate according to any one of the preceding claims, wherein the third metal layer includes a carrier layer, and the carrier layer is removed from the third metal layer after the first substrate is heated and pressurized in the second substrate forming step (c).
[0024] <6> According to the aforementioned <1> ~ <5> In any one of the methods for manufacturing a semiconductor element mounting package substrate, at least any one of the first metal layer, the second metal layer, and the third metal layer is a copper foil.
[0025] <7> According to the aforementioned <1> ~ <6> The method for manufacturing a semiconductor element mounting package substrate according to any one of the above-mentioned embodiments, wherein at least any one of the core resin layer, the first insulating resin layer and the second insulating resin layer is a prepreg in which a base material is impregnated with a resin.
[0026] Effects of the Invention
[0027] According to the present invention, it is possible to provide a method for manufacturing a semiconductor element mounting package substrate having good production efficiency and excellent yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1This is a schematic diagram for explaining one embodiment of a method for manufacturing a semiconductor element mounting package substrate according to the present invention. DETAILED DESCRIPTION
[0029] Hereinafter, the present invention will be described by taking the embodiments as examples, but the aspects of the present invention are not limited to the embodiments described below.
[0030] A method for manufacturing a semiconductor element mounting package substrate according to the present embodiment (hereinafter, sometimes simply referred to as “the manufacturing method of the present embodiment”) is a method for manufacturing a semiconductor element mounting package substrate including an insulating layer and a wiring conductor provided on the insulating layer.
[0031] The manufacturing method comprises the following steps:
[0032] A first substrate forming step (a) of forming a laminate having a first metal layer, a first insulating resin layer and a second metal layer arranged in sequence on both sides of a core resin layer having a thickness of 1 μm to 80 μm, and simultaneously heating and pressing the laminate to form a first substrate, wherein the first metal layer has a thickness of 1 μm to 70 μm and can be peeled off from the core resin layer;
[0033] A patterning step (b) of forming a pattern on the second metal layer of the first substrate;
[0034] A second substrate forming step (c) of sequentially disposing a second insulating resin layer and a third metal layer on the surface of the second metal layer of the first substrate to form a laminate, and heating and pressurizing the formed laminate to form a second substrate; and
[0035] The peeling step (d) is to peel off a third substrate from the core resin layer, the third substrate including the first metal layer, the first insulating resin layer, the second metal layer, the second insulating resin layer and the third metal layer in this order.
[0036] In the manufacturing method of the package substrate for mounting semiconductor elements of the present embodiment, a laminated body having a first metal layer, a first insulating resin layer and a second metal layer arranged in sequence is formed on both sides of a core resin layer having a thickness of 1 μm to 80 μm, and the aforementioned laminated body is heated and pressurized at the same time to form a first substrate, wherein the thickness of the first metal layer is 1 μm to 70 μm and can be peeled off from the aforementioned core resin layer. The first substrate is a substrate equivalent to a circuit forming substrate. Here, "circuit forming substrate" refers to a laminated body comprising a core resin layer, a metal foil and a resin layer, in a state where patterning, etc. is not performed on the metal foil. In addition, in the manufacturing method of the present embodiment, the first substrate (circuit forming substrate) is formed at the same time. Here, "simultaneously forming the first substrate (circuit forming substrate)" means that in the first substrate forming step (a), after the first metal layer, the first insulating resin layer and the second metal layer are sequentially arranged on both sides of the core resin layer with the core resin layer as the center, heating and pressurizing (implementing a pressurizing step) are performed to form the first substrate (circuit forming substrate). Its meaning is: omitting the pressurizing step for forming a copper-clad laminate (a state in which only the first metal layer is laminated on both sides of the core resin layer), and forming the first substrate by implementing a single pressurizing step.
[0037] Furthermore, the manufacturing method of the present embodiment uses a core resin layer having a thickness of 1 μm to 80 μm. That is, in the manufacturing method of the present embodiment, by using a core resin layer having a thickness of 1 μm to 80 μm, even if the first substrate (circuit forming substrate) is formed at the same time, it is possible to suppress the occurrence of wrinkles and bumps in the metal layer on the core resin layer side of the substrate (third substrate) peeled off from the core resin layer in the peeling step (d). Therefore, the manufacturing method of the present embodiment improves production efficiency by simultaneously forming the first substrate (circuit forming substrate), and further suppresses the occurrence of wrinkles and bumps in the metal layer that cause poor patterning, thereby improving the yield of the packaging substrate for mounting semiconductor elements.
[0038] Hereinafter, the production method of this embodiment will be described in detail.
[0039] [First substrate forming step (a)]
[0040] The first substrate forming step (a) is a step of forming a laminated body having a thickness of 1 μm to 70 μm and a first insulating resin layer and a second metal layer which are sequentially arranged on both sides of a core resin layer having a thickness of 1 μm to 80 μm and can be peeled off from the core resin layer, and heating and pressurizing the laminated body at the same time to form the first substrate. Figure 1 The structure of the first substrate (circuit forming substrate) will be described. Figure 1 1 is a schematic diagram for explaining one embodiment of a method for manufacturing a semiconductor element mounting package substrate according to the present invention. Figure 1 (A) and Figure 1 As shown in (B), the circuit forming substrate (first substrate) 1 has a first metal layer 3, a first insulating resin layer 4 and a second metal layer 5 provided on both sides of a core resin layer 2 (eg, prepreg) in this order from the surface side of the core resin layer 2.
[0041] In the first substrate forming step (a), the first metal layer, the first insulating resin layer and the second metal layer are sequentially arranged on both sides of the core resin layer, and after forming a laminate, heating and pressing are performed to form the first substrate. At this time, the pressing step for forming a copper-clad laminate (a state in which only the first metal layer is stacked on both sides of the core resin layer) is not performed, and after the first insulating resin layer and the second metal layer are stacked, a pressing step is performed once to form the first substrate.
[0042] The stacking method and conditions for forming the laminate are not particularly limited. For example, the laminate can be subjected to vacuum pressing at a temperature of 220±2°C, a pressure of 5±0.2MPa, and a holding time of 60 minutes to form the first substrate. In addition, in order to obtain the adhesion between each metal layer and the core resin layer or each insulating resin layer, the surface of each metal layer can be roughened. The roughening treatment is not particularly limited, and known means can be used appropriately, for example, means using a copper surface roughening liquid can be cited.
[0043] (Core resin layer)
[0044] The core resin layer in the first substrate forming step (a) is not particularly limited, and for example, a prepreg in which an insulating resin material (insulating material) such as a thermosetting resin is impregnated into a base material such as glass cloth, or an insulating film material can be used.
[0045] The thickness of the core resin layer is 1 μm to 80 μm. If the thickness of the core resin layer is less than 1 μm, the resin molding will be poor. If it exceeds 80 μm, when the first substrate is formed simultaneously, wrinkles and unevenness will occur in the metal layer on the surface of the third substrate peeled off from the core resin layer after the peeling process. From the viewpoint of stacking moldability, the thickness of the core resin layer is preferably 3 μm to 40 μm, and more preferably 10 μm to 25 μm.
[0046] "Prepreg" is formed by impregnating or coating an insulating material such as a resin composition on a substrate. The substrate is not particularly limited, and known substances used in laminates for various electrical insulating materials can be used appropriately. Examples of materials constituting the substrate include inorganic fibers such as E glass, D glass, S glass, or Q glass; organic fibers such as polyimide, polyester, or tetrafluoroethylene; and mixtures thereof. The substrate is not particularly limited, and for example, shaped substrates such as woven fabrics, non-woven fabrics, rovings, chopped strands, and cushions can be used appropriately. The material and shape of the substrate can be selected according to the purpose and performance of the target molded product, and can be used alone or in combination of two or more materials and shapes as needed.
[0047] The thickness of the substrate is not particularly limited as long as the thickness of the core resin layer is in the range of 1 μm to 80 μm, and a substrate of 10 μm to 30 μm can usually be used. In addition, as the substrate, a substrate that has been surface treated with a silane coupling agent or the like or a substrate that has been mechanically fiberized can be used, and these substrates are suitable from the aspects of heat resistance, moisture resistance, and processability.
[0048] As the aforementioned insulating material, there is no particular limitation, and a known resin composition used as an insulating material for a printed circuit board can be appropriately selected and used. As the aforementioned resin composition, a thermosetting resin with good heat resistance and chemical resistance can be used as a basis. As the thermosetting resin, there is no particular limitation, and examples thereof include phenolic resin, epoxy resin, cyanate resin, maleimide resin, isocyanate resin, benzocyclobutene resin, vinyl resin, etc. The thermosetting resin can be used alone or in combination of two or more.
[0049] Among thermosetting resins, epoxy resins can be used as insulating materials from the aspects of heat resistance, chemical resistance, excellent electrical properties, and relatively low cost. As epoxy resins, for example, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, alicyclic epoxy resins, aliphatic chain epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, diglycidyl ethers of biphenols, diglycidyl ethers of naphthalene diols, diglycidyl ethers of phenols, diglycidyl ethers of alcohols, and their alkyl substituted bodies, halides, hydrides, etc. can be cited. One epoxy resin can be used alone, or two or more can be mixed and used. In addition, the curing agent used together with the epoxy resin can be used without limitation as long as it can cure the epoxy resin, and examples thereof include: polyfunctional phenols, polyfunctional alcohols, amines, imidazole compounds, acid anhydrides, organic phosphorus compounds, and halides thereof, etc. These epoxy resin curing agents can be used alone or in combination of two or more.
[0050] The cyanate resin is a resin that generates a cured product with triazine ring as a repeating unit by heating, and the cured product has excellent dielectric properties. Therefore, it is particularly suitable for situations where high-frequency properties are required. As a cyanate resin, there is no particular limitation, and for example, 2,2-bis(4-cyanophenyl)propane, bis(4-cyanophenyl)ethane, 2,2-bis(3,5-dimethyl-4-cyanophenyl)methane, 2,2-(4-cyanophenyl)-1,1,1,3,3,3-hexafluoropropane, α,α'-bis(4-cyanophenyl)-m-diisopropylbenzene, phenol novolac and alkylphenol novolac cyanate esters, etc. can be cited. Among them, the balance between the dielectric properties and curability of the cured product of 2,2-bis(4-cyanophenyl)propane is particularly good, and it is also cheap in terms of cost, so it is preferred. These cyanate resins such as cyanate ester compounds can be used alone or in combination of two or more. In addition, a part of the cyanate ester compound may be oligomerized in advance to form a trimer or a pentamer.
[0051] Furthermore, a curing catalyst and a curing accelerator may be used in combination for the cyanate resin. As the curing catalyst, for example, metals such as manganese, iron, cobalt, nickel, copper, and zinc may be used, and specifically, organic metal salts such as 2-ethylhexanoate and octanoate, and organic metal complexes such as acetylacetone complexes may be cited. The curing catalyst may be used alone or in combination of two or more.
[0052] In addition, as a curing accelerator, phenols are preferably used, and monofunctional phenols such as nonylphenol and p-cumylphenol, bifunctional phenols such as bisphenol A, bisphenol F, and bisphenol S, or polyfunctional phenols such as phenol novolac and cresol novolac can be used. The curing accelerator can be used alone or in combination of two or more.
[0053] In consideration of dielectric properties, impact resistance, film processability, etc., a thermoplastic resin may also be blended in the resin composition used as the aforementioned insulating material. The thermoplastic resin is not particularly limited, and examples thereof include fluororesins, polyphenylene ethers, modified polyphenylene ethers, polyphenylene sulfides, polycarbonates, polyetherimides, polyetheretherketones, polyacrylates, polyamides, polyamideimides, polybutadiene, etc. The thermoplastic resin may be used alone or in combination of two or more.
[0054] Among thermoplastic resins, it is useful to mix polyphenylene ether and modified polyphenylene ether for use from the viewpoint of improving the dielectric properties of the cured product. As polyphenylene ether and modified polyphenylene ether, for example, poly(2,6-dimethyl-1,4-phenylene) ether, alloy polymer of poly(2,6-dimethyl-1,4-phenylene) ether and polystyrene, alloy polymer of poly(2,6-dimethyl-1,4-phenylene) ether and styrene-butadiene copolymer, alloy polymer of poly(2,6-dimethyl-1,4-phenylene) ether and styrene-maleic anhydride copolymer, alloy polymer of poly(3,6-dimethyl-1,4-phenylene) ether and polyamide, alloy polymer of poly(2,6-dimethyl-1,4-phenylene) ether and styrene-butadiene-acrylonitrile copolymer, etc. can be cited. In order to impart reactivity and polymerizability to polyphenylene ether, functional groups such as amine, epoxy, carboxyl, styryl, etc. may be introduced at the polymer chain end or at the polymer chain side chain.
[0055] Among thermoplastic resins, polyamide-imide resins are useful from the viewpoint of excellent moisture resistance and good adhesion to metals. The raw materials of polyamide-imide resins are not particularly limited. As acidic components, trimellitic anhydride and trimellitic anhydride monochloride can be mentioned, and as amine components, metaphenylenediamine, paraphenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, bis[4-(aminophenoxy)phenyl]sulfone, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, etc. can be mentioned. Polyamide-imide resins can be modified with siloxane to improve drying properties. In this case, siloxane diamine can be used as an amino component. If film processability is considered, polyamide-imide resins preferably use those with a molecular weight of 50,000 or more.
[0056] The above-mentioned thermoplastic resins are described as insulating materials mainly used for prepregs, but these thermoplastic resins are not limited to the application as prepregs. For example, the above-mentioned thermoplastic resins can also be processed into a film (film material) as the core resin layer in the above-mentioned circuit forming substrate.
[0057] In the resin composition used as an insulating material, an inorganic filler may also be mixed. The inorganic filler is not particularly limited, and examples thereof include aluminum oxide, aluminum hydroxide, magnesium hydroxide, clay, talc, antimony trioxide, antimony pentoxide, zinc oxide, fused silica, glass powder, quartz powder, Shirasu balloon, etc. These inorganic fillers may be used alone or in combination of two or more.
[0058] The resin composition used as an insulating material may contain an organic solvent. As an organic solvent, there is no particular limitation, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, and trimethylbenzene can be used in combination as desired; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ether solvents such as tetrahydrofuran; alcohol solvents such as isopropanol and butanol; ether alcohol solvents such as 2-methoxyethanol and 2-butoxyethanol; amide solvents such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. It should be noted that the amount of solvent in the varnish when making the prepreg is preferably set to a range of 40 to 80% by mass relative to the entire resin composition. In addition, the viscosity of the aforementioned varnish is expected to be in the range of 20 to 100 cP (20 to 100 mPa·s).
[0059] The resin composition used as an insulating material may contain a flame retardant. The flame retardant is not particularly limited, and for example, bromine compounds such as decabromodiphenyl ether, tetrabromobisphenol A, tetrabromophthalic anhydride, tribromophenol, phosphorus compounds such as triphenyl phosphate, tri(xylene) phosphate, cresyl diphenyl phosphate, metal hydroxides such as magnesium hydroxide and aluminum hydroxide, red phosphorus and its modified products, antimony compounds such as antimony trioxide and antimony pentoxide, triazine compounds such as melamine, cyanuric acid, and melamine cyanurate can be used.
[0060] To the resin composition used as an insulating material, the above-mentioned curing agent, curing accelerator, and various additives and fillers such as thermoplastic particles, coloring agent, ultraviolet light opaque agent, antioxidant, and reducing agent may be further added as needed.
[0061] For the prepreg in this embodiment, for example, a resin composition (including varnish) is impregnated or applied to a substrate so that the amount of the resin composition attached to the substrate is 20 to 90% by mass based on the resin content in the dried prepreg, and then heated and dried at a temperature of 100 to 200° C. for 1 to 30 minutes, thereby obtaining a prepreg in a semi-cured state (B-stage state). As such a prepreg, for example, GHPL-830NSF series (product name) manufactured by Mitsubishi Gas Chemical can be used.
[0062] (1st metal layer)
[0063] The first metal layer uses a metal foil having a thickness of 1 μm to 70 μm and capable of being peeled off from the core resin layer. If the thickness of the first metal layer is less than 1 μm, the first to third substrates will be poorly formed, and if it exceeds 70 μm, the surface will be poor. From the viewpoint of circuit formation, the thickness of the first metal layer is preferably 1 μm to 12 μm, and more preferably 2 μm to 5 μm.
[0064] As described later, the third substrate is peeled off from the interface between the core resin layer and the first metal layer in the peeling process. From the viewpoint of reducing peeling failure, the surface roughness of the first metal layer when peeled off from the core resin layer in the peeling process (10-point average roughness (Rzjis) shown in JIS B0601:2001) is preferably 1 μm to 3 μm, more preferably 1 μm to 2 μm, and particularly preferably 1 μm to 1.5 μm. The surface roughness of the first metal layer can be measured, for example, as follows: after cutting the sample into 5×5 cm, the range of 1×1 cm is measured using a microscope VR-3100 (manufactured by KEYENCE).
[0065] As the first metal layer, for example, copper foil can be used. In addition, as the copper foil, for example, a peelable copper foil can be used. The "peelable" copper foil refers to an extremely thin copper foil having a release layer, and the release layer refers to a peelable copper foil, for example. When a peelable copper foil is used, the first metal layer is laminated in such a way that the release layer is in contact with the core resin layer.
[0066] As the release layer, for example, a layer containing at least a silicon compound can be cited, for example, a silicon compound formed by imparting a single or a combination of multiple silane compounds on a copper foil or an ultra-thin copper foil, thereby forming. It should be noted that the means for imparting the silicon compound is not particularly limited, for example, known means such as coating can be used. The bonding surface of the copper foil with the release layer can be subjected to rust prevention treatment (forming a rust prevention treatment layer). The aforementioned rust prevention treatment can be carried out using any of nickel, tin, zinc, chromium, molybdenum, cobalt, or their alloys.
[0067] The thickness of the release layer is not particularly limited, but is preferably 5 nm to 100 nm, more preferably 10 nm to 80 nm, and particularly preferably 20 nm to 60 nm from the viewpoint of removability and peelability.
[0068] (First insulating resin layer)
[0069] As the first insulating resin layer, the same material as the core resin layer (e.g., prepreg) can be used. In addition, the thickness of the first insulating resin layer can be appropriately set as desired, and therefore, is not particularly limited, and can be, for example, 10 μm to 100 μm, preferably 10 μm to 50 μm, and more preferably 10 μm to 30 μm.
[0070] (Metal Layer 2)
[0071] As the second metal layer, for example, the same material as the first metal layer (for example, copper foil) can be used. The thickness of the second metal layer can be appropriately set as desired, and therefore is not particularly limited, and can be, for example, 2 μm to 70 μm, preferably 2 μm to 18 μm, and more preferably 2 μm to 12 μm.
[0072] In addition, as the second metal layer, for example, an ultra-thin copper foil with a carrier can be used. In this case, the second metal layer is arranged so that the copper foil is in contact with the second insulating resin layer, and the carrier is peeled off after forming the first substrate by heating and pressing.
[0073] [Patterning step (b)]
[0074] The patterning step (b) is a step of forming a pattern on the second metal layer of the first substrate (circuit forming substrate). Figure 1 As shown in (C), a pattern is formed on the second metal layer 5 of the circuit-forming board 1. The means for forming the pattern of the second metal layer is not particularly limited, and the pattern can be formed, for example, by the following steps.
[0075] The patterning step (b) is not particularly limited. For example, the entire surface of the second metal layer is treated, a dry film resist is laminated, and then a negative mask is attached. Then, the circuit pattern is baked with an exposure machine, and the dry film resist is developed with a developer to form a resist layer. Thereafter, an etching treatment is performed, and copper in the portion without the resist layer is removed with an aqueous solution of ferric chloride, etc., and then the resist layer is removed, thereby forming a pattern on the second metal layer.
[0076] Above-mentioned resist is not particularly limited, for example can be suitable for selecting known materials such as commercially available dry film resist and use.In addition, the photolithography (comprising exposure, development, the removal of resist) when patterning on the 2nd metal layer is not particularly limited, can use known means and device and implement.
[0077] The pattern width of the second metal layer is not particularly limited, and can be appropriately selected depending on the intended use. For example, it can be 5 to 100 μm, and preferably 10 to 30 μm.
[0078] [Second substrate forming step (c)]
[0079] The second substrate forming step (c) is a step of sequentially placing a second insulating resin layer and a third metal layer on the surface of the second metal layer of the first substrate to form a laminate, and heating and pressurizing the laminate to form the second substrate. Figure 1 As shown in (D), the second substrate 8 in which the second insulating resin layer 6 and the third metal layer 7 are stacked on the second metal layer 5 can be obtained.
[0080] (Second Insulating Resin Layer)
[0081] As the second insulating resin layer, the same material as the core resin layer (e.g., prepreg) can be used. In addition, the thickness of the second insulating resin layer can be appropriately set as desired, and therefore, is not particularly limited, and can be set to, for example, 10 μm to 100 μm, preferably 10 μm to 50 μm, and more preferably 10 μm to 30 μm.
[0082] (Metal Layer 3)
[0083] As the third metal layer, for example, the same material as the first metal layer (for example, copper foil) can be used. The thickness of the third metal layer can be appropriately set as desired, and is therefore not particularly limited, and can be, for example, 2 μm to 70 μm, preferably 2 μm to 18 μm, and more preferably 2 μm to 5 μm.
[0084] In addition, as the third metal layer, for example, an ultra-thin copper foil with a carrier can be used. In this case, the third metal layer is arranged so that the copper foil is in contact with the second insulating resin layer, and the carrier is peeled off after forming the second substrate by heating and pressing.
[0085] (Lamination method / conditions)
[0086] In order to obtain the second substrate, the method and conditions for laminating the second insulating resin layer and the third metal layer are not particularly limited. For example, after laminating the second insulating resin layer and the third metal layer on the first substrate, vacuum pressing is performed under the conditions of temperature 220±2°C, pressure 5±0.2MPa, and holding time 60 minutes, thereby forming the second substrate. In addition, in order to obtain the adhesion between the second metal layer and the second insulating resin layer, the surface of the second metal layer can be roughened.
[0087] [Peeling step (d)]
[0088] The peeling step (d) is a step of peeling off the third substrate from the core resin layer, wherein the third substrate sequentially comprises the first metal layer, the first insulating resin layer, the second metal layer, the second insulating resin layer, and the third metal layer. Figure 1 As shown in (E), the second substrate is separated at the interface between the core resin layer 2 and the first metal layer 3 arranged on both sides thereof, thereby obtaining two third substrates 9 which sequentially have the first metal layer 3, the first insulating resin layer 4, the second metal layer 5, the second insulating resin layer 6 and the third metal layer 7.
[0089] The thickness of the third substrate can be appropriately set as desired and is not particularly limited, but can be, for example, 5 μm to 400 μm, preferably 5 μm to 200 μm, and more preferably 5 μm to 100 μm.
[0090] In the stripping step (d), the core resin layer is preferably stripped at the interface between the core resin layer and the first metal layer, but, for example, when the first metal layer has a release layer, a portion of it may be stripped together with the core resin layer. In addition, the core resin layer is also stripped together with the release layer at the interface between the release layer of the first metal layer and the copper foil. When the release layer remains on the first metal layer, the release layer may be removed using, for example, a sulfuric acid-based or hydrogen peroxide-based etching solution. The sulfuric acid-based or hydrogen peroxide-based etching solution is not particularly limited, and substances used in the art may be used.
[0091] [Wiring conductor forming step (e)]
[0092] The manufacturing method of this embodiment may further include the following wiring conductor forming step (e): forming a non-through hole on the surface of the third substrate that reaches the surface of the second metal layer, electrolytic copper plating and / or chemical copper plating are performed on the inner wall of the non-through hole to connect the second metal layer to the first metal layer and the third metal layer, respectively, forming a fourth metal layer on the surface of the third substrate, and forming a pattern on the fourth metal layer, thereby forming the wiring conductor. If the wiring conductor forming step (e) is performed, then Figure 1 As shown in (I), a semiconductor element mounting package substrate 12 having wiring conductors 11 formed on both sides of an insulating layer 10 can be obtained. It should be noted that the insulating layer 10 is composed of a first insulating resin layer 4 and a second insulating resin layer 6, and the wiring conductors 11 can be formed by interlayer connection of the first metal layer 3, the second metal layer 5 and the third metal layer 7, which are patterned respectively, by electrolytic copper plating and / or chemical copper plating.
[0093] (Formation of non-through holes)
[0094] In the wiring conductor forming step (e), a non-through hole reaching the surface of the second metal layer is formed on the surface of the third substrate. Figure 1 As shown in (F), the non-through holes 13 are provided on both sides of the third substrate 9. Figure 1 In (F), the non-through hole 13 is formed in the second insulating resin layer 6 via the third metal layer 7. Figure 1 On the lower side of the paper in (F), the non-through hole 13 is formed in the first insulating resin layer 4 via the first metal layer 3 .
[0095] The formation means of the non-through hole is not particularly limited, for example, known means such as lasers such as carbon dioxide gas lasers and drills can be used. The number and size of the non-through holes can be appropriately selected according to expectations. In addition, after the non-through holes are formed, a desmearing process can be implemented using a sodium permanganate aqueous solution or the like.
[0096] (Interlayer connection and formation of the 4th metal layer)
[0097] In the wiring conductor forming step (e), Figure 1 As shown in (G), after the non-through hole 13 is formed, electrolytic copper plating and / or chemical copper plating are performed to form a copper-plated film on the inner wall of the non-through hole 13, and the first metal layer 3, the second metal layer 5 and the third metal layer 7 which are patterned are electrically connected. Furthermore, by the electrolytic copper plating and / or chemical copper plating, the thickness of the first and third metal layers on both sides of the third substrate is increased, thereby forming the fourth metal layer 14. The method for implementing electrolytic copper plating and / or chemical copper plating is not particularly limited, and a known method can be used. The copper plating can be only any one of electrolytic copper plating and chemical copper plating, and preferably both electrolytic copper plating and chemical copper plating are implemented.
[0098] (Film thickness adjustment)
[0099] In the wiring conductor forming step (e), Figure 1 As shown in (H), after the electrolytic copper plating / chemical copper plating treatment, a known treatment such as etching treatment may be performed as necessary so that the fourth metal layer 14 has a desired thickness, thereby adjusting the film thickness of the fourth metal layer 14.
[0100] The thickness of the fourth substrate after adjustment can be appropriately set as desired, and is therefore not particularly limited, but can be, for example, 5 μm to 30 μm, preferably 5 μm to 20 μm, and more preferably 5 μm to 12 μm.
[0101] (Pattern)
[0102] In the wiring conductor forming step (e), after the entire surface of the fourth metal layer 14 is processed as needed, a dry film resist is laminated, and then a negative mask is attached. The circuit pattern is baked with an exposure machine, and the dry film resist is developed with a developer to form a resist layer. After that, an etching process is performed to remove the copper in the portion without the resist layer with an aqueous solution of ferric chloride, and then the resist layer is removed, so that Figure 1 As shown in (I), the wiring conductors 11 may be formed on both surfaces of the insulating layer 10 .
[0103] In addition, as an interlayer connection method that can be used in the present embodiment, the following methods can be applied: a method of applying chemical copper plating to a blind hole portion formed by a known laser (a method of forming a wiring circuit by laser processing and then patterning and interlayer connection by chemical copper plating); a method of piercing each insulating layer and making interlayer connections by using metal bumps (preferably copper bumps) formed by etching a plating layer, metal foil, etc. on a portion that has previously become a connection portion; and further, after a metal paste containing metal fillers such as solder, silver and copper in an insulating resin is printed on a specified position by means of bumps such as screen printing, the paste is solidified by drying, and electrical conductivity between the inner and outer layers is ensured by heating and pressurizing.
[0104] In the exemplary embodiment of the present invention, Figure 1 In the embodiment, the semiconductor element mounting package substrate 12 is a three-layered semiconductor element mounting package substrate, but the present invention is not limited thereto, and a semiconductor element mounting package substrate having a further laminated structure such as a five-layer structure can be formed. For example, in the wiring conductor forming step (e), after forming the wiring conductor, the insulating resin layer and the metal layer are stacked, and patterning and interlayer connection are repeated, thereby manufacturing a semiconductor element mounting package substrate having a laminated structure.
[0105] 《Method for manufacturing a package substrate for mounting a semiconductor element》
[0106] In the method for manufacturing a semiconductor element mounting package substrate of the present embodiment, after the semiconductor element mounting package substrate is formed as described above, a semiconductor element such as a bare chip can be mounted thereon as desired.
[0107] The aforementioned semiconductor element is not particularly limited, and the desired element can be used appropriately. For example, a bare chip with gold bumps formed by ball bonding of gold wire on an aluminum electrode portion can be used. The semiconductor element can be mounted on the wiring conductor of a semiconductor element mounting package substrate with the aid of a bonding material. The aforementioned bonding material is not particularly limited as long as it has a conductive means, for example, solder (such as solder balls, solder paste, etc.) can be used. In addition, the semiconductor element can be mounted with the aid of a bonding material after the wiring conductor of the semiconductor element mounting package substrate is subjected to surface treatment. The aforementioned surface treatment is not particularly limited, and for example, the formation of a nickel layer or a gold plating layer can be cited. In the case of using solder as the aforementioned bonding material, after the semiconductor element is mounted on the wiring conductor, a process such as reflow soldering can be performed. At this time, the temperature of the reflow soldering can be appropriately selected according to the melting point of the bonding material, for example, it can be set to above 260°C.
[0108] Example
[0109] Hereinafter, the production method of the present invention will be specifically described based on examples.
[0110] [Comparative Example 1]
[0111] Copper foils (manufactured by JX Nippon Mining & Metals Corp., trade name: PCS) prepared by coating a release layer on a 2 μm thick copper foil were arranged on both sides of a prepreg (core resin layer: thickness 0.087 mm: GHPL-830NSF FX64 manufactured by Mitsubishi Gas Chemical) in which a bismaleimide triazine resin (BT resin) was impregnated in a glass cloth (glass fiber) to form a B-stage, so that the release layer and the prepreg were bonded, and a prepreg (thickness 0.025 mm: GHPL-830NSF manufactured by Mitsubishi Gas Chemical) in which a bismaleimide triazine resin (BT resin) was impregnated in a glass cloth (glass fiber) to form a B-stage was further arranged thereon. FF70), and laminated with a 12 μm copper foil (manufactured by Mitsui Mining & Smelting Co., Ltd., trade name: 3EC-VLP) under vacuum pressure of 2.5±0.2 MPa, temperature of 220±2° C., and holding time of 60 minutes.
[0112] The entire surface of the obtained substrate was treated, and a dry film resist (Nichigo Morton Co., Ltd., trade name: NIT225) was laminated at a temperature of 110±10°C and a pressure of 0.50±0.02MPa. After that, a negative mask was attached, and the circuit pattern was baked with a parallel exposure machine, and the dry film resist was developed with a 1% sodium carbonate aqueous solution to form a resist layer, and the copper in the part without the resist layer was removed with an ferric chloride aqueous solution. After that, the dry film resist was removed with a sodium hydroxide aqueous solution to form a circuit pattern.
[0113] The surface of the substrate having the circuit pattern formed thereon was roughened with a copper surface roughening liquid (manufactured by MEC Co., Ltd., product name: CZ-8100), and on both sides of the substrate, a 2 μm copper foil with a carrier copper foil of 18 μm (manufactured by Mitsui Mining & Smelting Co., Ltd., product name: MTEx) was laminated under vacuum pressure of 2.5±0.2 MPa, temperature of 220±2° C., and holding time of 60 minutes, through a prepreg (thickness 0.025 mm: GHPL-830NSF FF70 manufactured by Mitsubishi Gas Chemical) formed in the B stage by impregnating bismaleimide triazine resin (BT resin) in glass cloth (glass fiber), and then the 18 μm carrier copper foil was peeled off.
[0114] The obtained substrate was peeled off by applying physical force to the boundary between the core resin layer, PCS and copper foil. However, the copper foil surface on the peeled side had many irregularities, which reduced the yield during laser processing and circuit formation.
[0115] [Example 1]
[0116] <First substrate forming step (a)>
[0117] In the process of impregnating glass cloth (glass fiber) with bismaleimide triazine resin (BT resin) to form a B-stage prepreg ( Figure 1 (A) The core resin layer 2; thickness 25μm: Mitsubishi Gas Chemical GHPL-830NSF FF70) on both sides, configured on a 2μm thick copper foil coated with a release layer (JX Nippon Mining & Metals Corp, trade name: PCS) with a release layer formed of copper foil ( Figure 1 The first metal layer 3 in (A) is formed so that the release layer contacts the core resin layer, and further a prepreg ( Figure 1 (A) in the first insulating resin layer 4; thickness 0.025mm: Mitsubishi Gas Chemical GHPL-830NSF FF70), vacuum pressurized, at a pressure of 2.5 ± 0.2MPa, a temperature of 220 ± 2 ° C, a holding time of 60 minutes under the conditions of laminated 12μm copper foil ( Figure 1 (A) The second metal layer 5; Mitsui Mining & Smelting Co., Ltd., trade name: 3EC-VLP), the first substrate ( Figure 1 (B) Circuit forming substrate (first substrate) 1).
[0118] <Patterning step (b)>
[0119] Next, the entire surface of the first substrate was treated, and a dry film resist (Nichigo Morton Co., Ltd., trade name: NIT225) was laminated on the surface of the second metal layer at a temperature of 110±10°C and a pressure of 0.50±0.02MPa. After that, a negative mask was attached, the circuit pattern was baked with a parallel exposure machine, and the dry film resist was developed with a 1% sodium carbonate aqueous solution to form a resist layer. After removing the copper in the part without the resist layer with an iron chloride aqueous solution, the dry film resist was removed with a sodium hydroxide aqueous solution to form a pattern on the second metal layer 5 (refer to Figure 1 (C)).
[0120] <Second substrate forming step (c)>
[0121] Next, the surface of the patterned second metal layer 5 is roughened with a copper surface roughening liquid (manufactured by MEC Co., Ltd., product name: CZ-8100), and the surfaces of the second metal layers 5 provided on both sides of the circuit forming substrate 1 are roughened with a prepreg ( Figure 1(D) in the second insulating resin layer 6; thickness 0.025mm: Mitsubishi Gas Chemical GHPL-830NSF FF70), vacuum pressurized, at a pressure of 2.5 ± 0.2MPa, a temperature of 220 ± 2 ° C, a holding time of 60 minutes, laminated with a 18μm carrier copper foil 2μm copper foil ( Figure 1 (D) The third metal layer 7; manufactured by Mitsui Mining & Smelting Co., Ltd., trade name: MTEx). Then, the 18 μm carrier copper foil was peeled off to prepare the second substrate ( Figure 1 (D) The second substrate 8).
[0122] <Peeling step (d)>
[0123] On the second substrate, a physical force is applied to the boundary between the copper foil with a release layer (the first metal layer 3) and the prepreg (the core resin layer 2) to separate them, thereby obtaining a third substrate ( Figure 1 (E) The third substrate 9) The surface irregularities of the copper foil on the peeled side were measured by the following method. The surface irregularities of the copper foil on the peeled side were 2.25 μm.
[0124] The surface irregularities of the copper foil on the peeled side were measured. The surface irregularities were measured using a microscope VR-3100 (manufactured by Keyence Corporation) and the sample cut into 5×5 cm was measured in an area of 1×1 cm using the above-mentioned device.
[0125] <Wiring conductor forming step (e)>
[0126] On both sides of the third substrate, a carbon dioxide gas laser processing machine (manufactured by Hitachi Via Mechanics, Ltd., trade name: LC-1C / 21) was used to process each hole under the conditions of beam irradiation diameter Φ0.21 mm, frequency 500 Hz, and pulse width 10 μs, thereby forming non-through holes ( Figure 1 (F) The non-through holes 13) are then subjected to a desmear treatment using a sodium permanganate aqueous solution at a temperature of 80±5°C and a concentration of 55±10 g / L.
[0127] Furthermore, electroless copper plating is performed to form a plating treatment to a thickness of 0.4 to 0.8 μm, and then electrolytic copper plating is performed to form a plating treatment to a thickness of 8 μm to form a fourth metal layer ( Figure 1(G) The fourth metal layer 14). As a result, the first and third metal layers become electrically connected through the non-through holes through the second metal layer. Next, the entire surface of the fourth metal layer is treated, and a dry film resist (manufactured by Nichigo Morton Co., Ltd., trade name: NIT225) is laminated at a temperature of 110±10°C and a pressure of 0.50±0.02MPa. After that, after attaching a negative mask, the circuit pattern is baked with a parallel exposure machine, and the dry film resist is developed with a 1% sodium carbonate aqueous solution to form an anti-etching layer, and the copper in the portion without the anti-etching layer is removed with an ferric chloride aqueous solution. After that, the dry film resist is removed with an aqueous sodium hydroxide solution, and a pattern is formed on the fourth metal layer to produce a packaging substrate for mounting a semiconductor element ( Figure 1 (I) A semiconductor element mounting package substrate 12 in which wiring conductors 11 are formed on both surfaces of an insulating layer 10 ).
[0128] The obtained semiconductor element mounting package substrate was subjected to solder resist formation and gold plating finishing, and then cut into a package size to obtain a semiconductor element mounting package substrate of Example 1.
[0129] [Example 2]
[0130] In Example 1, a semiconductor element mounting package substrate was obtained in the same manner as in Example 1 except that a prepreg (GHPL-830NSF FF67 manufactured by Mitsubishi Gas Chemical Co., Ltd.; thickness 20 μm) in which bismaleimide triazine resin (BT resin) was impregnated in glass cloth (glass fiber) to form a B-stage was used as the core resin layer 2. It should be noted that the unevenness of the copper foil surface on the peeled side was measured by the same method as in Example 1. The unevenness of the copper foil surface on the peeled side was 1.79 μm.
[0131] [Example 3]
[0132] In Example 1, a semiconductor element mounting package substrate was obtained in the same manner as in Example 1 except that a prepreg (GHPL-830NSF FF74 manufactured by Mitsubishi Gas Chemical Co., Ltd.; thickness 30 μm) in which a bismaleimide triazine resin (BT resin) was impregnated into a glass cloth (glass fiber) to form a B-stage was used as the core resin layer 2. It should be noted that the unevenness of the copper foil surface on the peeled side was measured by the same method as in Example 1. The unevenness of the copper foil surface on the peeled side was 3.15 μm.
[0133] [Example 4]
[0134] In Example 1, a semiconductor element mounting package substrate was obtained in the same manner as in Example 1 except that a prepreg (GHPL-830NSF FF78 manufactured by Mitsubishi Gas Chemical Co., Ltd.; thickness 35 μm) in which a bismaleimide triazine resin (BT resin) was impregnated into a glass cloth (glass fiber) to form a B-stage was used as the core resin layer 2. It should be noted that the unevenness of the copper foil surface on the peeled side was measured by the same method as in Example 1. The unevenness of the copper foil surface on the peeled side was 3.32 μm.
[0135] The semiconductor element mounting packaging substrate of Examples 1 to 4 simultaneously forms a circuit forming substrate (first substrate). Therefore, compared with the comparative example, the production efficiency is good, and there are fewer defective products in laser processing and circuit formation, and the yield is excellent.
[0136] [Comparative Example 2]
[0137] In Example 1, a semiconductor element mounting package substrate was obtained in the same manner as in Example 1 except that a prepreg (GHPL-830NXA manufactured by Mitsubishi Gas Chemical Co., Ltd.; thickness 110 μm) in which bismaleimide triazine resin (BT resin) was impregnated in glass cloth (glass fiber) to form a B-stage was used as the core resin layer 2. It should be noted that the unevenness of the copper foil surface on the peeled side was measured by the same method as in Example 1. The unevenness of the copper foil surface on the peeled side was 6.00 μm, and the resist adhesion in the circuit formation in the subsequent process was reduced, and the yield rate of the product was reduced.
[0138] The entire disclosure of Japanese Patent Application No. 2018-234665 filed on December 14, 2018 is incorporated herein by reference.
[0139] In addition, all documents, patent applications, and technical standards described in the specification are incorporated by reference into the specification to the same extent as if each document, patent application, and technical standard was specifically and individually described as being incorporated by reference.
[0140] Description of Reference Numerals
[0141] 1 circuit forming substrate (first substrate), 2 core resin layer, 3 first metal layer, 4 first insulating resin layer, 5 second metal layer, 6 second insulating resin layer, 7 third metal layer, 8 second substrate, 9 third substrate, 10 insulating layer, 11 wiring conductor, 12 semiconductor element mounting package substrate, 13 non-through hole, 14 fourth metal layer.
Claims
1. A method for manufacturing a semiconductor element mounting package substrate, the method comprising: First substrate forming step (a): forming a laminated body in which a first metal layer, a first insulating resin layer and a second metal layer are sequentially arranged on both sides of a core resin layer having a thickness of 1 μm to 80 μm without heating or pressurizing, and heating and pressurizing the laminated body simultaneously to form a first substrate, wherein the first metal layer has a thickness of 1 μm to 70 μm and can be peeled off from the core resin layer; Patterning step (b): forming a pattern on the second metal layer of the first substrate; A second substrate forming step (c): sequentially disposing a second insulating resin layer and a third metal layer on the surface of the second metal layer of the first substrate to form a laminate, and heating and pressurizing the formed laminate to form a second substrate; and, A peeling step (d) of peeling a third substrate from the core resin layer, the third substrate including the first metal layer, the first insulating resin layer, the second metal layer, the second insulating resin layer, and the third metal layer in this order.
2. The method for manufacturing a semiconductor element mounting package substrate according to claim 1, wherein: It also includes the following wiring conductor forming step (e): forming a non-through hole reaching the surface of the second metal layer on the surface of the third substrate, performing electrolytic copper plating and / or chemical copper plating on the inner wall of the non-through hole to connect the second metal layer to the first metal layer and the third metal layer respectively, forming a fourth metal layer on the surface of the third substrate, and forming a pattern on the fourth metal layer to form the wiring conductor.
3. The method for manufacturing a semiconductor element mounting package substrate according to claim 1 or 2, wherein: The thickness of the third substrate is 5 μm to 100 μm.
4. The method for manufacturing a semiconductor element mounting package substrate according to claim 1 or 2, wherein: The first metal layer includes a release layer, and the first metal layer is arranged in the laminate so that the release layer is in contact with the core resin layer.
5. The method for manufacturing a semiconductor element mounting package substrate according to claim 1 or 2, wherein: The third metal layer includes a carrier layer, and the carrier layer is removed from the third metal layer after the first substrate is heated and pressurized in the second substrate forming step (c).
6. The method for manufacturing a semiconductor element mounting package substrate according to claim 1 or 2, wherein: At least any one of the first metal layer, the second metal layer, and the third metal layer is copper foil.
7. The method for manufacturing a semiconductor element mounting package substrate according to claim 1 or 2, wherein: At least any one of the core resin layer, the first insulating resin layer, and the second insulating resin layer is a prepreg in which a base material is impregnated with a resin.