A method for manufacturing annular oriented aluminum nickel cobalt magnet
By using a double-layer copper tube structure and a pulse power supply to form a ring magnetic field in the preparation of ring magnets, combined with heat treatment and tempering processes, the problems of low ring orientation and cumbersome high-temperature operations are solved, the magnet performance and equipment efficiency are improved, and the energy consumption is reduced. Consumption.
Patent Information
- Application Number
- CN202110676994.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-06-18
AI Technical Summary
Existing ring magnet preparation methods have problems such as low ring orientation and cumbersome high-temperature operations. They also generate serious heat due to large currents, have low efficiency, cannot work for a long time, and have high energy consumption.
DC wires with a double-layer copper tube structure are used for cooling, combined with pulse power for intermittent continuous discharge to form a ring-shaped magnetic field, and ring-oriented AlNiCo magnets are prepared through heat treatment and tempering processes, and quartz tubes and ring-shaped refractory bricks are used for temperature-controlled cooling. , to prevent the magnet from cooling too quickly.
It realizes the preparation of ring-shaped magnets with high ring orientation and easy operation, improves the magnetic properties of the magnets and the efficiency of the equipment, and reduces energy consumption.
Smart Images

Figure CN113393993B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnetic material preparation, and in particular to a method for manufacturing a ring-oriented Al-Ni-Co magnet. Background Art
[0002] The principle of generating a circular magnetic field is that when electric current passes through a straight conductor, the size of the magnetic field is proportional to the size of the current. To allow a large current to pass through the conductor, a larger DC power supply is required, which is converted into a low voltage and large current through a thyristor. This method has the disadvantages of severe heat generation due to large current, inability to work for a long time, and high energy consumption. When operating at high temperatures, the operation is cumbersome and inefficient.
[0003] The existing patent (CN 102021307 B Annular orientation process of heat treatment of annular magnetic steel) discloses a preparation method in which a motor is used to drive the magnetic steel to rotate inside a parallel magnetic field. The disadvantage is that the annular orientation degree of this method is low and the operation is cumbersome under high temperature conditions. Summary of the invention
[0004] In view of the problems existing in the above-mentioned prior art, the object of the present invention is to provide a method for preparing a circularly oriented Al-Ni-Co magnet with high circular orientation degree and convenient operation.
[0005] In order to achieve the above objectives, the following technical solutions are proposed:
[0006] A method for manufacturing a ring-oriented AlNiCo magnet, characterized by comprising the following steps:
[0007] (1) Preparation of the orientation magnetization device: A DC conductor is energized. The structure is two copper tubes nested, including an outer copper tube and an inner copper tube. Cooling water flows through the inner copper tube and water flows out of the outer layer.
[0008] (2) The aluminum-nickel-cobalt magnet is solidified by heat treatment process, the solidification temperature is 1250-1300℃, the solidification time is 10-20 minutes, the furnace is air-cooled for 20-50 seconds, and the annular refractory bricks and quartz tubes are heated to 700-1000℃;
[0009] (3) The heated quartz tube in step (2) is placed on the outer copper tube, the AlNiCo magnet is placed on the quartz tube, the AlNiCo magnet is placed on the outside with the heated annular refractory brick, and then wrapped with insulation material to prevent the AlNiCo magnet from cooling too quickly;
[0010] (4) Turn on the magnetizing power supply, perform intermittent continuous discharge, form a circular magnetic field, and perform temperature-controlled cooling magnetization on the AlNiCo magnet. The magnet is cooled from 1000°C to 600°C, and the insulation time is controlled within 10-30 minutes. After the magnetization is completed, turn off the magnetization power switch;
[0011] (5) The AlNiCo magnet steel is subjected to a tempering process to obtain a ring-oriented AlNiCo magnet product, and the magnetic properties of the product are tested.
[0012] Furthermore, the magnetizing power supply is a pulse power supply, and the pulse power supply is used to perform intermittent continuous discharge.
[0013] Furthermore, the magnetizing power supply has multiple groups of discharge circuits, preferably 4 groups.
[0014] Furthermore, the magnetizing power supply voltage is set to 1000-2500V, the capacitance is 2000uf, the discharge interval is 0.1-2 seconds, and intermittent continuous discharge is performed, and the discharge current is more than 5000A.
[0015] Furthermore, the tempering process in step (5) is to keep the temperature at 630°C for 3 hours, then keep the temperature at 600°C for 6 hours, and then keep the temperature at 570°C for 9 hours.
[0016] Furthermore, the thermal insulation material is silicate wool.
[0017] Furthermore, the number of AlNiCo magnets sleeved on the quartz tube is one or more.
[0018] Furthermore, the energized DC conductor has a structure of two nested copper tubes, including an outer copper tube and an inner copper tube. The inner copper tube passes cooling water and has a water inlet. The outer layer discharges water and has a water outlet. The water outlet and the water inlet are arranged at the same end.
[0019] Furthermore, the heat treatment process of AlNiCo magnet is as follows: preheating temperature 800-1000℃, time 10-20 minutes, solution temperature 1250℃-1300℃, solution time 10-20 minutes, air cooling for 20-50 seconds, then temperature controlled cooling with annular refractory material, applying magnetic field at 1000℃-600℃, cooling time 10-30 minutes, tempering process 630℃*3h+600℃*6h+570℃*9h.
[0020] Furthermore, in the step (5), the heat-treated product is subjected to a magnetic property test. Specifically, the product is first cut into a square along the circumferential tangent direction, and then the square is tested. The magnetic properties obtained are as follows: Br: 11930Gs, Hcb: 650Oe, BHm: 4.15 MGOes; Br: 12080Gs, Hcb: 658Oe, BHm: 4.42MGOes.
[0021] Compared with the prior art, the method for manufacturing a ring-shaped oriented AlNiCo magnet of the present invention has the following beneficial effects:
[0022] 1. Use pulse power supply to generate high voltage, large current, continuous discharge, and obtain sustainable toroidal magnetic field;
[0023] 2. The DC conductor adopts a double-layer structure, with cooling water flowing through the inner layer and water flowing out through the outer layer. The water outlet and water inlet are at the same end, which is convenient for operation;
[0024] 3. During heat treatment cooling, use copper tubes covered with quartz tubes and magnets covered with insulation materials to prevent the aluminum-nickel-cobalt magnets from cooling too quickly, achieving better results. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic cross-sectional view of the structure of the orientation magnetization device of the present invention.
[0026] In the figure: 1. outer copper tube; 2. inner copper tube; 3. Al-Ni-Co magnet; 4. annular refractory material; 5. quartz tube; 6. thermal insulation material; 7. water inlet; 8. water outlet. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited thereto.
[0028] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or apparatus.
[0029] The magnetism of aluminum-nickel-cobalt permanent magnet alloy is generated during the heat treatment process. The process is to apply an oriented magnetic field during the heat treatment process and perform temperature-controlled cooling. The method adopted in the process of the present invention is that its principle is also the principle that a large current passes through a straight wire to generate a circular magnetic field. In order to avoid the shortcomings of the prior art, a pulse power supply is used for intermittent discharge. The pulse power supply generates a high voltage to generate a large current through the wire to form a circular magnetic field.
[0030] Example 1 This example takes 3 groups of Al-Ni-Co magnets
[0031] A method for manufacturing a ring-oriented AlNiCo magnet comprises the following steps:
[0032] (1) Preparation of the orientation magnetization device: The current-carrying conductor adopts a double copper tube nested structure, including an outer copper tube 1 and an inner copper tube 2. The inner copper tube 2 passes cooling water and has a water inlet 7. The outer layer discharges water and has a water outlet 8. The water inlet 7 and the water outlet 8 are arranged at the same end for easy operation.
[0033] (2) The aluminum nickel cobalt magnetic steel 3 is subjected to a heat treatment process, with a preheating temperature of 800°C for 20 minutes, followed by a solid solution treatment process, with a solid solution temperature of 1250°C for 20 minutes, followed by air cooling for 20 seconds, and the annular refractory brick 4 and the quartz tube 5 are heated to 1000°C;
[0034] (3) Use pliers to put the quartz tube 5 heated in step 2 onto the outer copper tube 1, and then put the AlNiCo magnet 3 onto the quartz tube 5. The AlNiCo magnet 3 is covered with the heated annular refractory brick 4, and then wrapped with insulation material 6 for insulation to prevent the AlNiCo magnet 3 from cooling too quickly. In this embodiment, the insulation material 6 is silicate wool.
[0035] (4) Turn on the magnetizing power supply, perform intermittent continuous discharge, and form a circular magnetic field. The magnetizing power supply of this embodiment is a pulse power supply, and the pulse power supply is used for intermittent continuous discharge. The magnetizing power supply has multiple sets of discharge circuits. The magnetizing power supply of this embodiment preferably has 4 sets of discharge circuits. The magnetizing voltage is set to 1000V, the capacitance is 2000uf, the discharge interval is 0.1 second, and intermittent continuous discharge is performed. The discharge current is more than 5000A.
[0036] The AlNiCo magnet 3 is subjected to temperature-controlled cooling and magnetization with refractory materials, and the magnet is cooled from 1000°C to 600°C. The cooling time is controlled within 10 minutes. After the magnetization is completed, the magnetization power switch is turned off;
[0037] (5) The AlNiCo magnet 3 is subjected to a tempering process. The specific tempering process is: keep at 630°C for 3 hours, then keep at 600°C for 6 hours, and then keep at 570°C for 9 hours. After the tempering is completed and cooled, a ring-oriented AlNiCo magnet product is obtained, and the magnetic properties of the product are tested.
[0038] Example 2 This example takes 5 groups of Al-Ni-Co magnets.
[0039] A method for manufacturing a ring-oriented AlNiCo magnet comprises the following steps:
[0040] (1) Preparation of the orientation magnetization device: The current-carrying conductor adopts a double copper tube nested structure, including an outer copper tube 1 and an inner copper tube 2. The inner copper tube 2 passes cooling water and has a water inlet 7. The outer layer discharges water and has a water outlet 8. The water inlet 7 and the water outlet 8 are arranged at the same end for easy operation.
[0041] (2) The aluminum nickel cobalt magnetic steel 3 is subjected to a heat treatment process, with a preheating temperature of 1000°C for 10 minutes, followed by a solid solution treatment process, with a solid solution temperature of 1300°C for 10 minutes, and then air-cooled for 50 seconds after being taken out of the furnace. The annular refractory brick 4 and the quartz tube 5 are heated to 700°C;
[0042] (3) Use pliers to put the quartz tube 5 heated in step 2 onto the outer copper tube 1, and then put the AlNiCo magnet 3 onto the quartz tube 5. The AlNiCo magnet 3 is covered with the heated annular refractory brick 4, and then wrapped with insulation material 6 for insulation to prevent the AlNiCo magnet 3 from cooling too quickly. In this embodiment, the insulation material 6 is silicate wool.
[0043] (4) Turn on the magnetizing power supply, perform intermittent continuous discharge, and form a circular magnetic field. The magnetizing power supply of this embodiment is a pulse power supply, and the pulse power supply is used for intermittent continuous discharge. The magnetizing power supply has multiple sets of discharge circuits. The magnetizing power supply of this embodiment preferably has 4 sets of discharge circuits. The magnetizing voltage is set to 1000V, the capacitance is 2000uf, the discharge interval is 2 seconds, and intermittent continuous discharge is performed. The discharge current is more than 5000A.
[0044] The AlNiCo magnet 3 is subjected to temperature-controlled cooling and magnetization with refractory materials, and the magnet is cooled from 1000°C to 600°C. The cooling time is controlled within 30 minutes. After the magnetization is completed, the magnetization power switch is turned off;
[0045] (5) The AlNiCo magnet 3 is subjected to a tempering process. The specific tempering process is: keep at 630°C for 3 hours, then keep at 600°C for 6 hours, and then keep at 570°C for 9 hours. After the tempering is completed and cooled, a ring-oriented AlNiCo magnet product is obtained, and the magnetic properties of the product are tested.
[0046] The magnetic properties of the heat-treated products were tested. Specifically, the product was first cut into a square along the circumferential tangent direction, and then the square was tested. The magnetic properties obtained were as follows: Br: 11930Gs, Hcb: 650Oe, BHm: 4.15MGOes; Br: 12080Gs, Hcb: 658Oe, BHm: 4.42MGOes.
Claims
1. A method for manufacturing a ring-oriented AlNiCo magnet, characterized in that: The steps include: (1) Preparation of an orientation magnetization device: A DC conductor is energized, and the structure is two copper tubes nested, including an outer copper tube (1) and an inner copper tube (2). The inner copper tube (2) passes cooling water and has a water inlet (7). The outer layer discharges water and has a water outlet (8). The water inlet (7) and the water outlet (8) are arranged at the same end; (2) Aluminum-nickel-cobalt magnet (3) is solid-solutionized by heat treatment process, the solid-solution temperature is 1250-1300°C, the solid-solution time is 10-20 minutes, the furnace is air-cooled for 20-50 seconds, and the annular refractory brick (4) and the quartz tube (5) are heated to 700-1000°C; (3) The quartz tube (5) heated in step (2) is placed on the outer copper tube (1), the AlNiCo magnet (3) is placed on the quartz tube (5), the AlNiCo magnet (3) is covered with the heated annular refractory brick (4), and then wrapped with a heat-insulating material (6) for heat preservation to prevent the AlNiCo magnet (3) from cooling too quickly; (4) Turn on the magnetizing power supply, perform intermittent continuous discharge, form a circular magnetic field, and perform temperature-controlled cooling magnetization on the AlNiCo magnet (3), the magnet is cooled from 1000°C to 600°C, and the insulation time is controlled within 10-30 minutes. After the magnetization is completed, turn off the magnetization power switch; (5) The AlNiCo magnet (3) is subjected to a tempering process to obtain a ring-oriented AlNiCo magnet product, and the magnetic properties of the product are tested; The magnetizing power supply is a pulse power supply, and the pulse power supply is used for intermittent continuous discharge; the magnetizing power supply voltage is set to 1000-2500V, the capacitance is 2000uf, the discharge interval is 0.1-2 seconds, and intermittent continuous discharge is performed, and the discharge current is more than 5000A; The tempering process in step (5) is to keep the temperature at 630°C for 3 hours, then keep the temperature at 600°C for 6 hours, and then keep the temperature at 570°C for 9 hours.
2. The method for manufacturing a ring-shaped oriented AlNiCo magnet according to claim 1, characterized in that: The magnetizing power supply has 4 groups of discharge circuits.
3. The method for manufacturing a ring-shaped oriented AlNiCo magnet according to claim 1, characterized in that: The thermal insulation material (6) is silicate wool.
4. The method for manufacturing a ring-shaped oriented AlNiCo magnet according to claim 1, characterized in that: The aluminum nickel cobalt magnet (3) sleeved on the quartz tube (5) is provided in one or more pieces.
5. The method for manufacturing a ring-shaped oriented AlNiCo magnet according to claim 1, characterized in that: The heat treatment process of AlNiCo magnet (3) is as follows: preheating temperature 800-1000°C, time 10-20 minutes, solution temperature 1250°C-1300°C, solution time 10-20 minutes, air cooling for 20-50 seconds after exiting the furnace, then temperature controlled cooling with annular refractory material, applying magnetic field at 1000°C-600°C, cooling time 10-30 minutes, tempering process 630°C*3h+600°C*6h+570°C*9h.
6. The method for manufacturing a ring-shaped oriented AlNiCo magnet according to claim 1, characterized in that: In the step (5), the heat-treated product is subjected to a magnetic property test. Specifically, the product is first cut into a square along the circumferential tangent direction, and then the square is tested. The magnetic properties obtained are as follows: Br: 11930Gs, Hcb: 650Oe, BHm: 4.15MGOes; Br: 12080Gs, Hcb: 658Oe, BHm: 4.42MGOes.