Polymer, semiconductor composition containing polymer, and method for producing film using semiconductor composition

By using a semiconductor composition composed of a polymer with specific structural units to form a film on a substrate, the problem of photoresist pattern dimensional accuracy and low yield is solved, and high-quality low-temperature film formation and complex substrate embedding are achieved. The shape of the resist pattern and the yield are improved.

CN113454131BActive Publication Date: 2024-10-29MERCK PATENT GMBH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202080015180.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-02-17
Publication Date
2024-10-29
Estimated Expiration
2040-02-17

AI Technical Summary

Technical Problem

In the manufacturing process of semiconductor devices, the dimensional accuracy of photoresist patterns is affected by the reflection of light from the substrate and the random reflection of exposure light, resulting in inaccurate dimensions and low yield. The existing anti-reflective film technology cannot meet the requirements of complex substrate embedding and low-temperature formation. membrane requirements.

Method used

A semiconductor composition composed of a polymer containing specific structural units is used to form a film by applying the composition on a substrate and heating to reduce sublimation, improve corrosion resistance and coating properties, and form a film with large absorbance and Films with optimized refractive index reduce standing waves and mixing, improving resist pattern shape and yield.

Benefits of technology

It achieves the formation of high-quality resist films at low temperatures, improves the embeddability and yield of complex substrates, reduces standing waves and mixing, enhances the flatness and storage stability of the film, and reduces the generation of sublimates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003217457270000021
    Figure BDA0003217457270000021
  • Figure BDA0003217457270000031
    Figure BDA0003217457270000031
  • Figure BDA0003217457270000041
    Figure BDA0003217457270000041
Patent Text Reader

Abstract

Provided are novel polymers that can reduce sublimates when forming a film and compositions containing the polymers. The polymer (A) according to the present invention comprises at least one structural unit selected from the group consisting of unit (a), unit (b), unit (c) and unit (d) described below, and the number of repetitions of each of the units (a), (b), (c) and (d) is a 、n b 、n c and n d Satisfies the following formula: n a +n b >0, nc≥0 and nd≥0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer containing a specific structural unit and a semiconductor composition containing the polymer. In addition, the present invention relates to a film using the semiconductor composition and a method for producing a device. Background Art

[0002] In the manufacturing process of semiconductor devices, micro-processing is usually performed by photolithography using photoresists. The micro-processing process is to form a thin photoresist layer on a semiconductor substrate such as a silicon wafer, cover the layer with a mask pattern corresponding to the pattern of the device to be used for the layer, expose the layer to active light such as ultraviolet rays through the mask pattern, develop the exposed layer to obtain a photoresist pattern, and etch the substrate using the obtained photoresist pattern as a protective film, thereby forming fine concavo-convex corresponding to the above pattern.

[0003] In these photolithography processes, the influence of standing waves caused by the reflection of light from the substrate and the influence of random reflection of exposure light caused by the step difference of the substrate lead to the problem of reduced dimensional accuracy of the photoresist pattern. Therefore, in order to solve this problem, the method of setting a lower anti-reflection film has been widely discussed. As the characteristics required of such a lower anti-reflection film, it can be listed that: it has a large absorbance to the radiation used for exposure of the photoresist, prevents random reflection, etc. so that the cross section of the photoresist after exposure and development is perpendicular to the substrate surface, and has poor solubility in the solvent contained in the photoresist composition (not easy to mix), etc.

[0004] Patent Document 1 discloses an antireflection coating composition containing a crosslinking agent. Patent Document 2 discloses a fine resist pattern forming composition containing a specific polymer, but does not describe whether an underlayer antireflection film can be formed or whether the composition has the required properties as an underlayer antireflection film.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent document 1: International Publication No. 2011 / 101737

[0008] Patent Document 2: Japanese Patent Application Publication No. 2014-71424

[0009] Patent document 3: International Publication No. 2007 / 111147 Summary of the invention

[0010] Problems to be solved by the invention

[0011] The inventors believe that there are more than one problem to be improved. For example, they can be listed as follows: reduction of sublimation products; suitable corrosion resistance; spreadability; embeddability in complex and fine substrates (for example, step-shaped substrates); ability to form films at low temperatures; large absorbance; suitable refractive index; reduction of standing waves; reduction of mixing with other compositions (for example, resist compositions) or films; flat upper surface of the formed film; high solubility of solutes; storage stability; good shape of the formed resist pattern and high yield: low LWR.

[0012] The present invention has been accomplished based on the above technical background, and provides a novel polymer and a composition containing the same.

[0013] Means for solving problems

[0014] The polymer (A) of the present invention comprises at least one structural unit selected from the group consisting of the following units (a), (b), (c) and (d):

[0015] Unit (a) represented by formula (a):

[0016]

[0017] (In formula (a), R a1 and R a2 H, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH,

[0018] L a For a single bond, C 1-5 Alkylene, -O-, or C 1-5 Alkyleneoxy,

[0019] ma is 0 to 1,

[0020] X a1 H or C 1-5 Hydrocarbon (C 1-5 One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the hydrocarbon group may be independently replaced by -NH2 and / or -COOH).

[0021] Y a is N or O, where Y a When N is pa, it is an integer of 1 or 2, Y a When it is O, pa is 1.

[0022] X a2 H or C 1-5 Hydrocarbon (C 1-5One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the hydrocarbon group may be replaced by -NH2 and / or -COOH, respectively. When pa is 2, two X a2 Can be the same or different,

[0023] Among them, it can also be X a1 With X a2 bonding, and / or 2 x when pa is 2 a2 bonding to form a saturated or unsaturated ring);

[0024] Unit (b) represented by formula (b):

[0025]

[0026] (In formula (b),

[0027] R b1 and R b2 H, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Alkoxyalkyl, or -COOH,

[0028] mb is 0 to 1,

[0029] L b For a single bond, C 1-5 Alkylene, C 6-20 Arylene, -O-, or C 1-5 Alkyleneoxy,

[0030] Z b C 6-20 Aromatic hydrocarbons or C 7-20 Aromatically substituted aliphatic hydrocarbons,

[0031] pb is 0 to 4,

[0032] qb is 1 to 3,

[0033] R b3 H, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Alkoxyalkyl, or -COOH, when pb>1, each R b3 Can be the same or different,

[0034] R b4 is H or methyl, when qb>1, each R b4 Can be the same or different,

[0035] wherein unit (b) comprises an aromatic group containing at least one condensed structure);

[0036] Unit (c) represented by formula (c):

[0037]

[0038] (In formula (c),

[0039] R c1 and R c2 H, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH,

[0040] mc is 0 to 1,

[0041] L c For a single bond, C 1-5 Alkylene, -O-, or C 1-5 Alkyleneoxy,

[0042] V c is a condensed aromatic hydrocarbon or a condensed heterocyclic ring, V c It is formed by condensation of 3 to 6 rings.

[0043] pc is 0 to 5,

[0044] R c3 C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH, when pc>1, each R c3 may be the same or different); and

[0045] The unit (d) represented by the following formula (d):

[0046]

[0047] (In formula (d),

[0048] R d1 and R d2 H, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH,

[0049] md is 0 to 1,

[0050] L d For a single bond, C 1-5 Alkylene (C 1-5 One or more -CH2- in the alkylene group may be replaced by -NH-, -C(=O)- and / or -O-, and C 1-5One or more -CH3 in the alkylene group may be replaced by -OH, -NH2 and / or -COOH), -O-, or C 1-5 alkyleneoxy),

[0051] The number of repetitions of units (a), (b), (c) and (d) are n respectively. a 、n b 、n c and n d , which satisfies the following formula:

[0052] n a +n b >0,n c ≥0, and n d ≥0.

[0053] The semiconductor composition of the present invention contains the above-mentioned polymer (A) and a solvent (B).

[0054] The method for producing the film of the present invention comprises the following steps:

[0055] (1) applying the semiconductor composition of the present invention onto a substrate; and

[0056] (2) The semiconductor composition is heated to form a film.

[0057] The method for manufacturing the device of the present invention includes the method described above.

[0058] Effects of the Invention

[0059] Sublimates can be reduced. Corrosion resistance can be controlled. A composition with good coating properties can be obtained. The composition can be well embedded in a complex and fine substrate (e.g., a stepped substrate). A film can be formed at a low temperature. A film with a large absorbance can be obtained. A film with a preferred refractive index can be obtained. Standing waves can be reduced. Mixing with other compositions (e.g., resist compositions) or films can be reduced. The flatness of the upper surface of the formed film can be improved. A composition with high solute solubility can be obtained. A composition with high storage stability can be obtained. A resist pattern with a good shape can be formed with a high yield. A pattern with a low LWR can be formed. DETAILED DESCRIPTION

[0060] In this specification, unless otherwise specified, the singular form includes the plural form, and "one" or "it" means "at least one". In this specification, unless otherwise specified, some conceptual elements may be embodied in multiple types, and if the amount (such as mass % or mole %) is described, the amount means the sum of multiple types.

[0061] "And / or" includes all combinations of elements and also includes individual uses.

[0062] In the present specification, when "~" or "-" is used to indicate a numerical range, unless otherwise specified, they include both endpoints and the units are common. For example, 5 to 25 mol% means 5 mol% or more and 25 mol% or less.

[0063] In this manual, “C x-y ”, “C x ~C y ” and “C x " etc. indicates the number of carbon atoms in a molecule or a substituent. For example, C 1-6 The alkyl group represents an alkyl chain having 1 to 6 carbon atoms (such as methyl, ethyl, propyl, butyl, pentyl, and hexyl).

[0064] In this specification, if a polymer has multiple repeating units, these repeating units are copolymerized. Unless otherwise specified, these copolymerizations may be alternating copolymerizations, random copolymerizations, block copolymerizations, graft copolymerizations, or mixtures thereof. When a polymer or resin is represented by a structural formula, n or m, etc., recorded in brackets, indicates the number of repetitions.

[0065] In this specification, unless otherwise specified or mentioned, the temperature unit is Celsius. For example, 20 degrees means 20 degrees Celsius.

[0066] Polymer (A)

[0067] The polymer (A) according to the present invention comprises at least one structural unit selected from the group consisting of unit (a), unit (b), unit (c) and unit (d) described below, and the respective repetition numbers n of units (a), (b), (c) and (d) are a 、n b 、n c and n d Satisfies the following formula: n a +n b >0,n c ≥0 and n d ≥0, preferably n a >0.

[0068] The unit (a) is represented by the formula (a).

[0069]

[0070] In formula (a),

[0071] R a1 and R a2 H, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH,

[0072] L a For a single bond, C 1-5 Alkylene, -O-, or C 1-5 Alkyleneoxy,

[0073] ma is 0 to 1,

[0074] X a1 H or C 1-5 Hydrocarbon (C 1-5 One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the hydrocarbon group may be independently replaced by -NH2 and / or -COOH).

[0075] Y a is N or O, where Y a When N is N, pa is an integer of 1 or 2, Y a When it is O, pa is 1.

[0076] X a2 H or C 1-5 Hydrocarbon (C 1-5 One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the hydrocarbon group may be replaced by -NH2 and / or -COOH, respectively. When pa is 2, two X a2 Can be the same or different,

[0077] Among them, it can also be X a1 With X a2 bonding, and / or when pa is 2, 2 X a2 bonded to form a saturated or unsaturated ring.

[0078] The unit (a) introduced as a pendant is considered to be cross-linkable per se. Therefore, when a film is formed using a composition containing the polymer (A), a cross-linked polymer can be formed even without containing a cross-linking agent.

[0079] R a1 It is preferably H, methyl, ethyl, t-butyl or methoxy, more preferably H or methyl, and even more preferably H.

[0080] R a2 It is preferably H, methyl, ethyl, t-butyl or methoxy, more preferably H or methyl, and further preferably methyl.

[0081] L aPreferred is a single bond, methylene, vinyl, propenyl, -O- or methyleneoxy (methoxylene), more preferred is methylene or vinyl, and more preferred is methylene.

[0082] ma is preferably 0 or 1, more preferably 1. The polymer (A) may have a plurality of types of units (a), but in this case, the number may be a non-integer number, for example, ma = 0.5. Hereinafter, the numbers in the formula of the polymer are the same unless they are explicitly integers.

[0083] Y a Preferably, it is N, and pa is preferably 2. As another form, Y a is N, and pa is 1, but at this time N and X a2 It is a double bond (-N=X a2 ).

[0084] X a1 C 1-5 The hydrocarbon group may be a straight chain or a branched chain. a1 Preferred is H, methyl, ethyl or propyl, and more preferred is H.

[0085] X a2 C 1-5 The hydrocarbon groups may be independently straight chain or branched. a2 Each independently preferably is C 1-5 Hydrocarbon (C 1-5 One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, and C 1-5 One or more -CH3 in the hydrocarbon group may be independently replaced by -NH2).

[0086] It is preferred that formula (a) is represented by the following formula (a-1).

[0087]

[0088] In formula (a),

[0089] R a1 , R a2 , L a , ma, and X a1 As mentioned above, X a3 and X a4 are independently H, or C 1-5 Hydrocarbon (C 1-5 One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the hydrocarbon group may be independently replaced by -NH2 and / or -COOH),

[0090] Among them, it can also be X a1 With X a3 or X a4 Bonding, and / or X a3 With X a4 bonded to form a saturated or unsaturated ring.

[0091] X a3 and X a4 C 1-5 The hydrocarbon groups may be independently straight chain or branched. a3 and X a4 Each independently preferably is C 1-5 Hydrocarbon (C 1-5 One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, and C 1-5 One or more -CH3 in the hydrocarbon group may be independently replaced by -NH2).

[0092] X a1 With X a3 or X a4 Preferably no ring is formed. a3 With X a4 When forming a ring, it is preferably a 5- to 7-membered ring, in which one or two atoms among the atoms constituting the ring are nitrogen atoms and the remaining atoms are carbon atoms.

[0093] X a3 With X a4 When no ring is formed, X a3 With X a4 Each is independently H, methyl or ethyl, more preferably H or methyl. A preferred form is X a3 and X a4 Any one of them is methyl.

[0094] Specific examples of formula (a-1) are as follows.

[0095]

[0096] In addition, formula (a) may be represented by formula (a-2).

[0097]

[0098] In formula (a-2), R a1 , R a2 , L a , ma, and X a1 As mentioned above, X a5 C 1-5 Hydrocarbon (C 1-5One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the hydrocarbon group may be independently replaced by -NH2 and / or -COOH),

[0099] Among them, it can also be X a1 With X a5 bond to form a saturated or unsaturated ring. a1 With X a5 No ring is formed.

[0100] X a5 C 1-5 The hydrocarbon group may be a straight chain or a branched chain, preferably a branched chain. a5 C 1-4 Hydrocarbon, C 1-4 The -CH2- in the hydrocarbon group is not replaced by -NH-, -C(=O)-, and -O-, and C 1-4 The -CH3 in the hydrocarbon group is not replaced by -NH2 and -COOH.

[0101] Specific examples of formula (a-2) are as follows.

[0102]

[0103] In addition, formula (a) may be represented by formula (a-3).

[0104]

[0105] In formula (a-3), R a1 , R a2 , L a , ma, and X a1 As mentioned above, X a6 C 1-5 Hydrocarbon (C 1-5 One or more -CH2- in the hydrocarbon group may be independently replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the hydrocarbon group may be independently replaced by -NH2 and / or -COOH),

[0106] Among them, it can also be X a1 With X a6 bonded to form a saturated or unsaturated ring.

[0107] X a6 Preferred examples include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and a tert-butyl group, and more preferred examples include a methyl group and an n-propyl group.

[0108] Specific examples of formula (a-3) are as follows.

[0109]

[0110] The unit (b) is represented by the formula (b).

[0111]

[0112] In formula (b),

[0113] R b1 and R b2 H, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Alkoxyalkyl, or -COOH,

[0114] mb is 0 to 1,

[0115] L b For a single bond, C 1-5 Alkylene, C 6-20 Arylene, -O-, or C 1-5 Alkyleneoxy,

[0116] Z b C 6-20 Aromatic hydrocarbons or C 7-20 Aromatically substituted aliphatic hydrocarbons,

[0117] pb is 0 to 4,

[0118] qb is 1 to 3,

[0119] R b3 H, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Alkoxyalkyl, or -COOH, when pb>1, each R b3 Can be the same or different,

[0120] R b4 is H or methyl, when qb>1, each R b4 Can be the same or different,

[0121] Among them, it can be said that the unit (b) contains at least one condensed aromatic group. The unit (b) contains at least one condensed cyclic hydrocarbon. Such a condensed cyclic hydrocarbon is preferably naphthyl or anthracene.

[0122] As R b1 , preferably H, methyl, ethyl, or tert-butyl, more preferably H.

[0123] As R b2, preferably H, methyl, ethyl, or tert-butyl, more preferably H or methyl, further preferably methyl.

[0124] mb is preferably 0 or 1, more preferably 1.

[0125] Lb is preferably a single bond, methylene, vinyl, propenyl, naphthalene, anthracenylene, -O-, methoxylene or ethoxylene, more preferably a single bond, methylene or naphthalene, further preferably a single bond or naphthalene, and further preferably a single bond.

[0126] R b3 Preferably, it is H, methyl, ethyl, propyl, methoxy, or methoxymethyl, more preferably H, methyl, or methoxymethyl, further preferably H or methoxymethyl, and further preferably H. pb is preferably 0 to 3, more preferably 0 to 2, further preferably 0 or 1, and further preferably 0. When pb=0, it can be said that R b3 In fact, it is H. To ensure clarity, when pb = 0, R b3 ≠H is also acceptable.

[0127] R b4 It is preferably H. qb is preferably 1 to 2, more preferably 1 or 2, and even more preferably 1.

[0128] By having the unit (b), the film formed by the polymer (A) is considered to have a preferred refractive index (n). Therefore, the polymer (A) having the unit (b) is useful for the resist lower layer film forming composition, and is more useful for the lower layer antireflection film forming composition. In addition, it is also useful for the upper layer antireflection film forming composition.

[0129] It should be noted that the following structure is an example of unit (b), in which case: in the above formula (b), R b1 and R b2 is H, mb is 1,

[0130] L b and Z b They are the following structures respectively,

[0131] pb is 4, qb is 2,

[0132] R b3 All are -CH2-O-CH3,

[0133] R b4 All are H.

[0134]

[0135] Z bPreferably, Z is a benzene ring, a naphthalene ring, an anthracene ring, diphenylmethyl ester, diphenylethyl ester, or phenylnaphthyl ester. b It is a naphthalene ring.

[0136] The unit (b) can also be represented by the following formula (b-1).

[0137]

[0138] In formula (b-1),

[0139] R b1 , R b2 mb,L b , pb, qb, R b3 and R b4 Each independently as described above.

[0140] Specific examples of formula (b-1) are as follows.

[0141]

[0142] As formula (b-1), the following is more preferable.

[0143]

[0144] The unit (c) is represented by the formula (c).

[0145]

[0146] In formula (c),

[0147] R c1 and R c2 H, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH,

[0148] mc is 0 to 1,

[0149] L c For a single bond, C 1-5 Alkylene, -O-, or C 1-5 Alkyleneoxy,

[0150] V c is a condensed aromatic hydrocarbon or a condensed heterocyclic ring, V c It is formed by condensation of 3 to 6 rings.

[0151] pc is 0 to 5,

[0152] R c3 C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH, when pc>1, each R c3Can be the same or different.

[0153] As R c1 , preferably H, methyl, or ethyl, more preferably H.

[0154] As R c2 , preferably H, methyl, or ethyl, more preferably H or methyl, further preferably methyl.

[0155] As L c , preferably a single bond, methylene, ethenyl, propenyl, -O-, or methoxylene, more preferably a single bond or methylene, further preferably a methylene.

[0156] mc is preferably 0 or 1, more preferably 1.

[0157] R c3 It is preferably H, methyl or ethyl, more preferably H or methyl, and still more preferably H.

[0158] pc is preferably 0, 1, 2, 3, 4, or 5, more preferably 0, 1, or 2, further preferably 0 or 1, and further preferably 0. When pc=0, it can be said that R c3 In fact, it is H. To ensure clarity, when pc = 0, R c3 ≠H is also acceptable.

[0159] By having unit (c), it is believed that the film formed by polymer (A) can show preferred absorption parameter (k) and refractive index (n). For example, it can be believed that the (k) value and / or (n) value can be increased. Therefore, polymer (A) having unit (c) is useful for resist lower film forming composition, and is more useful for lower anti-reflection film forming composition. In addition, it is also useful for upper anti-reflection film forming composition.

[0160] V c An anthracene derivative, a phenanthrene derivative or a xanthene derivative is preferred, an anthracene derivative or a phenanthrene derivative is more preferred, and an anthracene derivative is further preferred.

[0161] Preferably, formula (c) is represented by the following formula (c-1) or (c-2).

[0162]

[0163] In formula (c-1), R c1 , R c2 , R c3 , L c and mc are independently as described above.

[0164] Belong to V cOne carbon in the anthracene may be substituted with oxygen, but unsubstituted form is more preferred.

[0165]

[0166] In formula (c-2), R c1 , R c2 , R c3 , L c and mc are independently as described above.

[0167] One carbon in phenanthrene may be substituted with oxygen, but unsubstituted form is more preferred.

[0168] R c3 C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH, when pc" is 2, 3, 4, or 5, each R c3 Can be the same or different, or can be 2 R c3 A saturated ring or an unsaturated ring is formed.

[0169] Specific examples of formula (c-1) are as follows.

[0170]

[0171] Specific examples of formula (c-2) are as follows.

[0172]

[0173] Specific examples of formula (c) other than the above-mentioned specific examples are as follows.

[0174]

[0175] The unit (d) is represented by the formula (d).

[0176]

[0177] In formula (d),

[0178] R d1 and R d2 H, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH, md is 0 to 1,

[0179] L d For a single bond, C 1-5 Alkylene (C 1-5 One or more -CH2- in the alkylene group may be replaced by -NH-, -C(=O)- and / or -O-, and C 1-5One or more -CH3 in the alkylene group may be replaced by -OH, -NH2 and / or -COOH), -O-, or C 1-5 Alkylene oxide.

[0180] As R d1 , preferably H, methyl, ethyl, tert-butyl or methoxy, more preferably H or methyl, further preferably H.

[0181] As R d2 , preferably H, methyl, ethyl, tert-butyl or methoxy, more preferably H or methyl, further preferably methyl.

[0182] Md is preferably 0 or 1, more preferably 1.

[0183] L d Preferably C 1-5 Alkylene (C 1-5 One or more -CH2- in the alkylene group may be replaced by -C(=O)-, and C 1-5 More than one -CH3 in the alkylene group may be replaced by -OH and / or -COOH), more preferably C 1-4 Alkylene (C 1-4 One or more -CH2- in the alkylene group may be replaced by -C(=O)-, and C 1-4 More than one -CH3 in the alkylene group may be replaced by -OH and / or -COOH), and more preferably C 1-4 Alkylene (C 1-4 One -CH2- in the alkylene group may be replaced by -C(=O)-, and C 1-4 One -CH3 in the alkylene group may also be replaced by -OH and / or -COOH).

[0184] It is believed that by having unit (d), the film formed by polymer (A) can show a preferred absorption parameter (k), a refractive index (n) or a fast etching rate. In addition, unit (d) can also be used as a crosslinking position when forming a film, and can contribute to film formation and crosslinking. Therefore, polymer A) having unit (d) is useful for resist lower film forming composition, and is more useful for lower anti-reflection film forming composition. In addition, it is also useful for upper anti-reflection film forming composition.

[0185] Specific examples of formula (d) are as follows.

[0186]

[0187] In polymer (A), the number of repetitions of units (a), (b), (c) and (d) is n respectively. a 、n b 、nc and n d Satisfies the following formula: n a +n b >0,n c ≥0, and n d ≥0.

[0188] n a / (n a +n b +n c +n d ) is preferably 2 to 80%, more preferably 5 to 50%, further preferably 10 to 50%, and further preferably 20 to 40%.

[0189] n b / (n a +n b +n c +n d ) is preferably 10 to 90%, more preferably 20 to 80%, further preferably 30 to 80%, and further preferably 25 to 60%.

[0190] n c / (n a +n b +n c +n d ) is preferably 3 to 80%, more preferably 5 to 40%, further preferably 5 to 50%, and further preferably 8 to 20%.

[0191] n d / (n a +n b +n c +n d ) is preferably 0 to 80%, more preferably 0 to 40%, further preferably 5 to 30%, and further preferably 10 to 30%.

[0192] Preferably, they satisfy the following formula:

[0193] 5%≤n a / (n a +n b +n c +n d )≤50%,30%≤n b / (n a +n b +n c +n d )≤80%,5%≤n c / (n a +n b +n c +nd )≤40%, and / or 0%≤n d / (n a +n b +n c +n d )≤40%.

[0194] Preferably, the total number of all repeating units contained in the polymer (A) is n total Satisfies the following formula:

[0195] 80%≤(n a +n b +n c +n d ) / n total ≤100%.

[0196] More preferably, the following formula is satisfied:

[0197] 90%≤(n a +n b +n c +n d ) / n total ≤100%.

[0198] More preferably, the following formula is satisfied:

[0199] 95%≤(n a +n b +n c +n d ) / n total ≤100%.

[0200] (n a +n b +n c +n d ) / n total = 100%, that is, no n a 、n b 、n c 、n d Repeating units other than these are also a preferred embodiment of the present invention.

[0201] The mass average molecular weight (hereinafter, sometimes referred to as Mw) of the polymer (A) is preferably 1,000 to 50,000, more preferably 3,000 to 40,000, and further preferably 5,000 to 20,000.

[0202] The number average molecular weight (hereinafter, sometimes referred to as Mn) of the polymer (A) is preferably 1,000 to 50,000, more preferably 5,000 to 10,000.

[0203] In the present invention, Mw and Mn can be measured by gel permeation chromatography (GPC). In this measurement, a preferred example is to set the GPC column to 40 degrees Celsius, set the elution solvent tetrahydrofuran to 0.6 mL / min, and use monodisperse polystyrene as a standard.

[0204] The synthesis method of the polymer (A) according to the present invention is not particularly limited, and specific examples are described in the synthesis examples described below. Known synthesis methods can also be combined with the synthesis examples.

[0205] <Semiconductor composition>

[0206] Here, in the present invention, the semiconductor composition refers to a composition used in a semiconductor manufacturing process, more preferably used in a photolithography process. The semiconductor composition according to the present invention is preferably a composition for semiconductor manufacturing. The semiconductor composition according to the present invention can also be removed by a semiconductor manufacturing process and ultimately does not remain in the semiconductor. The semiconductor composition is preferably a resist underlayer film composition, more preferably a lower anti-reflective film composition. Here, the resist underlayer film and the lower anti-reflective film are formed above the substrate and below the resist film. The resist underlayer film or the lower anti-reflective film can be formed in contact with the substrate or the resist film, or can be formed through an intermediate layer.

[0207] The content of the polymer (A) is preferably 1 to 30% by mass, more preferably 1 to 15% by mass, based on the total mass of the composition.

[0208] Solvent (B)

[0209] The solvent used in the composition of the present invention preferably includes water, a hydrocarbon solvent, an ether solvent, an ester solvent, an alcohol solvent or a ketone solvent.

[0210] Specific examples of the solvent include water, n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, 2,2,4-trimethylpentane, n-octane, isooctane, cyclohexane, methylcyclohexane, benzene, toluene, xylene, ethylbenzene, trimethylbenzene, methylethylbenzene, n-propylbenzene, isopropylbenzene, diethylbenzene, isobutylbenzene, triethylbenzene, diisopropylbenzene, n-pentylnaphthalene, trimethylbenzene, methanol, ethanol, n-propanol, isopropyl alcohol, n-butanol, isobutyl alcohol, sec-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, sec-pentanol, tert-Amyl alcohol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, sec-hexanol, 2-ethylbutanol, sec-heptanol, 3-heptanol, n-octanol, 2-ethylhexanol, sec-octanol, n-nonanol, 2,6-dimethylheptanol-4, n-decanol, sec-undecyl alcohol, trimethylnonanol, sec-tetradecanol, sec-heptadecanol, phenol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, benzyl alcohol, diacetone alcohol, cresol, ethylene glycol, propylene glycol, 1,3-butanediol, pentanediol-2,4,2-methylpentanediol-2, 4, hexanediol-2,5, heptanediol-2,4,2-ethyl hexanediol-1,3, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, acetone, methyl ethyl ketone, methyl n-propyl ketone, methyl n-butyl ketone, diethyl ketone, methyl isobutyl ketone, methyl n-amyl ketone, ethyl n-butyl ketone, methyl n-hexyl ketone, diisobutyl ketone, trimethyl nonanone, cyclohexanone, cyclopentanone, methyl cyclohexanone, 2,4-pentanedione, acetone acetone, diacetone alcohol, acetophenone, fenchone, ethyl ether, isopropyl ether, n-butyl ether, n-hexyl ether, 2-ethylhexane ether, ethylene oxide, 1,2-propylene oxide, dioxolane, 4-methyldioxolane, dioxane, dimethyldioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-n-hexyl ether, ethylene glycol monophenyl ether, ethylene glycol mono-2-ethyl butyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol di-n-butyl ether, diethylene glycol mono-n-hexyl ether, ethoxytriethylene glycol, tetraethylene glycol di-n-butyl ether, propylene glycol monomethyl ether (PGME),

[0211] Propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, diethyl carbonate, methyl acetate, ethyl acetate, γ-butyrolactone, γ-valerolactone, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, n-pentyl acetate, sec-pentyl acetate, ethyl 3-methoxybutyl acetate, methyl amyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, benzyl acetate, cyclohexyl acetate, methylcyclohexyl acetate, nonyl acetate, methyl acetoacetate, ethyl acetoacetate, ethylene glycol acetate monomethyl ether, ethylene glycol acetate monoethyl ether, diethylene glycol acetate monomethyl ether, diethylene glycol acetate monoethyl ether, diethylene glycol acetate monobutyl ether, propylene glycol acetate monomethyl ether, propylene glycol acetate monoethyl ether, propylene glycol acetate mono Propyl ether, propylene glycol acetate monobutyl ether, dipropylene glycol acetate monomethyl ether, dipropylene glycol acetate monoethyl ether, ethylene glycol diacetate, methoxytriethylene glycol acetate, ethyl propionate, n-butyl propionate, isopentyl propionate, diethyl oxalate, di-n-butyl oxalate, methyl lactate, ethyl lactate (EL), γ-butyrolactone, n-butyl lactate, n-pentyl lactate, diethyl malonate, dimethyl phthalate, diethyl phthalate, propylene glycol 1-monomethyl Ester solvents such as propylene glycol monoethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate; N-methylformamide, N,N-dimethylformamide, N,N-diethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropionamide, N-methylpyrrolidone, dimethyl sulfide, diethyl sulfide, thiophene, tetrahydrothiophene, dimethyl sulfoxide, cyclopentane and 1,3-propane sultone. These solvents can be used alone or in combination of two or more.

[0212] As the solvent (B), PGMEA, PGME or a mixture thereof is more preferred.

[0213] It is also an embodiment that the solvent (B) does not contain water compared to other layers and the film. For example, the amount of water in the entire solvent (B) is preferably 0.1 mass % or less, more preferably 0.01 mass % or less, and further preferably 0.001 mass % or less.

[0214] The content of the solvent (B) is preferably 50 to 99% by mass, more preferably 70 to 98% by mass, and further preferably 80 to 95% by mass based on the total mass of the composition. The film thickness after film formation can be controlled by increasing or decreasing the amount of the solvent in the entire composition.

[0215] Crosslinking agent (C)

[0216] The composition according to the present invention may further contain a crosslinking agent. It should be noted that in the present invention, a crosslinking agent refers to a compound having a crosslinking function. Although a compound having a crosslinking function is sometimes dissolved or dispersed in a solvent and included in the composition, it is preferred that such a solvent is included in the semiconductor composition as a solvent (B) or other components.

[0217] Since the crosslinking agent is used to improve the film-forming property when forming the composition, eliminate the mixing with the film (such as the resist film) formed on it, and eliminate the diffusion of the small molecule component to the upper film, it is useful. As described in the embodiments described later, the polymer (A) of the present invention has excellent film-forming property, embedding property and crosslinking property even if it does not contain a crosslinking agent. In addition, the sublimated substances (degassing) in the film forming process can be suppressed, which helps to avoid device contamination. Therefore, as one embodiment of the present invention, it is preferred that the content of the crosslinking agent added is small. Therefore, the content of the crosslinking agent is based on the total mass of the polymer (A), preferably 0 to 5% by mass, more preferably 0 to 1% by mass, and further preferably 0% by mass. By introducing a structure capable of crosslinking in the structure of the polymer (A), the content of the crosslinking agent can be reduced.

[0218] Examples of the crosslinking agent include melamine compounds, guanamine compounds, glycoluril compounds or urea compounds substituted with at least one group selected from hydroxymethyl, alkoxymethyl and acyloxymethyl, epoxy compounds, thioepoxy compounds, isocyanate compounds, azide compounds, and compounds containing double bonds such as alkenyl ether groups. In addition, compounds containing hydroxyl groups are also used as crosslinking agents.

[0219] Examples of epoxy compounds include tris(2,3-epoxypropyl)isocyanurate, trimethylolmethane triglycidyl ether, trimethylolpropane triglycidyl ether, and triethylolethane triglycidyl ether. Examples of melamine compounds include hexamethylolmelamine, hexamethoxymethylmelamine, compounds in which 1 to 6 methylol groups of hexamethylolmelamine are methoxymethylated, and mixtures thereof, hexamethoxyethylmelamine, hexaacyloxymethylmelamine, compounds in which 1 to 6 methylol groups of hexamethylolmelamine are acyloxymethylated, and mixtures thereof. Examples of guanamine compounds include tetramethylolguanamine, tetramethoxymethylguanamine, compounds in which 1 to 4 methylol groups of tetramethylolguanamine are methoxymethylated, and mixtures thereof, tetramethoxyethylguanamine, tetraacyloxyguanamine, compounds in which 1 to 4 methylol groups of tetramethylolguanamine are acyloxymethylated, and mixtures thereof. Examples of the glycoluril compound include tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, compounds in which 1 to 4 hydroxymethyl groups of tetramethylol glycoluril are methoxymethylated, or mixtures thereof, and compounds in which 1 to 4 hydroxymethyl groups of tetramethylol glycoluril are acyloxymethylated, or mixtures thereof. Examples of the urea compound include tetramethylol urea, tetramethoxymethyl urea, compounds in which 1 to 4 hydroxymethyl groups of tetramethylol urea are methoxymethylated, or mixtures thereof, and tetramethoxyethyl urea. Examples of the alkenyl ether group-containing compound include ethylene glycol divinyl ether, triethylene glycol divinyl ether, 1,2-propylene glycol divinyl ether, 1,4-butylene glycol divinyl ether, tetramethylene glycol divinyl ether, neopentyl glycol divinyl ether, trimethylolpropane trivinyl ether, hexanediol divinyl ether, 1,4-cyclohexanediol divinyl ether, pentaerythritol trivinyl ether, pentaerythritol tetravinyl ether, sorbitol tetravinyl ether, sorbitol pentavinyl ether, and trimethylolpropane trivinyl ether.

[0220] Examples of other cross-linking agents include those represented by the following formulae.

[0221]

[0222] Where, L 3 is a directly bonded substituted or unsubstituted C 1-3 Alkyl, R 20 L is hydrogen or methyl. 3 Preferably, it is a direct bond or a methyl group, and more preferably a direct bond. The substituent is preferably hydrogen, methyl, C 6-10 Aryl, one of the following two formulas, more preferably methyl or one of the following two formulas.

[0223]

[0224] Specific examples of the cross-linking agent represented by the above formula are as follows, but the scope of the present invention is not limited thereto.

[0225]

[0226] The crosslinking temperature when the present composition is formed into a film is preferably 50 to 230°C, more preferably 80 to 220°C, and even more preferably 80 to 190°C.

[0227] Acid generator (D)

[0228] The composition of the present invention may further contain an acid generator. In the present invention, the acid generator refers to the compound itself having an acid generating function. The compound having an acid generating function may be dissolved or dispersed in a solvent and contained in the composition, and such a solvent is preferably contained in the semiconductor composition as a solvent (B) or other components.

[0229] The content of the acid generator (D) is preferably 0.01 to 10% by mass, more preferably 1 to 7% by mass, based on the total mass of the polymer (A).

[0230] As the acid generator, a thermal acid generator (TAG) capable of generating a strong acid by heating can be used. The acid generator used in the present invention is preferably a compound that generates an acid capable of reacting with the polymer (A) according to the present invention and promoting the crosslinking of the polymer by heating. In a preferred embodiment, the acid generated is a strong acid such as sulfonic acid.

[0231] Preferably, the acid generator is activated at a temperature above 80°C. Examples of thermal acid generators are metal-free sulfonium and iodonium salts, such as triarylsulfonium, dialkylarylsulfonium and diarylalkylsulfonium salts of strong non-nucleophilic acids, alkylaryliodonium and diaryliodonium salts of strong non-nucleophilic acids; and ammonium, alkylammonium, dialkylammonium, trialkylammonium and tetraalkylammonium salts of strong non-nucleophilic acids. In addition, covalent thermal acid generators are also considered useful additives, such as 2-nitrobenzyl esters of alkyl or arylsulfonic acids, and other esters of sulfonic acids that thermally decompose to form free sulfonic acids. Examples thereof include diaryliodonium perfluoroalkylsulfonates, diaryliodonium tris(fluoroalkylsulfonyl)methides, diaryliodonium bis(fluoroalkylsulfonyl)methides, diaryliodonium bis(fluoroalkylsulfonyl)imides, diaryliodonium quaternary ammonium perfluoroalkylsulfonates. Examples of unstable esters are 2-nitrobenzyl toluenesulfonate, 2,4-dinitrobenzyl toluenesulfonate, 2,6-dinitrobenzyl toluenesulfonate, 4-nitrobenzyl toluenesulfonate; benzenesulfonates such as 2-trifluoromethyl-6-nitrobenzyl 4-chlorobenzenesulfonate and 2-trifluoromethyl-6-nitrobenzyl 4-nitrobenzenesulfonate; phenolsulfonates such as phenyl 4-methoxybenzenesulfonate; tris(fluoroalkylsulfonyl)methyl quaternary ammonium salts and bis(fluoroalkylsulfonyl)imide quaternary ammonium salts, alkylammonium salts of organic acids, such as triethylammonium salt of 10-camphorsulfonic acid. Various aromatic (anthracene, naphthalene or benzene derivative) sulfonic acid amine salts such as those disclosed in US Pat. Nos. 3,474,054, 4,200,729, 4,251,665 and 5,187,019 can also be used as TAG. The acid generator used in the present invention may be two or more compounds.

[0232] Surfactant (E)

[0233] The composition of the present invention may further contain a surfactant to improve coating properties. Here, in the present invention, the surfactant refers to the compound itself having a surface active effect. The compound having a surface active effect may be dissolved or dispersed in a solvent and included in the composition, and this solvent is preferably included in the semiconductor composition as a solvent (B) or other components.

[0234] The content of the surfactant (E) is preferably 0.001 to 5% by mass, more preferably 0.01 to 0.5% by mass, based on the total mass of the polymer (A).

[0235] As the surfactant (E) that can be used in the present invention, there can be listed (I) anionic surfactants, (II) cationic surfactants or (III) nonionic surfactants, and specifically, preferred are (I) alkyl sulfonates, alkylbenzene sulfonic acids and alkylbenzene sulfonates, (II) lauryl pyridinium chloride and lauryl methylammonium chloride, and (III) polyoxyethylene octyl ether, polyoxyethylene lauryl ether and polyoxyethylene acetylene glycol ether.

[0236] Additives (F)

[0237] The composition according to the present invention may contain further additives (F) in addition to (A) to (E).

[0238] There is no particular limitation on the additive (F), but preferably, the additive is selected from a base generator, a smoothing agent, a monomer dye, a lower alcohol (C 1-6 The additive refers to a compound having a certain function, for example, in the case of a base generator, it refers to a compound that generates a base. The compound can be dissolved or dispersed in a solvent and contained in the composition, and the solvent is preferably contained in the semiconductor composition as a solvent (B) or other components.

[0239] The content of the additive (F) is preferably 0 to 10% by mass, more preferably 0 to 5% by mass, based on the total mass of the polymer (A). No additive (F) (0% by mass) is also a suitable example of the composition according to the present invention.

[0240] <Method for producing film>

[0241] The method for producing a film according to the present invention comprises the following steps:

[0242] (1) applying the semiconductor composition of the present invention onto a substrate; and

[0243] (2) The semiconductor composition is heated to form a film.

[0244] Here, the film according to the present invention refers to a film derived from the semiconductor composition of the present invention, and is hereinafter referred to as the film (2). The film (2) is preferably a resist underlayer film, and more preferably an underlayer antireflection film.

[0245] Hereinafter, one embodiment of the production method according to the present invention will be described.

[0246] The semiconductor composition according to the present invention is coated on the top of a substrate (e.g., a silicon / silicon dioxide coated substrate, a silicon nitride substrate, a silicon wafer substrate, a glass substrate, and an ITO substrate, etc.) by an appropriate method. Here, in the present invention, the top includes the case where it is directly formed on the top and the case where it is formed through another layer. For example, a planarization film can be formed directly on the substrate, and the composition according to the present invention can be directly coated on the top of the planarization film. The coating method is not particularly limited, and for example, a coating method by a spinner and a coating machine can be cited. After coating, the film of the present invention is formed by heating. The heating of (2) is performed, for example, by a hot plate. The heating temperature is preferably 100 to 250°C, more preferably 125 to 225°C, and further more preferably 150 to 200°C. The temperature here is a heating atmosphere, such as a heating surface temperature of a hot plate. The heating time is preferably 30 to 300 seconds, and more preferably 45 to 180 seconds. The heating is preferably performed in an air or nitrogen atmosphere. By this heating, a cross-linking reaction is performed in the composition. Therefore, the film of (2) is not easily dissolved in subsequent steps.

[0247] The film thickness of the film of (2) is preferably 10 to 1000 nm, more preferably 30 to 500 nm, and even more preferably 50 to 100 nm.

[0248] The absorption parameter (k) of the film of (2) is measured by polarization analysis and has a value of 0.01 to 1.0 depending on the exposure wavelength. The refractive index (n) is also optimized and can be a value of 1.3 to 2.0, preferably 1.5 to 1.9 depending on the exposure wavelength. The values ​​of n and k can be calculated using an ellipsometer such as a JA Woollam WVASE VU-32 (trademark) ellipsometer. The exact values ​​of the optimal range of k and n depend on the exposure wavelength and the coating method used to expose the resist film coated on the film of (2).

[0249] The resist film may be manufactured by a method further comprising the steps of:

[0250] (3) applying a resist composition over the film of (2); and

[0251] (4) The resist composition is heated to form a resist film.

[0252] For the sake of clarity, steps (1) and (2) are performed before step (3). The numbers in brackets representing the steps indicate the order. The same applies to the following.

[0253] The resist composition is coated on the film of (2) by an appropriate method. The coating method is not particularly limited, but may be the same as the above-mentioned coating.

[0254] There is no particular limitation on the resist composition, as long as it is sensitive to the exposure light for pattern formation, and any positive resist composition, negative resist composition or negative tone development (NTD) resist composition can be used. The resist composition used in the present invention is preferably a positive resist composition or a negative resist composition, more preferably a chemically amplified positive resist composition or a chemically amplified negative resist composition. In addition, the resist composition preferably contains an acid generator or a base generator.

[0255] After coating, the resist film is formed by heating. The heating temperature in (4) is preferably 80 to 250° C., more preferably 80 to 200° C., and further preferably 90 to 180° C. The heating time is preferably 30 to 600 seconds, more preferably 30 to 300 seconds, and further preferably 60 to 180 seconds. The heating is preferably performed in air or nitrogen atmosphere.

[0256] The thickness of the resist film varies depending on the exposure wavelength, but is preferably 100 to 50000 nm. When the exposure is performed using a KrF excimer laser, the thickness of the resist film is preferably 100 to 5000 nm, more preferably 100 to 1000 nm, and further preferably 400 to 600 nm.

[0257] The resist pattern may be manufactured by a method further comprising the steps of:

[0258] (5) exposing the resist film to light; and

[0259] (6) The resist film is developed.

[0260] The resist film is exposed through a predetermined mask. The wavelength of the light used for exposure is not particularly limited, but it is preferably exposed with light with a wavelength of 13.5 to 248 nm. Specifically, KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), extreme ultraviolet light (wavelength 13.5 nm), etc. can be used, preferably KrF excimer laser. The allowable range of these wavelengths is ±1%. After exposure, if necessary, post-exposure baking can be performed. The temperature of post-exposure baking is preferably 80 to 150°C, more preferably 100 to 140°C, and the heating time is 0.3 to 5 minutes, preferably 0.5 to 2 minutes.

[0261] The exposed resist film is developed with a developer. The developer used is preferably a 2.38 mass % aqueous solution of tetramethylammonium hydroxide (TMAH). The temperature of the developer is preferably 5 to 50° C., more preferably 25 to 40° C., and the development time is preferably 10 to 300 seconds, more preferably 30 to 60 seconds.

[0262] By using such a developer, the resist film and / or the film of (2) can be easily dissolved and removed at room temperature. In addition, for example, a surfactant can be added to these developers.

[0263] When a positive resist composition is used, the positive photoresist layer in the exposed portion is removed by development to form a resist pattern. The resist pattern can also be further miniaturized by using, for example, a shrink material.

[0264] The engineered substrate may be manufactured by a method further comprising the steps of:

[0265] (7) Etching using the resist pattern as a mask

[0266] Using the resist pattern as a mask, the film or substrate of (2) is preferably etched. At this time, the substrate can be processed by etching the film and substrate of (2) once, or the substrate can be etched using the film (2) as a mask after etching the film, so as to perform staged processing. Etching can be one of dry etching or wet etching. This allows a gap to be formed in the substrate or the layer above the substrate. After the gap is formed, the resist pattern can be removed by contact with water, a mixture of a water-soluble organic solvent and water, or an alkaline aqueous solution. In addition, wiring can be formed using the gap formed. The substrate can also be processed by methods other than etching.

[0267] Then, as required, the substrate is further processed to form a device. Known methods can be applied to these further processes. After the device is formed, as required, the substrate is cut into wafers, connected to a lead frame, and encapsulated with a resin. In the present invention, the encapsulated device is referred to as a device.

[0268] Example

[0269] The present invention will be described below by various examples, but aspects of the present invention are not limited to these examples.

[0270] Synthesis of polymer 1

[0271] 350 g of PGMEA was added to a three-necked flask, followed by 32.79 g of MOI-BP (Karenzu MOI-BP, Showa Denko), 20 g of McHN (Kawasaki Chemical Industry), 6.422 g of DYE-M9A (Osaka Shinyaku), and 8.16 g of HPMA (Light Ester HOP, Kyoeisha Chemical), which correspond to unit (a), unit (b), unit (c), and unit (d), respectively.

[0272]

[0273] In addition, V-601 / oil-soluble azo polymerization initiator (Fujifilm Wako Pure Chemical Industries, Ltd.) was added. Nitrogen was filled into a three-necked flask, the lid was closed, and the mixture was heated while stirring, and the mixture was reacted at 80° C. for 4 hours. In addition, 3 g of PGME was added and stirred to complete the polymerization. The reaction solution was returned to room temperature. The reaction solution was added dropwise to 1500 g of hexane to precipitate a polymer. It was filtered and dried under reduced pressure to obtain polymer 1.

[0274]

[0275] The polymer 1 (molar ratio, n a :n b :n c :n d =26:49:14:11) were measured, and the Mn and Mw of polymer 1 were 9900 and 22200.

[0276] Synthesis of polymers 2 to 11 and comparative polymers 1 and 2

[0277] Polymers 2 to 11 and comparative polymers 1 and 2 were obtained by synthesizing in the same manner as the synthesis example of polymer 1 except that the molar ratios of unit (a), unit (b), unit (c) and unit (d) were changed as shown in Table 1.

[0278] It was visually confirmed that gelation occurred in Comparative Polymers 1 and 2. Comparative Polymers 1 and 2 were not used for subsequent evaluations because they were judged to be unsuitable for fine processing.

[0279] Table 1 shows the results of measuring Mn and Mw of each polymer using GPC (elution solvent: tetrahydrofuran).

[0280] Table 1

[0281] Unit (a) Unit (b) Unit (c) Unit (d) Mn / Mw Polymer 1 26 49 14 11 9900 / 22200 Polymer 2 49 40 11 0 9800 / 39000 Polymer 3 26 49 12 13 8600 / 20200 Polymer 4 25 49 14 12 7800 / 19600 Polymer 5 18 49 14 19 9200 / 20000 Polymer 6 11 49 14 26 11300 / 25100 Polymer 7 18 59 12 11 8400 / 19900 Polymer 8 44 29 8 19 10100 / 22000 Polymer 9 33 49 8 30 10100 / 22000 Polymer 10 0 55 15 30 4200 / 17800 Polymer 11 0 15 5 80 5800 / 19400 Comparison polymer 1 0 0 50 50 Gelation Comparison polymer 2 0 0 33 67 Gelation

[0282] Preparation of Composition 1

[0283] A surfactant (MEGAFACE R-40, DIC) was dissolved in PGMEA to give a concentration of 5% by mass. This was referred to as a 5% by mass surfactant solution.

[0284] 68.4 g of PGMEA and 29.4 g of PGME were mixed as a solvent. 0.04 g of camphorsulfonic acid (Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.018 g of triethylamine (Kanto Chemical) were added thereto. These were used as a thermal acid generator.

[0285]

[0286] 2 g of polymer 1 and 0.048 g of a 5% by mass surfactant solution were added thereto, and the mixture was stirred and mixed at room temperature for 1 hour. Thus, composition 1 was obtained.

[0287] When the composition 1 was visually confirmed, it could be confirmed that the solute was dissolved.

[0288] Preparation of Compositions 2 to 11

[0289] Except that the polymer used was changed as shown in Table 2, the same preparation method as the above-mentioned composition 1 was carried out to obtain compositions 2 to 11.

[0290] By visually inspecting each composition, dissolution of the solute can be confirmed.

[0291] Preparation of Composition 12

[0292] A surfactant (MEGAFACE R-40) was dissolved in PGMEA to give a concentration of 5% by mass. This was referred to as a 5% by mass surfactant solution.

[0293] 68.4 g of PGMEA and 29.4 g of PGME were mixed as a solvent. 0.04 g of camphorsulfonic acid and 0.018 g of triethylamine were added thereto. These were used as a thermal acid generator.

[0294] 2 g of polymer 1, 0.6 g of the following crosslinking agent Nicarac MX-270 (Sanwa Chemical) and 0.048 g of a 5 mass % surfactant solution were added thereto, and stirred and mixed at room temperature for 1 hour.

[0295]

[0296] When the composition 12 is visually confirmed, it can be confirmed that the solute is dissolved.

[0297] Preparation of Compositions 13 and 14

[0298] Except that the polymer used was changed as shown in Table 2, the same preparation as the above-mentioned composition 12 was carried out to obtain compositions 13 and 14.

[0299] By visually inspecting each composition, dissolution of the solute can be confirmed.

[0300] Preparation of Comparative Composition 1

[0301] The P090D polymer described below was dissolved in PGMEA to give 17% by mass. This is referred to as a P090D polymer solution.

[0302] A surfactant (MEGAFACE R-40) was dissolved in PGMEA to give a 5% by mass concentration. This was referred to as a 5% by mass surfactant solution.

[0303] 68.4 g of PGMEA and 29.4 g of PGME were mixed as solvents. 0.04 g of camphorsulfonic acid and 0.018 g of triethylamine were added thereto. These were used as thermal acid generators. 3.2 g of the following VPS-2515 (poly(hydroxystyrene / styrene) copolymer), 4.6 g of P090D polymer solution, 0.6 g of crosslinking agent (TMOM-BP), and 0.048 g of 5% by mass surfactant solution were added to the fragrance and stirred and mixed at room temperature for 1 hour. Thus, comparative composition 1 was obtained. Hereinafter, when VPS-2515 and P090D are polymer components, they will be referred to as VPS+P090D for simplicity.

[0304] When Comparative Composition 1 was visually confirmed, it was confirmed that the solute was dissolved.

[0305]

[0306] (P090D polymer, Toho Chemical, a:b:c:d=35.7:35.7:17.9:10.7. Molecular weight 4000-8000)

[0307]

[0308] (VPS-2515, Japan Soda Co., Ltd., molecular weight 3300~4300)

[0309]

[0310] (TMOM-BP, Honshu Chemical Industry)

[0311] Preparation of Comparative Composition 2

[0312] The P090D polymer was dissolved in PGMEA to a concentration of 17% by mass. This was referred to as a P090D polymer solution.

[0313] A surfactant (MEGAFACE R-40) was dissolved in PGMEA to give a concentration of 5% by mass. This was referred to as a 5% by mass surfactant solution.

[0314] 68.4 g of PGMEA and 29.4 g of PGME were mixed as a solvent. 0.04 g of camphorsulfonic acid and 0.018 g of triethylamine were added thereto. These were used as a thermal acid generator.

[0315] 3.2 g of a poly(hydroxystyrene / styrene) copolymer (VPS-2515), 4.6 g of a P090D polymer solution, and 0.048 g of a 5 mass % surfactant solution were added thereto, and the mixture was stirred and mixed at room temperature for 1 hour. Thus, a comparative composition 2 was obtained.

[0316] When Comparative Composition 2 was visually confirmed, it was confirmed that the solute was dissolved.

[0317] Evaluation of film formation

[0318] Each composition was spin-coated on a Si bare wafer using a coater / developer Mark 8 (Tokyo Electron Co., Ltd.) The wafer was baked at 180° C. for 60 seconds in air to form a film.

[0319] Through this procedure, if a film was formed from the composition, the film formation evaluation was A, and if a film was not formed, the film formation evaluation was B. The evaluation results are shown in Table 2.

[0320] The film thickness of the film was measured by Lambda Ace VM-1210 (SCREEN) and was 45 nm.

[0321] Uniformity evaluation

[0322] The uniformity of the film formed by the above film formation was evaluated. The evaluation criteria were as follows. The evaluation results are shown in Table 2.

[0323] A: Visually confirmed that the coating was uniform.

[0324] B: Visually check to confirm the presence of spots.

[0325] When the film thickness of the film formed by using Composition 1 was measured at 21 points on a straight line, the difference between the maximum value and the minimum value was 2 nm or less.

[0326] Table 2

[0327] Polymer (A) Crosslinking agent Film formation Uniformity Composition 1 Polymer 1 none A A Composition 2 Polymer 2 none A A Composition 3 Polymer 3 none A A Composition 4 Polymer 4 none A A Composition 5 Polymer 5 none A A Composition 6 Polymer 6 none A A Composition 7 Polymer 7 none A A Composition 8 Polymer 8 none A A Composition 9 Polymer 9 none A A Composition 10 Polymer 10 none A A Composition 11 Polymer 11 none A A Composition 12 Polymer 1 none A A Composition 13 Polymer 10 none A A Composition 14 Polymer 11 none A A Comparative composition 1 VPS+P090D none A A Comparative composition 2 VPS+P090D none A A

[0328] Evaluation of optical constants

[0329] The optical constants of the film formed by the above film formation were evaluated. The reflected light was measured at a wavelength of 248 nm using an ellipsometer M2000-D (JA Woolam). Thus, the optical constants n and k were obtained. The evaluation results are shown in Table 3.

[0330] It was confirmed that the film formed from Composition 1 had sufficient performance as an antireflection film.

[0331] Evaluation of filling

[0332] Each composition was spin-coated on a silicon step substrate (line-to-space ratio 1:2, spacing width 48 nm (L16 nm / S32 nm), depth 100 nm), and the substrate cross section was confirmed by SEM to evaluate the filling property. The evaluation criteria are as follows. The evaluation results are shown in Table 3.

[0333] A: In the SEM photograph, no voids were confirmed in the steps filled with the composition.

[0334] B: In the SEM photograph, a void exists in a part of the step filled with the composition.

[0335] Cross-linking evaluation

[0336] The film thickness of the film formed by the above-mentioned film formation is defined as the initial film thickness. The wafer is soaked in a PGMEA / PGME solution (AZ EBR7030, Merck Performance Materials, hereinafter referred to as MPM) for 60 seconds, then spin-dried, and the film thickness is measured again. If the reduction in film thickness compared to the initial film thickness is less than 2nm, it is evaluated as sufficient cross-linking. When sufficiently cross-linked, the baking temperature used for film formation is reduced in the order of 170°C, 160°C and 150°C until the reduction in film thickness is more than 2nm (insufficient cross-linking), and the same experiment and evaluation are performed. Thus confirm the cross-linking. The baking temperature conditions (sufficient cross-linking conditions) before insufficient cross-linking are listed in the table.

[0337] When the particle size was 10 nm or more due to the PGMEA / PGME solution, it was evaluated as B.

[0338] The evaluation results are shown in Table 3.

[0339] Formation of resist pattern

[0340] A resist composition (AZ DX3200P, MPM) was spin-coated on the film formed by the above film formation, and baked at 90° C. for 60 seconds. Thus, a resist film having a film thickness of 580 nm was formed.

[0341] The wafer was exposed under PFA-3000EX-5 (Canon) with a wavelength of 248 nm, a mask size of 200 nm, and a line:space of 1:1. The exposed wafer was exposed at 120° C. for 90 seconds, then baked and developed with a 2.38 mass % TMAH aqueous solution for 60 seconds. It was rinsed with water and spun dry. Thus, a resist pattern was formed.

[0342] Standing wave evaluation

[0343] The resist pattern formed as above was observed with a scanning electron microscope, and the state of the standing wave was evaluated. The evaluation criteria were as follows. The evaluation results are shown in Table 3.

[0344] A: The standing waves are reduced and there are almost no ripples on the resist wall.

[0345] B: The standing wave is reduced, but the resist wall surface has slight ripples.

[0346] C: No reduction in standing waves was observed.

[0347] Table 3

[0348] Polymer (A) Crosslinking agent n value k value Filling Cross-linking Standing Wave Composition 1 Polymer 1 none 1.8 0.32 A 150℃ A Composition 2 Polymer 2 none 1.79 0.31 A 160℃ A Composition 3 Polymer 3 none 1.83 0.28 A 150℃ A Composition 4 Polymer 4 none 1.8 0.31 A 150℃ A Composition 5 Polymer 5 none 1.8 0.32 A 150℃ A Composition 6 Polymer 6 none 1.8 0.32 A 150℃ A Composition 7 Polymer 7 none 1.85 0.3 A 150℃ A Composition 8 Polymer 8 none 1.81 0.31 A 150℃ A Composition 9 Polymer 9 none 1.81 0.31 A 150℃ A Composition 10 Polymer 10 none 1.83 0.36 A B B Composition 11 Polymer 11 none 1.64 0.14 A B B Composition 12 Polymer 1 have 1.81 0.31 A 150℃ A Composition 13 Polymer 10 have 1.83 0.36 A 150℃ A Composition 14 Polymer 11 have 1.64 0.14 A 150℃ A Comparative composition 1 VPS+P090D none 1.8 0.01 A B B Comparative composition 2 VPS+P090D have 1.8 0.01 A 180℃ A

[0349] Evaluation of sublimates

[0350] The test and evaluation were performed according to the method of measuring sublimates in a heat-cured film using a QCM sensor described in International Publication No. 2007 / 111147 (Patent Document 3).

[0351] Composition 1 was applied onto a silicon wafer substrate having a diameter of 4 inches using a spin coater at a speed of 2500 rpm during 60 seconds. The film thickness was measured to be 78 nm.

[0352] The wafer was placed in a sublimation measuring device integrated with a hot plate adjusted to 205° C. and baked for 60 seconds, and the sublimation was collected and quantified using a QCM sensor (TH-Q100 and sensor SEN-9E-H10, Tama Instruments).

[0353] During measurement, the temperature of the hot plate was raised to 180°C and the pump flow rate was set to 1m 3 / s, and aged during the first 60 seconds. Immediately thereafter, the wafer coated with the thin film was placed on a hot plate (mounting the measurement object) from the slide port, and the sublimates were collected from the 60-second time point to the 120-second time point (60 seconds).

[0354] A nozzle with a diameter of 2 mm is installed on the flow attachment (detection part) connecting the QCM sensor and the collection funnel part, and the distance between the sensor and the nozzle is kept at 0.5 mm. In addition, the QCM sensor uses an electrode made of a material made of a compound containing silicon and aluminum, and uses a crystal oscillator diameter (sensor diameter) of 14 mm, a crystal oscillator surface electrode diameter of 5 mm, and a sensor with a resonant frequency of 9 MHz.

[0355] The evaluation criteria are as follows.

[0356] A: Sublimation amount <0.1ng

[0357] B: Sublimation amount ≧0.1ng, ≦0.5ng

[0358] C: Sublimation amount> 0.5ng

[0359] The same tests and evaluations as above were carried out on the respective compositions shown in Table 4. The results are shown in Table 4.

[0360] Table 4

[0361] Polymer (A) Crosslinking agent Substrates Composition 1 Polymer 1 none A Composition 2 Polymer 2 none A Composition 3 Polymer 3 none A Composition 4 Polymer 4 none A Composition 5 Polymer 5 none A Composition 6 Polymer 6 none A Composition 7 Polymer 7 none A Composition 8 Polymer 8 none A Composition 9 Polymer 9 none A Composition 10 Polymer 10 none B Composition 11 Polymer 11 none B Composition 12 Polymer 10 Contains C Composition 13 Polymer 11 Contains C Comparative composition 1 VPS+P090D none A Comparative composition 2 VPS+P090D Contains B

[0362] It was confirmed that when the compositions 1 to 9 composed of the polymers 1 to 9 were formed into films, generation of sublimates was small. By using these compositions, contamination of equipment can be prevented, which is considered to be advantageous in the manufacturing process.

Claims

1. A lower antireflection film composition, which is a semiconductor composition containing a polymer (A) and a solvent (B), wherein the polymer (A) contains at least one structural unit selected from the group consisting of the following units (a), (b), (c) and (d): Unit (a) represented by formula (a): In formula (a), R a1 and R a2 H, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH, L a For a single bond, C 1-5 Alkylene, -O-, or C 1-5 Alkyleneoxy, ma is 1, X a1 H or C 1-5 Hydrocarbon, C 1-5 One or more -CH2- in the hydrocarbon group are independently replaced by -NH-, -C(=O)- and / or -O- or not, and C 1-5 One or more -CH3 in the hydrocarbon group are independently replaced by -NH2 and / or -COOH or not, Y a is N or O, where Y a When N is pa, pa is 2, Y a When it is O, pa is 1. X a2 H or C 1-5 Hydrocarbon, C 1-5 One or more -CH2- in the hydrocarbon group are independently replaced by -NH-, -C(=O)- and / or -O- or not, and C 1-5 One or more -CH3 in the hydrocarbon group are independently replaced by -NH2 and / or -COOH or not, and when pa is 2, two X a2 Same or different, Or, X a1 With X a2 bonding, and / or 2 x when pa is 2 a2 Bonding to form a saturated or unsaturated ring; Unit (b) represented by formula (b): In formula (b), R b1 and R b2 H, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Alkoxyalkyl, or -COOH, mb is 1, L b For a single bond, C 1-5 Alkylene, C 6-20 Arylene, -O-, or C 1-5 Alkyleneoxy, Z b C 6-20 Aromatic hydrocarbons or C 7-20 Aromatically substituted aliphatic hydrocarbons, pb is 0 to 4, qb is 1 to 3, R b3 H, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Alkoxyalkyl, or -COOH, when pb>1, each R b3 Same or different, R b4 is H or methyl, when qb>1, each R b4 Same or different, wherein unit (b) comprises an aromatic group containing at least one condensed structure; Unit (c) represented by formula (c): In formula (c), R c1 and R c2 H, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH, mc is 1, L c For a single bond, C 1-5 Alkylene, -O-, or C 1-5 Alkyleneoxy, V c is a condensed aromatic hydrocarbon or a condensed heterocyclic ring, V c It is formed by condensation of 3 to 6 rings. pc is 0 to 5, R c3 C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH, when pc>1, each R c3 the same or different; and The unit (d) represented by the following formula (d): In formula (d), R d1 and R d2 H, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH, md is 1, L d For a single bond, C 1-5 Alkylene, -O-, or C 1-5 Alkyleneoxy, C 1-5 One or more -CH2- in the alkylene group may or may not be replaced by -NH-, -C(=O)- and / or -O-, and C 1-5 One or more -CH3 in the alkylene group may or may not be replaced by -OH, -NH2 and / or -COOH, The number of repetitions of units (a), (b), (c) and (d) are n respectively. a 、n b 、n c and n d , which satisfies the following formula: n a +n b >0,n c >0, and n d ≥0, n a / (n a +n b +n c +n d ) is 2 to 80%, n b / (n a +n b +n c +n d ) is 10 to 90%, n c / (n a +n b +n c +n d ) is 3 to 80%, and n d / (n a +n b +n c +n d ) is 0~80%.

2. The lower antireflection film composition according to claim 1, wherein Satisfies the following formula: 5% ≤ n a / (n a + n b + n c + n d ) ≤ 50%, 30% ≤ n b / (n a + n b + n c + n d ) ≤ 80%, 5% ≤ n c / (n a + n b + n c + n d ) ≤ 40%, and / or 0% ≤ n d / (n a + n b + n c + n d ) ≤ 40%.

3. The lower antireflection film composition according to claim 1 or 2, wherein: The total number of all repeating units contained in the polymer (A) is n total Satisfies the following formula: 80%≤(n a +n b +n c +n d ) / n total ≤100%。 4. The lower antireflection film composition according to claim 1, wherein The solvent (B) contains water, a hydrocarbon solvent, an ether solvent, an ester solvent, an alcohol solvent or a ketone solvent.

5. The lower antireflection film composition according to claim 1, further comprising a crosslinking agent (C), wherein the content of the crosslinking agent (C) is 0 to 5% by mass based on the total mass of the polymer (A) in the lower antireflection film composition.

6. The lower anti-reflection film composition according to claim 1 further comprises an acid generator (D), optionally comprising an acid generator (D) in an amount of 0.01 to 10% by mass based on the total mass of the polymer (A) in the lower anti-reflection film composition; and optionally further comprises a surfactant (E), wherein the surfactant (E) in an amount of 0.001 to 5% by mass based on the total mass of the polymer (A) in the lower anti-reflection film composition.

7. The lower antireflection film composition according to claim 1, further comprising other additives (F), wherein the additives (F) are selected from the group consisting of base generators, smoothing agents, monomer dyes, C 1-6alcohol, a surface leveling agent, a substrate adhesive, a defoaming agent and an antiseptic, and optionally, the content of the additive (F) is 0 to 10% by mass based on the total mass of the polymer (A) in the lower antireflective film composition.

8. The lower antireflection film composition according to claim 1, wherein The content of the polymer (A) is 1 to 30% by mass based on the total mass of the lower antireflection film composition.

9. The lower antireflection film composition according to claim 1, wherein The content of the solvent (B) is 50 to 99% by mass based on the total mass of the lower antireflection film composition.

10. The lower antireflection film composition according to claim 1, wherein The mass average molecular weight of the polymer (A) is 1,000 to 50,000.

11. A method for producing a film, comprising the following steps: (1) an underlayer antireflection film composition according to any one of claims 1 to 10 applied above a substrate; and (2) The lower antireflection film composition is heated to form a film.

12. The manufacturing method according to claim 11, wherein: The heating in the above-mentioned (2) is performed at 100 to 250° C. and / or for 30 to 300 seconds.

13. The manufacturing method according to claim 11, wherein: The heating in the above-mentioned (2) is performed in an air atmosphere or a nitrogen atmosphere.

14. The manufacturing method according to claim 11, wherein: The thickness of the formed film is 10 to 1,000 nm.

15. A method for manufacturing a resist film, comprising the following steps: Manufacturing a film according to the method of claim 11; (3) applying a resist composition over the film according to claim 11; and (4) The resist composition is heated to form a resist film.

16. The manufacturing method according to claim 15, wherein: The heating in the above-mentioned (4) is performed at 80 to 250° C. and / or for 30 to 600 seconds.

17. The manufacturing method according to claim 15, wherein: The heating in the above-mentioned (4) is performed in an air atmosphere or a nitrogen atmosphere.

18. The manufacturing method according to claim 15, wherein: The thickness of the formed resist film is 100 to 50,000 nm.

19. A method for manufacturing a resist pattern, comprising the following steps: Manufacturing a resist film according to the method of claim 15; (5) exposing the resist film to light; and (6) The resist film is developed.

20. The manufacturing method according to claim 19, wherein: The exposure in the above (5) uses a light source of 248nm±1% or 193nm±1%.

21. The manufacturing method according to claim 19, wherein: The resist composition is a chemically amplified resist composition.

22. The manufacturing method according to claim 19, wherein: The aforementioned resist composition is a positive resist composition or a negative resist composition.

23. The manufacturing method according to claim 19, wherein: The aforementioned resist composition contains an acid generator or a base generator.

24. A method for manufacturing a processed substrate, comprising the following steps: Manufacturing a resist pattern according to the method of claim 19; and (7) Etching is performed using the resist pattern as a mask.

25. The manufacturing method according to claim 24, wherein: The aforementioned (7) is to etch the film or substrate of the aforementioned (2).

26. A method for manufacturing a device, comprising the method according to any one of claims 11 to 25.

Citation Information

Patent Citations

  • Composition for forming fine resist pattern and pattern forming method using the same

    JP2014071424A

  • Surface coating compositions containing pyridine salts or aromatic sulfonic acids

    US3474054A

  • Curing amino resins with aromatic sulfonic acid oxa-azacyclopentane adducts

    US4200729A

  • Aromatic sulfonic acid oxa-azacyclopentane adducts

    US4251665A

  • Latent catalysts

    US5187019A