Covering window
By using a thin glass substrate and a multi-layer coating structure in a display device for mobile electronic devices, combined with polymer materials and inorganic films, the problem of both flexibility and impact resistance of the cover window in the existing technology is solved, and efficient Protective effect.
Patent Information
- Application Number
- CN202110295258.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-19
- Filing Date
- 2021-03-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-03-19
Smart Images

Figure CN113493314B_ABST
Abstract
Description
[0001] This application claims priority to and all benefits from Korean Patent Application No. 10-2020-0033962, filed on March 19, 2020, the contents of which are incorporated herein by reference in their entirety. Technical Field
[0002] Embodiments of the present invention relate to a cover window and a display device including the cover window. Background Art
[0003] Various mobile electronic devices such as a portable phone, a navigation device, a digital camera, an electronic book, a portable game machine, or various types of terminals to which a liquid crystal display or an organic light emitting diode display is applied as a display device have been recently used.
[0004] Generally, a display device includes a display panel, and a cover window is provided at the front side of the display panel, the cover window is transparently formed so that a user can see the display part. Since the cover window is provided at the outermost side of the display device, the cover window should be sufficiently strong to resist external impact, thereby protecting the display panel inside the display device, etc.
[0005] In addition, research on a flexible display device is being actively conducted recently, and it is preferable that a cover window applied to the flexible display device has foldable flexibility. Summary of the invention
[0006] The embodiments have been completed in an effort to provide a cover window that is foldable and has enhanced impact resistance and a display device including the cover window.
[0007] An embodiment of the present invention provides a cover window, the cover window comprising: a glass substrate; a first coating layer, the first coating layer being disposed on a first surface of the glass substrate; and a second coating layer, the second coating layer being disposed on the first coating layer, wherein the thickness of the glass substrate may be equal to or less than 100 micrometers (μm), and the thickness of each of the first coating layer and the second coating layer may be between 50 angstroms and 100 angstroms. to within the range.
[0008] In an embodiment, the first coating layer and the second coating layer may include materials different from each other, respectively.
[0009] In an embodiment, each of the first coating and the second coating may include at least one of a polyimine oligomer having an average molecular weight in a range of 300 grams per mole (g / mol) to 5000 g / mol, an epoxy oligomer having an average molecular weight in a range of 300 g / mol to 5000 g / mol, an epoxy silane, an amino silane, sodium silicate, and polyvinyl alcohol ("PVA").
[0010] In an embodiment, the cover window may further include: an inorganic film disposed between the first coating layer and the second coating layer.
[0011] In an embodiment, the first coating layer may include sodium silicate, and the second coating layer may include a polyimine oligomer having an average molecular weight in a range of 300 g / mol to 5000 g / mol.
[0012] In an embodiment, the first coating may include epoxy silane, and the second coating may include PVA.
[0013] In an embodiment, the cover window may further include: a first upper layer disposed on the second surface of the glass substrate.
[0014] In an embodiment, the cover window may further include: a second upper layer disposed on the first upper layer, wherein the first upper layer may be disposed between the glass substrate and the second upper layer.
[0015] In an embodiment, the cover window may further include: a third upper layer disposed on the second upper layer; or a third upper layer and a fourth upper layer, the third upper layer disposed on the second upper layer, and the fourth upper layer disposed on the third upper layer.
[0016] In an embodiment, the cover window may further include: a third coating layer disposed in contact with the second coating layer.
[0017] In an embodiment, the first coating layer, the second coating layer, and the third coating layer may respectively include materials different from each other, and each of the first coating layer, the second coating layer, and the third coating layer may include at least one of a polyimide oligomer having an average molecular weight in the range of 300 g / mol to 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of 300 g / mol to 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA.
[0018] In an embodiment, the first coating layer may include epoxy silane, the second coating layer includes PVA, and the third coating layer includes sodium silicate.
[0019] In an embodiment, the cover window may further include: a first upper layer disposed on the second surface of the glass substrate.
[0020] In an embodiment, the cover window may further include: a second upper layer disposed on the first upper layer, wherein the first upper layer may be disposed between the glass substrate and the second upper layer.
[0021] In an embodiment, the cover window may further include: a third upper layer disposed on the second upper layer; or a third upper layer and a fourth upper layer, the third upper layer disposed on the second upper layer, and the fourth upper layer disposed on the third upper layer.
[0022] In an embodiment, the cover window may further include: a fourth coating layer disposed in contact with the third coating layer.
[0023] In an embodiment, the first coating layer, the second coating layer, the third coating layer, and the fourth coating layer may respectively include materials different from each other, and each of the first coating layer, the second coating layer, the third coating layer, and the fourth coating layer may include at least one of a polyimide oligomer having an average molecular weight in the range of 300 g / mol to 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of 300 g / mol to 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA.
[0024] In an embodiment, the first coating layer may include epoxy silane, the second coating layer may include PVA, the third coating layer may include sodium silicate, and the fourth coating layer may include polyimine oligomer having an average molecular weight in a range of 300 g / mol to 5000 g / mol.
[0025] In an embodiment, the cover window may further include: an upper layer disposed on the second surface of the glass substrate.
[0026] Another embodiment of the present invention provides a display device, including: the cover window, and a display panel, wherein the display panel overlaps the cover window.
[0027] According to the embodiments, it is possible to provide a cover window which is foldable and has enhanced impact resistance, and a display device including the cover window. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The above and other exemplary embodiments, advantages and features of the present disclosure will become more apparent by describing exemplary embodiments of the present disclosure in more detail with reference to the accompanying drawings, in which:
[0029] Figure 1 A cross-sectional view showing an embodiment of a cover window;
[0030] Figure 2 The principle of enhancing the impact resistance of a cover window comprising a glass substrate having a thin first coating and a second coating is shown;
[0031] Figure 3 An embodiment of a cover window is shown;
[0032] Figure 4 A cross-sectional view of another embodiment of a cover window is shown. Figure 3 The same cross section;
[0033] Figure 5 Another embodiment of the cover window is shown with Figure 1 Same cross-section;
[0034] Figure 6 Another embodiment of the cover window is shown with Figure 5 Same cross-section;
[0035] Figure 7 Another embodiment of the cover window is shown with Figure 1 Same cross-section;
[0036] Figure 8 A cross-sectional view of another embodiment of a cover window is shown. Figure 5 The same cross section;
[0037] Fig. 9 A cross-sectional view of another embodiment of a cover window is shown. Figure 8 The same cross section;
[0038] Fig.10 A cross-sectional view of another embodiment of a cover window is shown. Figure 1 The same cross section;
[0039] Fig.11 A cross-sectional view of another embodiment of a cover window is shown. Fig.10 The same cross section;
[0040] Fig.12 A cross-sectional view of another embodiment of a cover window is shown. Fig.11 The same cross section;
[0041] Fig.13 A cross-sectional view of another embodiment of a cover window is shown. Fig.12 The same cross section;
[0042] Fig.14 A cross-sectional view of another embodiment of a cover window is shown. Figure 5 The same cross section;
[0043] Fig.15 A cross-sectional view of another embodiment of a cover window is shown. Fig.14 The same cross section;
[0044] Fig.16 A cross-sectional view of another embodiment of a cover window is shown. Fig.15 The same cross section;
[0045] Fig.17 A cross-sectional view of another embodiment of a cover window is shown. Fig.16 The same cross section;
[0046] Fig.18 A cross-sectional view of another embodiment of a cover window is shown. Figure 6 The same cross section;
[0047] Fig.19 A cross-sectional view of another embodiment of a cover window is shown. Fig.18 The same cross section;
[0048] Fig. 20 A cross-sectional view of another embodiment of a cover window is shown. Fig.19 The same cross section;
[0049] Fig.21 A cross-sectional view of another embodiment of a cover window is shown. Fig. 20 The same cross section;
[0050] Fig. 22 shows the maximum free-fall height for each example that the cover window can withstand without breaking after the pen free-fall test; and
[0051] Fig.23 A cross-sectional view schematically shows an embodiment of a display device according to the present invention. DETAILED DESCRIPTION
[0052] Embodiments of the present invention will be described more fully hereinafter with reference to the accompanying drawings, in which embodiments of the present invention are shown. As will be appreciated by those skilled in the art, the described embodiments may be modified in various different ways, all without departing from the spirit or scope of the present disclosure.
[0053] Parts irrelevant to the description will be omitted to clearly describe the present disclosure, and like reference numerals refer to like elements throughout the specification.
[0054] In addition, in the drawings, the size and thickness of each element are arbitrarily shown for the convenience of description, and the present disclosure is not necessarily limited to the size and thickness shown in the drawings. In the drawings, the thickness of layers, films, panels, regions, etc. are exaggerated for the sake of clarity. In the drawings, the thickness of some layers and regions is exaggerated for the convenience of description.
[0055] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, the element may be directly on the other element, or there may also be an intermediate element. In contrast, when an element is referred to as being "directly on" another element, there are no intermediate elements. In addition, in the specification, the words "on..." or "above..." refer to being disposed on or under an object portion, and do not necessarily mean being disposed on the upper side of an object portion based on the direction of gravity.
[0056] In addition, unless explicitly described to the contrary, the words “comprise”, “comprises” or “comprising” will be understood to imply the inclusion of stated elements but not the exclusion of any other elements.
[0057] It will be understood that, although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or parts, these various elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Thus, without departing from the teachings herein, the first element, component, region, layer or part discussed below may be referred to as a second element, component, region, layer or part.
[0058] The terms used in this article are only for the purpose of describing specific embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms of "one", "a kind" and "the" as used in this article are intended to include plural forms including "at least one". "Or" means "and / or". As used in this article, the term "and / or" includes any combination and all combinations of one or more of the associated listed items. It will be further understood that when used in this specification, the terms "comprises and / or comprising" and "includes and / or including" illustrate the existence of stated features, regions, wholes, steps, operations, elements and / or components, but do not exclude the existence or increase of one or more other features, regions, wholes, steps, operations, elements, components and / or their groups.
[0059] As used herein, "about" or "approximately" includes the stated value and means within an acceptable range of deviation of the particular value determined by one of ordinary skill in the art, taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±30%, ±20%, ±10%, or ±5% of the stated value.
[0060] Furthermore, throughout this specification, the phrase “in a plan view” refers to observing a target portion from the top, and the phrase “in a cross section” refers to observing a cross section defined by vertically cutting the target portion from the side.
[0061] Unless otherwise defined, all terms (including technical and scientific terms) used in this article have the same meaning as commonly understood by ordinary technicians in the field to which the present invention belongs. It will be further understood that, unless explicitly defined as such in this article, terms such as those defined in general dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant field and this disclosure, and will not be interpreted in an idealized or overly formalized meaning.
[0062] Embodiments are described herein with reference to cross-sectional views, which are schematic views of idealized embodiments. Thus, shapes that deviate from the views due to, for example, manufacturing techniques and / or tolerances will be expected. Thus, the embodiments described herein should not be interpreted as being limited to the specific shapes of the regions as shown herein, but will include deviations in shapes caused by, for example, manufacturing. In an embodiment, the regions shown or described as flat typically may have rough and / or nonlinear features. In addition, the sharp angles shown may be rounded. Thus, the regions shown in the accompanying drawings are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions and are not intended to limit the scope of the claims.
[0063] Hereinafter, embodiments of a cover window and a display device including the same according to the present invention will be described in detail with reference to the accompanying drawings.
[0064] Figure 1 A cross-sectional view of an embodiment of a cover window is shown. The cover window 300 in the embodiment may include a glass substrate 310 , a first coating layer 320 , and a second coating layer 330 .
[0065] Although not shown, when the cover window 300 is applied to the display device, a display panel (not shown) may be disposed at a lower portion of the second coating layer 330. That is, in the specification, based on Figure 1 The first direction DR1 shown in FIG. 1 distinguishes the upper part and the lower part. In other words, the direction indicated by the arrow of the first direction DR1 is upward, and the opposite direction of the direction indicated by the arrow of the first direction DR1 is downward. In the cover window 300, the glass substrate 310 may be disposed at the uppermost position, and the second coating layer 330 may be disposed at the lowermost position.
[0066] The glass substrate 310 includes glass and may be thin and bendable. In an embodiment, for example, the thickness of the glass substrate 310 may be equal to or less than 100 micrometers (μm). A typical glass substrate having a thickness of several hundred micrometers is not easily bendable, but for example, in the illustrated embodiment, the glass substrate 310 has a thickness equal to or less than 100 μm and thus may be easily bendable.
[0067] The bendable glass substrate 310 has a bending property similar to that of a polymer substrate and has excellent transmission properties compared to the polymer substrate. In addition, since the deterioration of the appearance level according to the external environment is lower than that of the polymer substrate, it can have excellent display quality in a curved display device.
[0068] The first coating layer 320 and the second coating layer 330 are disposed on one side of the glass substrate 310. The first coating layer 320 and the second coating layer 330 may increase impact resistance so that the thin glass substrate 310 is not damaged by external impact.
[0069] Figure 2 The principle of enhancing the impact resistance of a cover window 300 is shown, the cover window 300 comprising a glass substrate 310 provided with a thin first coating layer 320 and a second coating layer 330. Figure 2 , the first coating layer 320 fills the fine cracks defined in the glass substrate 310. The fine cracks defined in the glass substrate 310 may be points where cracks start when impact is applied to the cover window 300. However, when the first coating layer 320 fills these fine cracks, even if impact is applied to the cover window 300, the cracks are not easily developed, and thus the impact resistance of the cover window 300 may be enhanced.
[0070] In addition, the second coating layer 330 disposed on the first coating layer 320 may include a material different from that of the first coating layer 320 to increase the impact resistance of the cover window 300 in a different manner from that of the first coating layer 320. As an example, the second coating layer 330 may include a material that is more resistant to moisture than the material of the first coating layer 320. In an alternative embodiment, the second coating layer 330 may include a material having higher stress resistance than the material of the first coating layer 320. In this way, when the second coating layer 330 includes a material having higher stress resistance than the material of the first coating layer 320, the second coating layer 330 may fix the first coating layer 320 with high stress resistance, and thus, even if an impact is applied to the cover window 300, the cover window 300 may be prevented from being easily damaged.
[0071] The materials of the first coating layer 320 and the second coating layer 330 may vary. In an embodiment, for example, the first coating layer 320 may include one or more of polyimide oligomer, epoxy oligomer, epoxy silane, amino silane, sodium silicate, and polyvinyl alcohol ("PVA").
[0072] In the illustrated embodiment, the polyimine oligomer refers to a material whose carbon chain includes two or more imine groups. In an embodiment, for example, the average molecular weight of the polyimine oligomer of the illustrated embodiment may be about 300 g / mol to about 5000 g / mol.
[0073] The oligomer with the mean molecular weight less than about 300g / mol has the form of a single molecule, and thus the oligomer with the mean molecular weight less than about 300g / mol does not have enough elasticity. Therefore, when the oligomer is applied to the first coating 320 or the second coating 330, the first coating 320 or the second coating 330 may not have enough impact resistance. In addition, when using the oligomer with the mean molecular weight greater than about 5000g / mol, because it is not manufactured by thermal evaporation method due to its excessive molecular weight, the oligomer with the mean molecular weight greater than about 5000g / mol is not preferred. That is to say, when using the polymer with the mean molecular weight greater than about 5000g / mol, in the manufacturing process using the thermal evaporation method, carbonization may occur before evaporation. In certain embodiments, for example, the mean molecular weight of the polyimide oligomer can be about 300g / mol to about 5000g / mol. This range is that the oligomer can have enough elasticity and can easily provide the range of coating during manufacture.
[0074] In the illustrated embodiment, epoxy oligomer refers to a material whose carbon chain includes one or more epoxy groups. In an embodiment, for example, the average molecular weight of the epoxy oligomer of the illustrated embodiment can be in the range of about 300 g / mol to about 5000 g / mol. This range is a range in which the epoxy oligomer can have sufficient elasticity and can easily form a coating during manufacturing.
[0075] In the illustrated embodiment, epoxysilane is a material including both epoxy groups and silane groups. In the illustrated embodiment, epoxysilane may include two or more epoxy groups.
[0076] In the illustrated embodiment, the aminosilane is a material that includes both amino groups and silane groups. In the illustrated embodiment, the aminosilane may include one or more amino groups.
[0077] In an embodiment, for example, the thickness of each of the first coating layer 320 and the second coating layer 330 may be about 50 angstroms. To about When the thickness of each of the first coating 320 and the second coating 330 is less than When the thickness of each of the first coating layer 320 and the second coating layer 330 is greater than When the cover window 300 is formed, the bending property may be degraded because the overall thickness of the cover window 300 is increased.
[0078] The first coating layer 320 and the second coating layer 330 may respectively include materials different from each other. Figure 3An embodiment of a cover window is shown. Figure 3 , the first coating layer 320 may include sodium silicate, and the second coating layer 330 may include polyimide oligomer. In this case, the first coating layer 320 may fill the cracks of the glass substrate 310 to increase the impact resistance. In addition, since sodium silicate has water resistance, it is possible to increase the water resistance of the cover window 300. Since the polyimide oligomer of the second coating layer 330 has high stress resistance, the polyimide oligomer of the second coating layer 330 may fix the first coating layer 320 and the glass substrate 310, and even if an impact is applied to the cover window 300, the impact may be prevented from being transmitted.
[0079] Figure 4 A cross-sectional view of another embodiment of a cover window is shown. Figure 3 Same cross section as in. Figure 4 , the first coating 320 may include epoxy silane, and the second coating 330 may include PVA. In this case, the epoxy silane of the first coating 320 fills the cracks of the glass substrate 310, and the epoxy silane has high stress resistance, so that the glass substrate 310 can be fixed. Therefore, even if an impact is applied to the glass substrate 310, it is possible to prevent such an impact from being transmitted. In addition, the PVA of the second coating 330 has high elasticity, so that the PVA of the second coating 330 can absorb the impact and increase the flexibility of the cover window 300.
[0080] Figure 1 , Figure 3 and Figure 4 The coating layer having a double-layer structure is shown, but the coating layer may have a three-layer or more-layer structure.
[0081] Figure 5 Another embodiment of the cover window is shown with Figure 1 Same cross-section. Figure 5 In addition to providing a third coating layer 340 below the second coating layer 330, the cover window 300 in the illustrated embodiment is Figure 1 The description of the first coating layer 320 and the second coating layer 330 is the same as the description of the first coating layer 320 and the second coating layer 330 described above, so the description of the first coating layer 320 and the second coating layer 330 is omitted.
[0082] The third coating layer 340 may include a material different from that of the first coating layer 320 and the second coating layer 330. In an embodiment, for example, the thickness of the third coating layer 340 may be about 1000 nm. To about When the thickness of the third coating 340 is less than When the thickness of the third coating 340 is greater than When the cover window 300 is formed, the bending property may be degraded because the overall thickness of the cover window 300 is increased.
[0083] In an embodiment, for example, the third coating 340 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. The detailed description of each material is the same as the detailed description of each material described above, so the detailed description of each material is omitted.
[0084] Figure 6 Another embodiment of the cover window is shown with Figure 5 Same cross-section. Figure 6 In addition to providing a fourth coating layer 350 below the third coating layer 340, the cover window 300 in the illustrated embodiment is Figure 5 The description of the first coating layer 320, the second coating layer 330 and the third coating layer 340 is the same as the description of the first coating layer 320, the second coating layer 330 and the third coating layer 340 described above, so the description of the first coating layer 320, the second coating layer 330 and the third coating layer 340 is omitted.
[0085] The fourth coating layer 350 may include a material different from that of the first coating layer 320, the second coating layer 330, and the third coating layer 340. In an embodiment, for example, the thickness of the fourth coating layer 350 may be about 1000 nm. To about When the thickness of the fourth coating 350 is less than When the thickness of the fourth coating 350 is greater than When the cover window 300 is formed, the bending property may be degraded because the overall thickness of the cover window 300 is increased.
[0086] In an embodiment, for example, the fourth coating 350 may include one or more of a polyimide oligomer having an average molecular weight in a range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in a range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. The detailed description of each material is the same as the detailed description of each material described above, so the detailed description of each material is omitted.
[0087] In the previous embodiment, the first to fourth coating layers 320 to 350 may include an organic material. However, an embodiment of the present invention also includes a structure in which an inorganic layer is included between the respective coating layers.
[0088] Figure 7 In another embodiment of the cover window 300, Figure 1 Same cross-section. Figure 7 In addition to including an inorganic layer 500 between the first coating layer 320 and the second coating layer 330, the cover window 300 in the illustrated embodiment is Figure 1 Detailed description of the same constituent elements will be omitted.
[0089] The inorganic layer 500 may include silicon nitride or silicon oxide. When the inorganic layer 500 is included as described above, even if an impact is applied to the cover window 300, the inorganic layer 500 supports the cover window 300, so that the impact resistance can be increased. Specifically, as in the illustrated embodiment, in a structure in which the inorganic layer 500 is disposed between the first coating layer 320 and the second coating layer 330 (the first coating layer 320 and the second coating layer 330 are organic layers), the inorganic layer 500 can absorb the impact by increasing the overall strength while preventing the cover window 300 from breaking.
[0090] Figure 8 A cross-sectional view of another embodiment of a cover window is shown. Figure 5 Same cross section as in. Figure 8 , the first coating layer 320 may include epoxy silane, the second coating layer 330 may include PVA, and the third coating layer 340 may include sodium silicate.
[0091] In this case, the epoxy silane of the first coating 320 fills the fine cracks of the glass substrate 310, and the epoxy silane has high stress resistance, so that the glass substrate 310 can be fixed. Therefore, even if an impact is applied to the glass substrate 310, it is possible to prevent such an impact from being transmitted. In addition, the PVA of the second coating 330 has high elasticity, so the PVA of the second coating 330 can absorb the impact and increase the flexibility of the cover window 300. In addition, since the sodium silicate of the third coating 340 has water resistance, it is possible to increase the water resistance of the cover window 300.
[0092] Fig. 9 A cross-sectional view of another embodiment of a cover window is shown. Figure 8 Same cross section as in. Fig. 9 In addition to including a fourth coating 350, the cover window 300 in the illustrated embodiment is Figure 8 Detailed description of the same constituent elements will be omitted.
[0093] The fourth coating layer 350 may include polyimide oligomer. Since the polyimide oligomer of the fourth coating layer 350 has high stress resistance, the polyimide oligomer of the fourth coating layer 350 may fix the cover window 300 and prevent the impact from being transferred even if the impact is applied to the cover window 300.
[0094] Fig.10 A cross-sectional view of another embodiment of a cover window is shown. Figure 1 Same cross section as in. Fig.10 In addition to including a first upper layer 410 disposed on the upper surface of the glass substrate 310, the cover window 300 in the illustrated embodiment is Figure 1 Detailed description of the same constituent elements will be omitted.
[0095] In an embodiment, for example, the first upper layer 410 may include one or more of a polyimide oligomer having an average molecular weight in a range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in a range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the first upper layer 410 may be about 1000 Å. To about
[0096] Fig.11 A cross-sectional view of another embodiment of a cover window is shown. Fig.10 Same cross section as in. Fig.11 In addition to including a second upper layer 420 disposed on the first upper layer 410, the cover window 300 in the illustrated embodiment is Fig.10 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the second upper layer 420 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the second upper layer 420 may be about To about
[0097] Fig.12 A cross-sectional view of another embodiment of a cover window is shown. Fig.11 Same cross section as in. Fig.12 In addition to including a third upper layer 430 disposed on the second upper layer 420, the cover window 300 in the illustrated embodiment is Fig.11 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the third upper layer 430 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the third upper layer 430 may be about To about
[0098] Fig.13 A cross-sectional view of another embodiment of a cover window is shown. Fig.12 Same cross section as in. Fig.13 In addition to including a fourth upper layer 440 disposed on the third upper layer 430, the cover window 300 in the illustrated embodiment is Fig.12 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the fourth upper layer 440 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the fourth upper layer 440 may be about To about
[0099] Fig.14 A cross-sectional view of another embodiment of a cover window is shown. Figure 5 Same cross section as in. Fig.14 In addition to including a first upper layer 410 disposed on the upper surface of the glass substrate 310, the cover window 300 in the illustrated embodiment is Figure 5 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the first upper layer 410 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the first upper layer 410 may be about To about
[0100] Fig.15A cross-sectional view of another embodiment of a cover window is shown. Fig.14 Same cross section as in. Fig.15 In addition to including a second upper layer 420 disposed on the first upper layer 410, the cover window 300 in the illustrated embodiment is Fig.14 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the second upper layer 420 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the second upper layer 420 may be about To about
[0101] Fig.16 A cross-sectional view of another embodiment of a cover window is shown. Fig.15 Same cross section as in. Fig.16 In addition to including a third upper layer 430 disposed on the second upper layer 420, the cover window 300 in the illustrated embodiment is Fig.15 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the third upper layer 430 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the third upper layer 430 may be about 1000 to 2000 μm. To about within the range.
[0102] Fig.17 A cross-sectional view of another embodiment of a cover window is shown. Fig.16 Same cross section as in. Fig.17 In addition to including a fourth upper layer 440 disposed on the third upper layer 430, the cover window 300 in the illustrated embodiment is Fig.16Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the fourth upper layer 440 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the fourth upper layer 440 may be about To about
[0103] Fig.18 A cross-sectional view of another embodiment of a cover window is shown. Figure 6 Same cross section as in. Fig.18 In addition to including a first upper layer 410 disposed on the upper surface of the glass substrate 310, the cover window 300 in the illustrated embodiment is Figure 6 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the first upper layer 410 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the first upper layer 410 may be about To about
[0104] Fig.19 A cross-sectional view of another embodiment of a cover window is shown. Fig.18 Same cross section as in. Fig.19 In addition to including a second upper layer 420 disposed on the first upper layer 410, the cover window 300 in the illustrated embodiment is Fig.18 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the second upper layer 420 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the second upper layer 420 may be about To about
[0105] Fig. 20 A cross-sectional view of another embodiment of a cover window is shown. Fig.19 Same cross section as in. Fig. 20 In addition to including a third upper layer 430 disposed on the second upper layer 420, the cover window 300 in the illustrated embodiment is Fig.19 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the third upper layer 430 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the third upper layer 430 may be about To about
[0106] Fig.21 A cross-sectional view of another embodiment of a cover window is shown. Fig. 20 Same cross section as in. Fig.21 In addition to including a fourth upper layer 440 disposed on the third upper layer 430, the cover window 300 in the illustrated embodiment is Fig. 20 Detailed description of the same constituent elements will be omitted. In an embodiment, for example, the fourth upper layer 440 may include one or more of a polyimide oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, an epoxy oligomer having an average molecular weight in the range of about 300 g / mol to about 5000 g / mol, epoxy silane, amino silane, sodium silicate, and PVA. In an embodiment, for example, the thickness of the fourth upper layer 440 may be about To about
[0107] Hereinafter, the effects of the cover window according to the embodiment of the present invention will be described in detail with reference to the accompanying drawings and Table 1.
[0108] Fig. 22 The maximum free-fall height of each example that the cover window can withstand without breaking after the pen free-fall test is shown. Referring to Table 1, the pen free-fall test was performed on a glass substrate having a thickness of 30 μm while changing the materials of the first coating layer and the second coating layer. After the experiment, when the pen was freely falling, the maximum free-fall height that the cover window could withstand without breaking was measured and Fig. 22 An "X" in Table 1 indicates that the cover window does not include the corresponding coating.
[0109]
[0110]
[0111] Refer to Table 1 and Fig. 22 , it was confirmed that Example 1 including only a glass substrate and not including a coating layer had a significantly lower free fall height than the example including the coating layer. That is, it was confirmed that when the coating layer was included, the impact resistance of the cover window was increased.
[0112] In addition, when comparing Example 2 including only one coating layer and Examples 3 to 8 including two or more coating layers, it was confirmed that the examples including two or more coating layers had a more significant effect. That is, in Example 2, the maximum free fall height was low and the deviation was large, while in Examples 3 to 8, it was confirmed that the maximum free fall height increased and the deviation according to repeated experiments decreased. That is, it was confirmed that the impact resistance was improved when two or more coating layers were stacked on the glass substrate, as in the example shown.
[0113] Hereinafter, a display device in an embodiment of the present invention will be described with reference to the accompanying drawings. Fig.23 A cross-sectional view schematically shows an embodiment of a display device according to the present invention.
[0114] Reference Fig.23 , the display device in the illustrated embodiment may include a display panel 200 and a cover window 300. The display panel 200 and the cover window 300 may be bonded by an adhesive layer 11.
[0115] The display panel 200 may be a liquid crystal display panel including a liquid crystal layer or a light-emitting display panel including a light-emitting diode. The display panel 200 may include a substrate, a transistor disposed on the substrate, a first electrode connected to the transistor, and a second electrode overlapping the first electrode. In some embodiments, the liquid crystal layer may be disposed between the first electrode and the second electrode. In an alternative embodiment, the light-emitting layer may be disposed between the first electrode and the second electrode. The substrate of the display panel 200 is flexible, so that the substrate of the display panel 200 can be bent.
[0116] The cover window 300 may be one of the above-mentioned embodiments. Fig.23 The cover window 300 may be Figure 1 and Figures 3 to 21 One of the cover windows 300.
[0117] As mentioned above, including Figure 1 and Figures 3 to 21 The display device of one of the cover windows 300 may be bent and has excellent impact resistance.
[0118] While the invention has been described in connection with what are presently considered to be practical embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but on the contrary is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the inventive concept.
Claims
1. A covering window, in, The cover window comprises: Glass substrate; a first coating layer disposed on a first surface of the glass substrate; and a second coating layer, the second coating layer being disposed on the first coating layer, Wherein, the thickness of the glass substrate is equal to or less than 100 micrometers, and The thickness of each of the first coating layer and the second coating layer is in the range of 50 angstroms to 400 angstroms, and Each of the first coating layer and the second coating layer includes at least one of a polyimine oligomer having an average molecular weight in a range of 300 to 5000 grams per mol, an epoxy oligomer having an average molecular weight in a range of 300 to 5000 grams per mol, epoxy silane, amino silane, sodium silicate, and polyvinyl alcohol.
2. The cover window according to claim 1, in, The first coating layer and the second coating layer include materials different from each other.
3. The cover window according to claim 1, in, The cover window further comprises: An inorganic film is disposed between the first coating layer and the second coating layer.
4. The cover window according to claim 1, in, The first coating comprises sodium silicate, and The second coating includes a polyimine oligomer having an average molecular weight in a range of 300 grams per mole to 5000 grams per mole.
5. The cover window according to claim 1, in, The first coating comprises epoxy silane, and The second coating layer includes polyvinyl alcohol.
6. The cover window according to claim 1, in, The cover window further comprises: a third coating layer, the third coating layer being arranged in contact with the second coating layer, and wherein The first coating layer, the second coating layer, and the third coating layer respectively include materials different from each other, and The third coating includes at least one of polyimine oligomer having an average molecular weight in the range of 300 to 5000 g / mol, epoxy oligomer having an average molecular weight in the range of 300 to 5000 g / mol, epoxy silane, amino silane, sodium silicate and polyvinyl alcohol.
7. The cover window according to claim 6, in, The first coating comprises epoxy silane, The second coating comprises polyvinyl alcohol, and The third coating includes sodium silicate.
8. The cover window according to claim 6, in, The cover window further comprises: a fourth coating layer, the fourth coating layer being arranged in contact with the third coating layer, and wherein The first coating layer, the second coating layer, the third coating layer, and the fourth coating layer respectively include materials different from each other, and Each of the third coating layer and the fourth coating layer includes at least one of a polyimine oligomer having an average molecular weight in a range of 300 to 5000 grams per mol, an epoxy oligomer having an average molecular weight in a range of 300 to 5000 grams per mol, epoxy silane, amino silane, sodium silicate, and polyvinyl alcohol.
9. The cover window according to claim 8, in, The first coating comprises epoxy silane, The second coating layer comprises polyvinyl alcohol, The third coating comprises sodium silicate, and The fourth coating layer includes a polyimine oligomer having an average molecular weight in a range of 300 grams per mole to 5000 grams per mole.