A kind of asphalt pavement structure using steel slag in a full-grained and refined manner
By using a finely designed asphalt pavement structure with full particle size, combined with the particle size and physical and mechanical properties of steel slag, the problem of low-value utilization of steel slag has been solved, achieving efficient and economical application of pavement materials and improving pavement durability and performance.
Patent Information
- Application Number
- CN202110878208.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-07-30
AI Technical Summary
In existing technologies, the differences in particle size and physical and mechanical properties of steel slag are not fully utilized, resulting in the low-value utilization of high-quality steel slag and the difficulty in meeting technical requirements for low-quality steel slag, thus hindering the resource utilization of steel slag.
By designing an asphalt pavement structure that utilizes all particle sizes, and matching the particle size and physical and mechanical properties of steel slag according to the function and role of different pavement structure layers, a differentiated design of the amount of steel slag aggregate in different layers is adopted to form an asphalt mixture layer, a graded crushed stone layer, and a cement-stabilized crushed stone layer, thereby achieving efficient and full-size utilization of steel slag.
This approach enables the high-value utilization of steel slag, improves pavement durability, extends pavement service life, reduces engineering costs, and meets the road performance and durability requirements of pavement materials.
Smart Images

Figure CN113529528B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of road engineering, and in particular relates to an asphalt pavement structure using steel slag in a full-grained and refined manner. Background Art
[0002] Steel slag is the slag discharged from steelmaking, accounting for about 10% to 15% of crude steel production, and is a major industrial solid waste. The main mineral phases of steel slag are tricalcium silicate, dicalcium silicate, calcium magnesium olivine, calcium magnesium rhodonite, calcium ferroaluminate, and solid solutions formed by oxides of silicon, magnesium, iron, manganese, and phosphorus. It also contains a small amount of free calcium oxide and metallic iron, fluoroapatite, etc. At present, the main way to dispose of steel slag is to use it as an ironmaking flux, directly adding it to the blast furnace or adding sintered ore, but steel slag with high sulfur and phosphorus content as a flux will directly reduce the utilization rate of blast furnace ironmaking. In order to actively implement the development concept of green transportation, aged steel slag is widely used as a road material in the cushion layer and structural layer of road subgrade, especially as an aggregate of asphalt mixture for paving the road surface layer. Road construction with steel slag has the advantages of high strength, good wear resistance and anti-skid properties, good durability, and low maintenance cost.
[0003] Steel slag is used in the field of road engineering, mainly using steel slag aggregate to replace ore aggregate, such as steel slag top layer SMA material (patent number 201911012831.X), steel slag bonding layer material (patent number 201911235856.6), steel slag permeable concrete material (patent number 201910940997.1, patent number 201911359583.6), steel slag recycled asphalt mixture (patent number 201711349397.5), etc. Since the particle size of steel slag is different, and the physical and mechanical properties of steel slag with different particle sizes are significantly different, the current utilization of steel slag is mainly based on its particle size to replace ore coarse and fine aggregates and ore fillers. This idea of using bagasse is to determine the utilization occasion based on its particle size, but it fails to combine the particle size and physical and mechanical properties of steel slag. For example, in road engineering, the physical and mechanical properties of the coarse aggregate in the upper asphalt mixture are quite different from those in other surface asphalt mixtures, the coarse aggregate in the cement stabilized macadam of the base layer, and the coarse aggregate in the graded macadam of the subbase layer. The price of the coarse aggregate is also different. According to the current idea of replacing ore coarse aggregate with extensive steel slag, many high-quality steel slags will be used at low value, and some low-quality steel slags cannot be used because they are difficult to meet technical requirements, which seriously hinders the resource utilization of industrial solid waste steel slag. Therefore, according to the different functions and effects of different layers of the road structure, and the differences in the composition, technical indicators and mechanical properties of the materials in each layer of the pavement structure, the present invention proposes a full-grained fine utilization of steel slag asphalt pavement structure that combines the particle size of steel slag with the differentiation of physical and mechanical properties. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an asphalt pavement structure that makes full-granular and refined utilization of steel slag. By combining the differentiation of the particle size and physical and mechanical properties of steel slag, the problems of high-quality steel slag being used at a low value and some low-quality steel slag being unable to be utilized due to difficulty meeting technical requirements can be avoided. The full-granular and refined utilization of steel slag can be achieved, steel slag solid waste can be disposed of on a large scale, the durability of the pavement can be improved, the service life of the pavement can be extended, and the project cost can be reduced.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] An asphalt pavement structure that utilizes steel slag in a full-grained and refined manner, the pavement structure comprises, from top to bottom, an asphalt mixture layer, a sealing layer, a graded crushed stone layer, and a cement-stabilized crushed stone layer, wherein the aggregates in the asphalt mixture layer, the graded crushed stone layer, and the cement-stabilized crushed stone layer all comprise natural aggregates and steel slag aggregates, wherein: the steel slag aggregate content in the asphalt mixture layer is 20%-70%; the steel slag aggregate content in the graded crushed stone layer is 70%-90%; and the steel slag aggregate content in the cement-stabilized crushed stone layer is 60%-80%.
[0007] Furthermore, the asphalt mixture layer also includes mineral powder and a bonding material, and the bonding material is any one of SBS modified asphalt and base asphalt.
[0008] Furthermore, the asphalt mixture layer includes, from top to bottom, an upper layer of asphalt mixture, a middle layer of asphalt mixture, and a lower layer of asphalt mixture.
[0009] Furthermore, the upper layer asphalt mixture is paved by mixing the following raw materials in the mass ratio: aggregate: mineral powder: fiber: bonding material = 100: (8-12): (0.2-0.5): (5.5-6.8), the natural aggregate content is 70%-80%, the steel slag aggregate content is 20%-30%, and the particle size of the steel slag aggregate is less than 4.75mm.
[0010] Furthermore, the middle surface layer asphalt mixture is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: binding material = 100: (4-8): (5.0-6.5), the natural aggregate content is 40%-60%, the steel slag aggregate content is 40%-60%, and the steel slag aggregate has a particle size of less than 9.5 mm.
[0011] Furthermore, the bottom layer asphalt mixture is paved by mixing the following raw materials in the mass ratio: aggregate: mineral powder: binding material = 100: (3-7): (4-5.5), the natural aggregate content is 30%-50%, the steel slag aggregate content is 50%-70%, and the particle size of the steel slag aggregate is less than 9.5mm.
[0012] Furthermore, the sealing layer is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: modified emulsified asphalt: water: cement = 100: (5-15): (10-15): (5-10): (1-3), and the aggregate is any one of neutral aggregate and neutral alkaline aggregate.
[0013] Furthermore, the aggregate has a particle size of 9.5-16 mm, and the seal layer is a synchronous crushed stone seal layer.
[0014] Furthermore, the graded crushed stone layer also includes crushed stone, using GA-4 graded crushed stone, and the particle size of the steel slag aggregate is less than 19 mm.
[0015] Furthermore, the cement-stabilized gravel layer is paved by mixing the following raw materials in a mass ratio: aggregate: cement = 100: (5-7), using CB-1 gravel grading, and the particle size of the steel slag aggregate is less than 13.2 mm.
[0016] Beneficial effects of the present invention:
[0017] 1. The present invention matches the differences in particle size and physical and mechanical properties of steel slag with the functions and effects of different layers of the pavement structure, thereby achieving high value and efficient utilization of the full particle size of steel slag;
[0018] 2. The present invention matches the difference in the amount of steel slag aggregate with the functions and effects of different layers of the pavement structure, thus achieving a high degree of unity among the utilization of industrial solid waste, the road performance of pavement materials and their durability;
[0019] 3. The inverted pavement structure formed by the graded crushed stone layer between the flexible lower asphalt mixture and the semi-rigid cement stabilized crushed stone layer adopted in the present invention can avoid or alleviate the expansion deformation of high-content steel slag and large-size steel slag, consume steel slag aggregates with low technical indicators, achieve a high degree of coordination between the steel slag aggregate dosage, particle size and technical characteristics and the pavement structure layer, and reduce the cost of engineering construction;
[0020] 4. The middle surface layer asphalt mixture of the present invention adopts high modulus asphalt mixture to give full play to the advantages of high modulus and high strength of steel slag aggregate, further ensuring the high temperature stability of the road surface and extending the service life of the road surface.
[0021] 5. The steel slag asphalt pavement structure obtained by implementing the present invention has higher dynamic stability, CBR value and unconfined compressive strength than the asphalt pavement structure in the comparative example. After the steel slag aggregate replaces the traditional ore aggregate, the mechanical properties of the material are equivalent and fully meet the requirements of the specifications. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the pavement structure of the present invention.
[0023] Among them, 1- asphalt mixture upper layer, 2- asphalt mixture middle layer, 3- asphalt mixture lower layer, 4- sealing layer, 5- graded gravel layer, 6- cement stabilized gravel layer. DETAILED DESCRIPTION
[0024] In order to better understand the present invention, the present invention is further described in detail below with reference to the accompanying drawings and preferred embodiments. However, it should be noted that many details listed in the specification are only for the purpose of enabling the reader to have a thorough understanding of one or more aspects of the present invention, and these aspects of the present invention can be implemented even without these specific details.
[0025] An asphalt pavement structure using steel slag in a full-grained and refined manner, the pavement structure comprises an asphalt mixture layer, a sealing layer, a graded crushed stone layer and a cement-stabilized crushed stone layer from top to bottom, the asphalt mixture layer, the graded crushed stone layer and the cement-stabilized crushed stone layer are all mixed with steel slag aggregates, the free calcium oxide in the steel slag aggregates is ≤ 3.0%, and the magnetic metallic iron is ≤ 2.0%, wherein: the steel slag aggregate content in the asphalt mixture layer is 20%-70%, and the water expansion rate of the steel slag aggregate is ≤ 2.0%; the steel slag aggregate content in the graded crushed stone layer is 70%-90%, and the water expansion rate of the steel slag aggregate is ≤ 4.0%; the steel slag aggregate content in the cement-stabilized crushed stone layer is 60%-80%, and the water expansion rate of the steel slag aggregate is ≤ 3.0%.
[0026] The asphalt mixture layer also includes natural aggregate, mineral powder and bonding material, and the bonding material is any one of SBS modified asphalt and base asphalt.
[0027] The asphalt mixture layer includes the upper asphalt mixture layer, the middle asphalt mixture layer, and the lower asphalt mixture layer from top to bottom, among which:
[0028] The upper asphalt mixture is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: fiber: bonding material = 100: (8-12): (0.2-0.5): (5.5-6.8), the natural aggregate content is 70%-80%, the steel slag aggregate content is 20%-30%, the crushing value of the steel slag aggregate is ≤26%, the Los Angeles abrasion loss is ≤28%, the water absorption rate is ≤2.0%, the firmness is ≤12%, the polishing value is ≤42%, the methylene blue value is ≤25g / kg, and the particle size of the steel slag aggregate is less than 4.75mm;
[0029] The middle surface layer asphalt mixture is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: bonding material = 100: (4-8): (5.0-6.5), the natural aggregate content is 40%-60%, the steel slag aggregate content is 40%-60%, the crushing value of the steel slag aggregate is ≤28%, the Los Angeles abrasion loss is ≤30%, the water absorption rate is ≤3.0%, the firmness is ≤12%, the polishing value is ≤42%, and the particle size of the steel slag aggregate is less than 9.5mm;
[0030] The lower layer of asphalt mixture is paved by mixing the following raw materials in the mass ratio: aggregate: mineral powder: binding material = 100: (3-7): (4-5.5), the natural aggregate content is 30%-50%, the steel slag aggregate content is 50%-70%, the crushing value of the steel slag aggregate is ≤28%, the needle-like shape is ≤18%, and the particle size of the steel slag aggregate is less than 9.5mm.
[0031] In the present invention, the thickness of the upper asphalt mixture is 4-6cm, the thickness of the middle asphalt mixture is 6-8cm, and the thickness of the lower asphalt mixture is 8-10cm; the upper asphalt mixture is any one of SMA-13, AC-13, and Superpave-13, and the bonding material is SBS modified asphalt; the middle asphalt mixture is HMA-16 high modulus asphalt mixture, and the bonding material is SBS modified asphalt; the lower asphalt mixture is any one of AC-20 and AC-25 asphalt mixture, and the bonding material is 70# base asphalt.
[0032] The sealing layer is paved by mixing the following raw materials in the mass ratio: aggregate: mineral powder: modified emulsified asphalt: water: cement = 100: (5-15): (10-15): (5-10): (1-3). The aggregate is any one of neutral aggregate and neutral alkaline aggregate. The aggregate particle size specification is 9.5-16mm. The sealing layer adopts synchronous crushed stone sealing layer. The thickness of the sealing layer is 4-7mm.
[0033] The graded crushed stone layer includes crushed stone, and GA-4 graded crushed stone is used. The crushing value of the steel slag aggregate in the graded crushed stone layer is not more than 30%, and the needle-like shape is not more than 20%. The particle size of the steel slag aggregate is less than 19mm, and the thickness of the graded crushed stone layer is 18-26cm.
[0034] The cement stabilized gravel layer is paved by mixing the following raw materials in a mass ratio: aggregate: ordinary Portland cement = 100: (5-7); the thickness of the cement stabilized gravel layer is 18-36 cm, and the CB-1 gravel grading is adopted. The crushing value of the steel slag aggregate in the cement stabilized gravel layer is not more than 30%, the needle-like value is not more than 22%, and the particle size of the steel slag aggregate is less than 13.2 mm.
[0035] In the present invention, the cement involved is ordinary Portland cement, the fiber is wood fiber, and the aggregate, mineral powder, modified emulsified asphalt, and SBS modified asphalt are all existing materials available on the market.
[0036] Example 1
[0037] The pavement structure in this embodiment includes an asphalt mixture upper layer 1, an asphalt mixture middle layer 2, an asphalt mixture lower layer 3, a sealing layer 4, a graded crushed stone layer 5, and a cement stabilized crushed stone layer 6.
[0038] The upper layer 1 of the asphalt mixture adopts SMA-13 asphalt mixture, in which aggregate: mineral powder: fiber: bonding material = 100:8:0.2:5.5, SBS modified asphalt, 6.3% oil-stone ratio, fiber is lignin fiber, steel slag content is 20%, steel slag technical indicators are shown in Table 1, and mineral grading is shown in Table 2.
[0039] Table 1 Technical indicators of steel slag
[0040] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.5% Water absorption 1.6% Free calcium oxide 2.2% Robustness 8% Magnetic Metal Iron 1.5% Polishing value 36% Crushing value 23% Methylene blue value 20g / kg Los Angeles Wear Loss 25%
[0041] Table 2 SMA-13 grading
[0042]
[0043] The surface layer 2 of the asphalt mixture adopts HMA-16, in which aggregate: mineral powder: bonding material = 100: 4: 5.0, SBS modified asphalt, 5.2% oil-stone ratio, 40% steel slag content, steel slag technical indicators are shown in Table 3, and mineral aggregate grading is shown in Table 4.
[0044] Table 3 Technical indicators of steel slag
[0045] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.6% Los Angeles Wear Loss 26% Free calcium oxide 2.3% Water absorption 2.3% Magnetic Metal Iron 1.5% Robustness 9% Crushing value 25% Polishing value 38%
[0046] Table 4 HMA-16 gradation
[0047]
[0048] The lower layer 3 of asphalt mixture adopts AC-20, in which aggregate: mineral powder: binding material = 100:3:4, the binding material is 70# matrix asphalt, 4.3% oil-stone ratio, 50% steel slag content, the technical indicators of steel slag are shown in Table 5, and the mineral grading is shown in Table 6.
[0049] Table 5 Technical indicators of steel slag
[0050] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.7% Crushing value 25% Free calcium oxide 2.7% Needle-like content 12% Magnetic Metal Iron 1.6%
[0051] Table 6 AC-20 gradation
[0052]
[0053] Seal layer 4 adopts synchronous crushed stone seal layer, aggregate: mineral powder: modified emulsified asphalt: water: cement = 100: 5: 10: 5: 1, using single particle size neutral aggregate or neutral alkaline aggregate, particle size specification is 9.5-16mm, aggregate should be clean, dry, non-weathered, free of impurities, regular in shape, and have sufficient strength and wear resistance.
[0054] The graded gravel layer 5 uses GA-4 graded gravel, with a steel slag content of 70%. The technical indicators of the steel slag are shown in Table 7, and the mineral grading is shown in Table 8.
[0055] Table 7 Technical indicators of steel slag
[0056] Technical indicators Numeric Technical indicators Numeric Water expansion rate 3.2% Crushing value 26% Free calcium oxide 2.6% Needle-like content 14% Magnetic Metal Iron 1.6%
[0057] Table 8 GA-4 graded crushed stone gradation
[0058]
[0059] The cement stabilized gravel layer 6 adopts the gradation of CB-1 cement stabilized gravel, aggregate: ordinary Portland cement = 100:5, cement strength grade 42.5, 6.0% cement dosage, 60% steel slag content, steel slag technical indicators are shown in Table 9, and mineral gradation is shown in Table 10.
[0060] Table 9 Technical indicators of steel slag
[0061] Technical indicators Numeric Technical indicators Numeric Water expansion rate 2.1% Crushing value 25% Free calcium oxide 2.6% Needle-like content 14% Magnetic Metal Iron 1.5%
[0062] Table 10 Grading of CB-1 cement stabilized crushed stone
[0063]
[0064] Example 2
[0065] The pavement structure in this embodiment includes an asphalt mixture upper layer 1, an asphalt mixture middle layer 2, an asphalt mixture lower layer 3, a sealing layer 4, a graded crushed stone layer 5, and a cement stabilized crushed stone layer 6.
[0066] The upper layer 1 of asphalt mixture adopts AC-13 asphalt mixture, in which aggregate: mineral powder: binding material = 100:10:6, the binding material is SBS modified asphalt, 4.8% oil-stone ratio, 25% steel slag content, the technical indicators of steel slag are shown in Table 11, and the mineral grading is shown in Table 12.
[0067] Table 11 Technical indicators of steel slag
[0068] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.5% Water absorption 1.6% Free calcium oxide 2.2% Robustness 8% Magnetic Metal Iron 1.5% Polishing value 36% Crushing value 23% Methylene blue value 20g / kg Los Angeles Wear Loss 25%
[0069] Table 12 AC-13 gradation
[0070]
[0071] The surface layer 2 of the asphalt mixture adopts HMA-16, in which aggregate: mineral powder: bonding material = 100: 6: 6, the bonding material is SBS modified asphalt, 5.2% oil-stone ratio, 50% steel slag content, the technical indicators of steel slag are shown in Table 13, and the mineral grading is shown in Table 14.
[0072] Table 13 Technical indicators of steel slag
[0073] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.6% Los Angeles Wear Loss 26% Free calcium oxide 2.3% Water absorption 2.3% Magnetic Metal Iron 1.5% Robustness 9% Crushing value 25% Polishing value 38%
[0074] Table 14 HMA-16 gradation
[0075]
[0076] The lower layer 3 of asphalt mixture adopts AC-25, in which aggregate: mineral powder: binding material = 100:5:5, the binding material is 70# matrix asphalt, 4.2% oil-stone ratio, 61% steel slag content, the technical indicators of steel slag are shown in Table 15, and the mineral grading is shown in Table 16.
[0077] Table 15 Technical indicators of steel slag
[0078] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.7% Crushing value 24% Free calcium oxide 2.6% Needle-like content 12% Magnetic Metal Iron 1.6%
[0079] Table 16 AC-25 gradation
[0080]
[0081] Seal layer 4 adopts synchronous crushed stone seal layer, in which aggregate: mineral powder: modified emulsified asphalt: water: cement = 100:10:13:7:2, and single-size neutral aggregate or neutral alkaline aggregate is used, with a particle size specification of 9.5-16mm. The aggregate should be clean, dry, non-weathered, free of impurities, regular in shape, and have sufficient strength and wear resistance.
[0082] The graded gravel layer 5 uses GA-4 graded gravel with a steel slag content of 78%. The technical indicators of the steel slag are shown in Table 17, and the mineral grading is shown in Table 18.
[0083] Table 17 Technical indicators of steel slag
[0084] Technical indicators Numeric Technical indicators Numeric Water expansion rate 3.1% Crushing value 26% Free calcium oxide 2.6% Needle-like content 15% Magnetic Metal Iron 1.7%
[0085] Table 18 GA-4 graded crushed stone gradation
[0086]
[0087] The cement stabilized gravel layer 6 adopts the gradation of CB-1 cement stabilized gravel, where aggregate: ordinary Portland cement = 100:6, cement strength grade 42.5, 5.7% cement dosage, 70% steel slag content, steel slag technical indicators are shown in Table 19, and mineral gradation is shown in Table 20.
[0088] Table 19 Technical indicators of steel slag
[0089] Technical indicators Numeric Technical indicators Numeric Water expansion rate 2.2% Crushing value 25% Free calcium oxide 2.6% Needle-like content 14% Magnetic Metal Iron 1.5%
[0090] Table 20 Grading of CB-1 cement stabilized crushed stone
[0091]
[0092] Example 3
[0093] The pavement structure in this embodiment includes an asphalt mixture upper layer 1, an asphalt mixture middle layer 2, an asphalt mixture lower layer 3, a sealing layer 4, a graded crushed stone layer 5, and a cement stabilized crushed stone layer 6.
[0094] The upper layer 1 of asphalt mixture adopts Superpave-13 asphalt mixture, in which aggregate: mineral powder: binding material = 100:12:6.8, the binding material is SBS modified asphalt, 6.3% oil-stone ratio, 30% steel slag content, the technical indicators of steel slag are shown in Table 21, and the mineral grading is shown in Table 22.
[0095] Table 21 Technical indicators of steel slag
[0096] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.5% Water absorption 1.6% Free calcium oxide 2.2% Robustness 8% Magnetic Metal Iron 1.5% Polishing value 36% Crushing value 23% Methylene blue value 20g / kg Los Angeles Wear Loss 25%
[0097] Table 22 Superpave-13 gradation
[0098]
[0099] The surface layer 2 of the asphalt mixture adopts HMA-16, aggregate: mineral powder: binding material = 100:8:6.5, the binding material is SBS modified asphalt, 5.2% oil-stone ratio, 60% steel slag content, the technical indicators of steel slag are shown in Table 23, and the mineral grading is shown in Table 24.
[0100] Table 23 Technical indicators of steel slag
[0101] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.6% Los Angeles Wear Loss 26% Free calcium oxide 2.3% Water absorption 2.3% Magnetic Metal Iron 1.5% Robustness 9% Crushing value 25% Polishing value 38%
[0102] Table 24 HMA-16 gradation
[0103]
[0104] The lower layer 3 of asphalt mixture adopts AC-20, aggregate: mineral powder: binding material = 100:7:5.5, the binding material is 70# matrix asphalt, 4.3% oil-stone ratio, 70% steel slag content, the technical indicators of steel slag are shown in Table 25, and the mineral grading is shown in Table 26.
[0105] Table 25 Technical indicators of steel slag
[0106] Technical indicators Numeric Technical indicators Numeric Water expansion rate 1.7% Crushing value 25% Free calcium oxide 2.7% Needle-like content 12% Magnetic Metal Iron 1.6%
[0107] Table 26 AC-20 gradation
[0108]
[0109] The seal layer 4 adopts synchronous crushed stone seal layer, in which aggregate: mineral powder: modified emulsified asphalt: water: cement = 100:15:15:10:3. Neutral aggregate or neutral alkaline aggregate with a single particle size is used, and the particle size specification is 9.5-16mm. The aggregate should be clean, dry, non-weathered, free of impurities, regular in shape, and have sufficient strength and wear resistance.
[0110] The graded gravel layer 5 uses GA-4 graded gravel with a steel slag content of 90%. The technical indicators of the steel slag are shown in Table 27, and the mineral grading is shown in Table 28.
[0111] Table 27 Technical indicators of steel slag
[0112] Technical indicators Numeric Technical indicators Numeric Water expansion rate 3.2% Crushing value 26% Free calcium oxide 2.6% Needle-like content 14% Magnetic Metal Iron 1.6%
[0113] Table 28 GA-4 graded crushed stone gradation
[0114]
[0115] The cement stabilized gravel layer 6 adopts the gradation of CB-1 cement stabilized gravel, where aggregate: ordinary Portland cement = 100:7, cement strength grade 42.5, 6.0% cement dosage, 80% steel slag content, steel slag technical indicators are shown in Table 29, and mineral gradation is shown in Table 30.
[0116] Table 29 Technical indicators of steel slag
[0117] Technical indicators Numeric Technical indicators Numeric Water expansion rate 2.1% Crushing value 25% Free calcium oxide 2.6% Needle-like content 14% Magnetic Metal Iron 1.5%
[0118] Table 30 Grading of CB-1 cement stabilized crushed stone
[0119]
[0120] Comparative Example 1
[0121] The asphalt mixture top layer 1 uses SMA-13 asphalt mixture, SBS modified asphalt, 6.2% oil-stone ratio, 0.3% lignin fiber, and the mineral grading is shown in Table 31.
[0122] Table 31 SMA-13 grading
[0123]
[0124] The surface layer 2 of the high modulus asphalt mixture uses HMA-16, SBS modified asphalt, 5.0% oil-stone ratio, and the mineral aggregate grading is shown in Table 32.
[0125] Table 32 HMA-16 gradation
[0126]
[0127] The lower layer 3 of the asphalt mixture uses AC-20, 70# base asphalt, 4.0% oil-stone ratio, and the mineral aggregate grading is shown in Table 33.
[0128] Table 33 AC-20 grading
[0129]
[0130] Seal layer 4 adopts synchronous crushed stone seal layer, and the binder can be one of road petroleum asphalt, SBS modified, and rubber asphalt. A single particle size neutral aggregate or neutral alkaline aggregate is used, and the particle size specification is 9.5-16mm. The aggregate should be clean, dry, non-weathered, free of impurities, regular in shape, and have sufficient strength and wear resistance.
[0131] The graded gravel layer 5 uses GA-4 graded gravel, and the mineral grading is shown in Table 34.
[0132] Table 34 GA-4 graded crushed stone gradation
[0133]
[0134] The cement stabilized gravel layer 6 adopts the grading of CB-1 cement stabilized gravel, cement strength grade 42.5, 6.0% cement dosage, and the mineral grading is shown in Table 25.
[0135] Table 35 Grading of CB-1 cement stabilized crushed stone
[0136]
[0137] Comparative Example 2
[0138] The asphalt mixture top layer 1 uses AC-13 asphalt mixture, SBS modified asphalt, 4.7% oil-stone ratio, and the mineral aggregate grading is shown in Table 36.
[0139] Table 36 AC-13 gradation
[0140]
[0141] The surface layer 2 of the high modulus asphalt mixture uses HMA-16, SBS modified asphalt, 5.0% oil-stone ratio, and the mineral aggregate grading is shown in Table 37.
[0142] Table 37 HMA-16 gradation
[0143]
[0144] The lower layer 3 of the asphalt mixture uses AC-25, 70# base asphalt, 4.0% oil-stone ratio, and the mineral aggregate grading is shown in Table 38.
[0145] Table 38 AC-25 gradation
[0146]
[0147] Seal layer 4 adopts synchronous crushed stone seal layer, and the binder can be one of road petroleum asphalt, SBS modified, and rubber asphalt. A single particle size neutral aggregate or neutral alkaline aggregate is used, and the particle size specification is 9.5-16mm. The aggregate should be clean, dry, non-weathered, free of impurities, regular in shape, and have sufficient strength and wear resistance.
[0148] The graded gravel layer 5 uses GA-4 graded gravel, and the mineral grading is shown in Table 39.
[0149] Table 39 GA-4 graded crushed stone gradation
[0150]
[0151] The cement stabilized gravel layer 6 adopts the grading of CB-1 cement stabilized gravel, cement strength grade 42.5, 5.7% cement dosage, and the mineral grading is shown in Table 40.
[0152] Table 40 Grading of CB-1 cement stabilized crushed stone
[0153]
[0154] Comparative Example 3
[0155] The upper layer 1 of the asphalt mixture adopts Superpave-13 asphalt mixture, SBS modified asphalt, 6.3% oil-stone ratio, and the mineral aggregate gradation is shown in Table 41.
[0156] Table 41 Superpave-13 gradation
[0157]
[0158] The surface layer 2 of the asphalt mixture uses HMA-16, SBS modified asphalt, 5.2% oil-stone ratio, and the mineral aggregate grading is shown in Table 42.
[0159] Table 42 HMA-16 gradation
[0160]
[0161] The lower layer 3 of the asphalt mixture uses AC-20, 70# base asphalt, 4.3% oil-stone ratio, and the mineral aggregate grading is shown in Table 43.
[0162] Table 43 AC-20 grading
[0163]
[0164]
[0165] The seal layer 4 adopts synchronous crushed stone seal layer, and the binder can be one of road petroleum asphalt, SBS modified, and rubber asphalt. A single particle size neutral aggregate or neutral alkaline aggregate is used, and the particle size specification is 9.5-16mm. The aggregate should be clean, dry, non-weathered, free of impurities, regular in shape, and have sufficient strength and wear resistance.
[0166] The graded gravel layer 5 uses GA-4 graded gravel, and the mineral grading is shown in Table 44.
[0167] Table 44 GA-4 graded crushed stone gradation
[0168]
[0169] The cement stabilized gravel layer 6 adopts the grading of CB-1 cement stabilized gravel, cement strength grade 42.5, 6.0% cement dosage, and the mineral grading is shown in Table 45.
[0170] Table 45 Grading of CB-1 cement stabilized crushed stone
[0171]
[0172] The dynamic stability test, graded crushed stone CBR test, and cement stabilized crushed stone unconfined compressive strength test of the asphalt mixture obtained by Implementation 1-3 and Comparative Example 1-3 were carried out. The method and standard of the dynamic stability test were respectively referred to the "Test Code for Asphalt and Asphalt Mixture in Highway Engineering JTG E20-2011" and "Technical Specification for Highway Asphalt Pavement Construction JTG F40-2004", and the test methods and standards of the CBR test and unconfined compressive strength test were respectively referred to the "Test Code for Inorganic Binder Stabilized Materials in Highway Engineering JTG E51-2015" and "Technical Specifications for Highway Pavement Base Construction JTG / T F20-2015". The test results are shown in Table 46.
[0173] Table 46 Example Effect Comparison
[0174]
[0175] As can be seen from Table 46, the dynamic stability, CBR value and unconfined compressive strength of the embodiments of the present invention are higher than those of the comparative examples, indicating that the mechanical properties of the materials according to the steel slag content and technical indicators of each layer of the pavement structure of the present invention are higher than or close to the mechanical properties of the materials without steel slag, and all meet the current specifications and standards. The gradation of HMA-16 asphalt mixture did not occur in different embodiments. Since the surface texture of steel slag aggregate is relatively rich, under the same gradation conditions, more asphalt wrapping is required to replace ore aggregate with steel slag aggregate, so the asphalt content of the comparative example is slightly higher than that of the embodiment. However, the above test results show that after steel slag aggregate replaces traditional ore aggregate, the mechanical properties of the material are equivalent and fully meet the requirements of the specification. At the same time, after steel slag aggregate replaces part of the ore aggregate, the cement dosage in cement-stabilized gravel is also increased appropriately. Although the asphalt (cement) cost of the embodiment is slightly higher, the social benefits, ecological benefits and economic benefits of steel slag aggregate replacing ore aggregate after large-scale application are significant, which obviously exceed the material cost of the slightly increased asphalt (cement) dosage. Therefore, the present invention can consume steel slag solid waste on a large scale, improve the durability of the road surface, extend the service life of the road surface, and reduce the engineering cost.
[0176] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An asphalt pavement structure using steel slag in a full-grained and refined manner, characterized in that: The pavement structure comprises an asphalt mixture layer, a seal layer, a graded crushed stone layer and a cement stabilized crushed stone layer from top to bottom, and the aggregates in the asphalt mixture layer, the graded crushed stone layer and the cement stabilized crushed stone layer all comprise natural aggregates and steel slag aggregates, wherein: the steel slag aggregate content in the asphalt mixture layer is 20%-70%; the steel slag aggregate content in the graded crushed stone layer is 70%-90%; the steel slag aggregate content in the cement stabilized crushed stone layer is 60%-80%; The asphalt mixture layer also includes mineral powder and a bonding material, and the bonding material is any one of SBS modified asphalt and base asphalt; The asphalt mixture layer includes, from top to bottom, an upper layer of asphalt mixture, a middle layer of asphalt mixture, and a lower layer of asphalt mixture; The upper layer asphalt mixture is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: fiber: bonding material = 100: (8-12): (0.2-0.5): (5.5-6.8), the natural aggregate content is 70%-80%, the steel slag aggregate content is 20%-30%, and the particle size of the steel slag aggregate is less than 4.75 mm; The middle surface layer asphalt mixture is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: bonding material = 100: (4-8): (5.0-6.5), the natural aggregate content is 40%-60%, the steel slag aggregate content is 40%-60%, and the steel slag aggregate particle size is less than 9.5 mm; The bottom layer asphalt mixture is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: binding material = 100: (3-7): (4-5.5), the natural aggregate content is 30%-50%, the steel slag aggregate content is 50%-70%, and the particle size of the steel slag aggregate is less than 9.5 mm; The cement stabilized gravel layer is paved by mixing the following raw materials in a mass ratio: aggregate: cement = 100: (5-7), using CB-1 gravel grading, and the particle size of the steel slag aggregate is less than 13.2 mm.
2. The asphalt pavement structure using steel slag in a full-grained fine manner as claimed in claim 1, characterized in that: The sealing layer is paved by mixing the following raw materials in a mass ratio: aggregate: mineral powder: modified emulsified asphalt: water: cement = 100: (5-15): (10-15): (5-10): (1-3), and the aggregate is any one of neutral aggregate and neutral alkaline aggregate.
3. The asphalt pavement structure using steel slag in a full-grained fine manner as claimed in claim 1, characterized in that: The aggregate has a particle size of 9.5-16 mm, and the seal layer is a synchronous crushed stone seal layer.
4. The asphalt pavement structure using steel slag in a full-grained fine manner as claimed in claim 1, characterized in that: The graded crushed stone layer also includes crushed stone, and GA-4 graded crushed stone is used. The particle size of the steel slag aggregate is less than 19 mm.