A high elastic rubber liquid phase production process

By using ultrasonic treatment of dispersion and mixed liquid in the rubber liquid phase production process, the nanoscale uniform dispersion is maintained, and the structural irregularity caused by the interruption of macromolecular chains in traditional rubber products is solved, and high elasticity and excellent wear performance are achieved. .

CN113563612BActive Publication Date: 2024-11-15WUXI RUIAO MINING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110866373.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-29
Publication Date
2024-11-15
Estimated Expiration
2041-07-29

AI Technical Summary

Technical Problem

During the production process of traditional rubber products, the macromolecular chains of natural rubber are interrupted, resulting in irregular network structure of the crosslinked molecular chains, affecting their elasticity and elongation, especially inadequate performance under wet wear conditions of mud and sand.

Method used

In the rubber liquid phase production process, the dispersion and mixed liquid are treated ultrasonically to keep the solute particles evenly dispersed at the nanometer level and avoid agglomeration. Liquid mixing and microwave heating and dehydration are used to ensure the integrity of the molecular chain network structure after crosslinking.

Benefits of technology

The production of high elastic rubber products has been achieved. The product has far surpassed traditional dry adhesive products in terms of elasticity and elongation. Its performance has been significantly improved especially under wet wear conditions of mud and sand, and the vulcanized cross-linking grid is ideal, reducing the formation of miscellaneous bonds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003187463400000041
    Figure BDA0003187463400000041
Patent Text Reader

Abstract

The invention discloses a high-elasticity rubber liquid phase production process, which relates to the field of rubber production process, and comprises the steps of preparing dispersion liquid, grinding, crushing, mixing, drying, forming lamination, vulcanization and the like, wherein the mass fractions of pure natural rubber, accelerator solute, crosslinking agent solute, antioxidant solute and zinc oxide in the mixed liquid are as follows: 100 parts of pure natural rubber, 1-1.5 parts of accelerator solute, 1-1.5 parts of crosslinking agent solute, 1-2 parts of antioxidant solute and 3-6 parts of zinc oxide; in the step of grinding the dispersion liquid to dryness to form a film, ultrasonic wave is added in each step to make the particles of the solute in the dispersion liquid uniformly dispersed in the natural rubber at nanometer level without agglomeration, so that the reaction is complete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of rubber production technology, and in particular to a high-elasticity rubber liquid phase production technology. Background Art

[0002] At present, most industrial rubber products are mixed rubber products with natural rubber as the main component and synthetic rubber as the auxiliary component. Natural rubber is obtained by collecting latex from rubber trees, solidifying, dehydrating and drying it to make dry rubber, which is then transported to the factory for cutting, plasticizing, mixing and vulcanization to produce the rubber products we need. This traditional rubber refining process must break the macromolecular chain of natural rubber and reduce its plasticity to facilitate mixing with other synthetic rubbers and additives to finally produce rubber products.

[0003] The dry rubber breaks the macromolecular chains and then cross-links them into a network of molecular chains through vulcanization. Because some of the broken macromolecular chains are CC bonds, not double bonds, and cross-linking can only be carried out on double bonds, the original state of natural rubber cannot be restored.

[0004] The liquid phase process is to mix the latex rubber and the nano-scale additives, mix them evenly in liquid state, and then use microwave heating to dehydrate. From the above liquid mixing process, it can be seen that the macromolecular chain is not interrupted, which ensures the original regularity of the molecular chain network structure after cross-linking, so that the stress distribution is more uniform after stress. In practical application, the product is far superior to the products produced by dry rubber in terms of elasticity and elongation, especially under mud and sand wet wear conditions, the performance is more outstanding, which is 5 to 8 times that of dry rubber products. Since the particles in the additive are particularly easy to condense in the nano-scale state, making the additive uniformly dispersed in the latex has become the key to liquid phase production. If the particle size of the additive after treatment is as small as possible and the size is consistent, the vulcanized cross-linked network can reach the ideal mode, reduce cross-linking impurities such as single sulfur bonds, disulfide bonds, and cyclic sulfur bonds, and ensure the ideal type and integrity of the cross-linked network. Summary of the invention

[0005] The purpose of the invention is to provide a high-elastic rubber liquid phase production process.

[0006] The innovation of the present invention is that in each step of grinding the dispersion to dryness to form a film, ultrasonic waves are added to keep the particles of the solute in the dispersion uniformly dispersed in the natural rubber at nanometer level without agglomeration, so that the reaction is complete.

[0007] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is:

[0008] A high elastic rubber liquid phase production process comprises the following steps:

[0009] (1) Dispersions are prepared respectively, and the weight proportions of the components of each dispersion are as follows:

[0010] Accelerator dispersion: 46-50 parts of accelerator solute, 42-48 parts of water, 0.6-1 part of dispersant;

[0011] Crosslinking agent dispersion: 60-70 parts of crosslinking agent solute, 30-40 parts of water, 1.5-2 parts of dispersant;

[0012] Antioxidant dispersion: 60-70 parts of antioxidant solute, 48-55 parts of water, 1.2-2 parts of dispersant;

[0013] Active agent dispersion: 46-55 parts zinc oxide, 48-55 parts water, 1.5-2 parts dispersant

[0014] (2) Grinding: Grinding each dispersion until the particle diameter of the solute in the dispersion reaches the nanometer level;

[0015] (3) Crushing: Use ultrasonic waves to crush each dispersion, keep the particle diameter of the solute in the dispersion at the nanometer level, and the crushing time is 30 to 60 minutes;

[0016] (4) Mixing: Each dispersion is mixed with pure natural rubber to form a mixed solution, and ultrasonic vibration is used to vibrate the mixed solution during the mixing. The mass ratio of pure natural rubber, accelerator solute, crosslinking agent solute, antioxidant solute, and zinc oxide in the mixed solution is: 100 parts of pure natural rubber, 1-1.5 parts of accelerator solute, 1-1.5 parts of crosslinking agent solute, 1-2 parts of antioxidant solute, and 3-6 parts of zinc oxide;

[0017] (5) Drying: Drying is performed immediately after the mixed solution is prepared. The mixed solution is dried by hot air and high-frequency microwave drying to dry the mixed solution into a film. Ultrasonic waves are also added during the drying process until a film is formed, so that the water content of the film is less than 2%;

[0018] (6) Forming and laminating: The dried film is plasticized by a rubber mixer to make the Mooney viscosity of the film reach 40-60. The film is rolled into a flat sheet by a calender. The laminating machine first stacks the film into the required thickness and then shapes and cuts the film.

[0019] (7) Vulcanization: vulcanize the film.

[0020] In the step of grinding the dispersion to dryness to form a film, ultrasonic waves are added in each step to keep the particles of the solute in the dispersion uniformly dispersed in the natural rubber at nanometer level without agglomeration, so that the reaction is complete.

[0021] Furthermore, in step (5), the drying temperature is 60 to 90°C

[0022] Furthermore, in step (7), the vulcanization temperature is 120-140° C., and the vulcanization time is 210-270 min.

[0023] The beneficial effects of the present invention are:

[0024] 1. In the step of grinding the dispersion to dryness to form a film, ultrasonic waves are added in each step to keep the solute particles in the dispersion uniformly dispersed in the natural rubber at nanometer level without agglomeration, so that the reaction is complete. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below.

[0026] Embodiment 1: A high elastic rubber liquid phase production process, firstly, separately prepare dispersions, the weight proportions of the components of each dispersion are: accelerator dispersion: 46 parts, 48 ​​parts of accelerator solute, 1 part of dispersant; crosslinker dispersion: 60 parts of crosslinker solute, 40 parts of water, 2 parts of dispersant; antioxidant dispersion: 60 parts of antioxidant solute, 55 parts of water, 2 parts of dispersant; activator dispersion: 46 parts of zinc oxide, 55 parts of water, 2 parts of dispersant; then grind each dispersion, the particle diameter of the solute in the dispersion reaches nanometer level; then use ultrasonic wave to crush each dispersion, the particle diameter of the solute in the dispersion remains at nanometer level, and the crushing time is 30 minutes; each dispersion is mixed with pure natural rubber to form a mixed liquid, and ultrasonic wave is used to vibrate the mixed liquid while mixing, The mass ratio of pure natural rubber, accelerator solute, crosslinker solute, antioxidant solute and zinc oxide in the mixed liquid is: 100 parts of pure natural rubber, 1 part of accelerator solute, 1 part of crosslinker solute, 1 part of antioxidant solute and 3 parts of zinc oxide; drying is performed immediately after the mixed liquid is prepared, and the mixed liquid is dried by hot air and high-frequency microwave at a drying temperature of 60°C to dry the mixed liquid into a film, and ultrasonic waves are also added during the drying process until a film is formed, so that the water content of the film is less than 2%; then a rubber mixer is used to plasticize the dried film to make the Mooney viscosity of the film reach 40, the film is rolled into a flat sheet by a calender, the film is first stacked into a required thickness by a stacking machine, and then the film is shaped and cut, and finally the film is vulcanized at a vulcanization temperature of 120°C and a vulcanization time of 210 minutes.

[0027] Embodiment 2: A high elastic rubber liquid phase production process, firstly, respectively prepare dispersions, the weight proportions of the components of each dispersion are: accelerator dispersion: accelerator solute 50 parts, water 42 parts, dispersant 0.6 parts; crosslinker dispersion: crosslinker solute 70 parts, water 30 parts, dispersant 1.5 parts; antioxidant dispersion: antioxidant solute 70 parts, water 48 parts, dispersant 1.2 parts; active agent dispersion: zinc oxide 55 parts, water 48 parts, dispersant 1.5 parts; then grind each dispersion, the particle diameter of the solute in the dispersion reaches nanometer level; then use ultrasonic wave to crush each dispersion, the particle diameter of the solute in the dispersion remains nanometer level, and the crushing time is 60 minutes; each dispersion is mixed with pure natural rubber to form a mixed solution, and ultrasonic vibration is used to mix the mixture while mixing. The mixed liquid comprises the following mass proportions: 100 parts of pure natural rubber, 1.5 parts of accelerator solute, 1.5 parts of crosslinker solute, 2 parts of antioxidant solute and 6 parts of zinc oxide; drying is performed immediately after the mixed liquid is prepared, and the mixed liquid is dried by hot air and high-frequency microwave at a drying temperature of 90° C., so that the mixed liquid is dried into a film, and ultrasonic waves are also added during the drying process until a film is formed, so that the water content of the film is less than 2%; then a rubber mixer is used to plasticize the dried film so that the Mooney viscosity of the film reaches 60, the film is rolled into a flat sheet by a calender, the film is first stacked into a desired thickness by a stacking machine, and then the film is shaped and cut, and finally the film is vulcanized at a vulcanization temperature of 140° C. and a vulcanization time of 270 min.

[0028] Embodiment 3: A high elastic rubber liquid phase production process, firstly, respectively prepare dispersions, the weight proportions of the components of each dispersion are: accelerator dispersion: 48 parts of accelerator solute, 46 parts of water, and 1.8 parts of dispersant; crosslinker dispersion: 65 parts of crosslinker solute, 35 parts of water, and 1.8 parts of dispersant; antioxidant dispersion: 65 parts of antioxidant solute, 50 parts of water, and 1.8 parts of dispersant; active agent dispersion: 50 parts of zinc oxide, 50 parts of water, and 1.8 parts of dispersant; then grind each dispersion, and the particle diameter of the solute in the dispersion reaches the nanometer level; then use ultrasonic wave to crush each dispersion, and the particle diameter of the solute in the dispersion remains at the nanometer level, and the crushing time is 45 minutes; each dispersion is mixed with pure natural rubber to form a mixed liquid, and ultrasonic vibration is used to mix while mixing The mixed solution comprises the following parts: 100 parts of pure natural rubber, 1.2 parts of accelerator solute, 1.2 parts of crosslinker solute, 1.5 parts of antioxidant solute and 4 parts of zinc oxide; drying is performed immediately after the mixed solution is prepared; the mixed solution is dried by hot air and high-frequency microwave at a drying temperature of 70° C., so that the mixed solution is dried into a film; ultrasonic waves are also added during the drying process until a film is formed, so that the water content of the film is less than 2%; then a rubber mixer is used to plasticize the dried film so that the Mooney viscosity of the film reaches 50; the film is rolled into a flat sheet by a calender; a laminating machine first stacks the film into a desired thickness, and then shapes and cuts the film; and finally the film is vulcanized at a vulcanization temperature of 130° C. and a vulcanization time of 240 min.

[0029] The data comparison in Table 1 shows that the physical indicators of the rubber produced by the preparation process provided in Examples 1, 2 and 3 are better than those of the rubber produced by the dispersion without crushing.

[0030] Table 1

[0031]

[0032] The described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A high elastic rubber liquid phase production process, characterized in that: The following steps are involved: Prepare the dispersions separately, and the weight proportions of the components of each dispersion are as follows: Accelerator dispersion: 46-50 parts of accelerator solute, 42-48 parts of water, 0.6-1 part of dispersant; Crosslinking agent dispersion: 60-70 parts of crosslinking agent solute, 30-40 parts of water, 1.5-2 parts of dispersant; Antioxidant dispersion: 60-70 parts of antioxidant solute, 48-55 parts of water, 1.2-2 parts of dispersant; Active agent dispersion: 46-55 parts of zinc oxide, 48-55 parts of water, 1.5-2 parts of dispersant; Grinding: Grind each dispersion until the particle diameter of the solute in the dispersion reaches nanometer level; Crushing: Use ultrasonic waves to crush each dispersion, the particle diameter of the solute in the dispersion remains at nanometer level, and the crushing time is 30 to 60 minutes; Mixing: Each dispersion is mixed with pure natural rubber to form a mixed solution, and ultrasonic vibration is used to vibrate the mixed solution. The mass ratio of pure natural rubber, accelerator solute, crosslinking agent solute, antioxidant solute and zinc oxide in the mixed solution is: 100 parts of pure natural rubber, 1-1.5 parts of accelerator solute, 1-1.5 parts of crosslinking agent solute, 1-2 parts of antioxidant solute and 3-6 parts of zinc oxide; Drying: Drying is performed immediately after the mixed liquid is prepared. The mixed liquid is dried by hot air and high-frequency microwave to dry the mixed liquid into a film. Ultrasonic waves are also added during the drying process until a film is formed, so that the water content of the film is less than 2%; the drying temperature is 60-90°C; Forming and laminating: The dried film is plasticized by a rubber mixer to make the Mooney viscosity of the film reach 40-60. The film is rolled into a flat sheet by a calender. The laminating machine first stacks the film into the required thickness and then shapes and cuts the film. Vulcanization: vulcanize the film; the vulcanization temperature is 120-140°C, and the vulcanization time is 210-270 minutes.