Lignin-based adhesive material, preparation method thereof, adhesive and glued product
By reacting with lignin with choline chloride and natural small molecule hydroxy aromatic aldehyde with lignin, lignin-based adhesive materials that do not require modification are prepared, solving the toxicity and cost problems of existing resin adhesives. , realizes high-performance, green and environmentally friendly adhesives, suitable for a variety of wood products.
Patent Information
- Application Number
- CN202411247394.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-05
AI Technical Summary
Existing resin-based adhesives release formaldehyde during use are harmful to the human body and the environment, the preparation process is complex and the raw material cost is high, and replacement aldehyde compounds are still toxic, making it difficult to achieve green and environmentally friendly low-cost adhesives.
A low-melt solvent is used to mix choline chloride with natural small molecule hydroxy aromatic aldehyde, as a solvent and an aldehyde donor, react with lignin to form a lignin-based adhesive material that does not require modification, and is used directly as an adhesive, with Strong bonding properties and bending strength.
Realize green and environmentally friendly low-cost adhesives, simplify the preparation process, avoid the use of toxic and harmful substances, and has better performance than traditional resin adhesives. It is suitable for density boards, plywood and bamboo wrapping products, with excellent water resistance and mildew resistance .
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to a lignin-based adhesive material, a preparation method thereof, an adhesive and an adhesive product. Background Art
[0002] At present, adhesives are widely used in the market, especially in furniture that people often come into contact with. The adhesives used for common density boards and plywoods are resin adhesives such as urea-formaldehyde resins and phenolic resins, which are also commonly used adhesives on the market. This type of adhesive contains a large amount of volatile aldehyde compounds, such as formaldehyde. This substance is very harmful to the human body and the environment. Therefore, when using this type of density board, plywood and particleboard, the formaldehyde volatilized from it may cause damage to the human body. Moreover, the preparation process of this type of adhesive is complicated, the raw material cost is high, and the raw materials used are toxic and harmful, and are not green and environmentally friendly. Therefore, people need a simple preparation process, green and environmentally friendly, low-cost adhesive to replace them.
[0003] In order to solve this kind of problem, lignin is used in the related art to replace phenol in traditional phenolic resins, but most of the adhesives using lignin need to be modified in various ways or partially replaced by lignin due to the low reactivity of lignin itself. This is not only cumbersome, but also increases the process cost. Not only that, most adhesives in the related art continue to use formaldehyde to react with lignin, and some use less toxic furfural or glyoxal to replace formaldehyde. Using low-toxic aldehydes to replace formaldehyde is indeed greener and more environmentally friendly, but these aldehyde compounds still have certain toxicity and are more expensive. Summary of the invention
[0004] In view of this, the technical problem to be solved by the present invention is to provide a lignin-based adhesive material, a preparation method thereof, an adhesive and a bonding product. The lignin-based adhesive material provided by the present invention uses lignin instead of phenol, does not require modification of lignin, can be directly used as an adhesive, and has strong bonding properties and bending strength.
[0005] The present invention provides a lignin-based adhesive material, which is obtained from a deep eutectic solvent and lignin;
[0006] The low eutectic solvent comprises choline chloride and natural small molecule hydroxy aromatic aldehyde.
[0007] The low eutectic solvent of the present invention is a natural small molecule aldehyde-based low eutectic solvent, which includes choline chloride and natural small molecule hydroxy aromatic aldehyde, wherein the choline chloride is a hydrogen bond acceptor, and the natural small molecule hydroxy aromatic aldehyde is a hydrogen bond donor. The two are mixed in a certain ratio to form a stable hydrogen bond to obtain a clear and transparent low eutectic solvent. The molar ratio of choline chloride to natural small molecule hydroxy aromatic aldehyde of the present invention is 1: (1-3), and the most preferred ratio is 1: 2. Relevant preliminary experiments show that more or less hydrogen bond donors cannot form a stable hydrogen bond structure.
[0008] In certain embodiments of the present invention, the natural small molecule hydroxy aromatic aldehyde is selected from at least one of vanillin, ethyl vanillin, o-vanillin, salicylaldehyde or protocatechuic aldehyde. The natural small molecule hydroxy aromatic aldehyde in the deep eutectic solvent of the present invention is preferably selected from vanillin. Vanillin has lower cost, higher reaction activity, and better performance of adhesives prepared with lignin. Compared with hydroxy aromatic aldehydes such as ethyl vanillin, o-vanillin, salicylaldehyde, and protocatechuic aldehyde, vanillin is the best substitute for formaldehyde.
[0009] In certain embodiments of the present invention, the lignin and the natural small molecule hydroxy aromatic aldehyde of the present invention are both derived from biomass raw materials, which are low-cost, easy to obtain, and avoid the introduction of substances such as phenol and formaldehyde, making the product more environmentally friendly. In certain embodiments of the present invention, the source of the lignin compound includes: one or more of straw, rice husk and corn cob; the source of the natural small molecule hydroxy aromatic aldehyde includes: one or more of vanilla beans or beets.
[0010] The present application adopts a natural small molecule aldehyde-based low eutectic solvent as both a solvent and an aldehyde donor, which can react with lignin to produce a lignin-based adhesive material. Lignin is used to replace phenol without modifying the lignin, and food-grade non-toxic and harmless natural hydroxyl aromatic aldehyde is used to replace formaldehyde. The obtained lignin-based adhesive material can be directly used as an adhesive and has strong bonding properties and bending strength.
[0011] The present invention also provides a method for preparing a lignin-based adhesive material according to any of the above technical solutions, comprising the following steps: reacting a low eutectic solvent with lignin to obtain a lignin-based adhesive material. The low eutectic solvent and lignin in the present invention are the same as those described above and will not be described in detail.
[0012] The deep eutectic solvent of the present invention is obtained by mixing choline chloride with a natural small molecule hydroxy aromatic aldehyde; specifically, the deep eutectic solvent is obtained by mixing choline chloride with a natural small molecule hydroxy aromatic aldehyde in a molar ratio of 1: (1-3), preferably by mixing choline chloride with a natural small molecule hydroxy aromatic aldehyde in a molar ratio of 1: 2. The mixing temperature of the present invention is 80°C to 100°C, and the mixing time is 20 min to 40 min.
[0013] The present invention first reacts a low eutectic solvent and lignin; specifically, the low eutectic solvent and lignin are dispersed and then reacted. In certain embodiments of the present invention, the lignin is evenly dispersed in the low eutectic solvent and then reacted. The dispersion temperature of the present invention is 80°C to 100°C, preferably 90°C, and the dispersion time is 6h to 12h. The present invention allows lignin to be evenly dispersed in the low eutectic solvent, which can allow lignin to be more fully contacted with the natural small molecule hydroxy aromatic aldehyde in the low eutectic solvent, thereby making the reaction more complete, and at the same time, the use of organic solvents can be eliminated, so that the reaction does not produce any waste, and the "one pot three-step method" for preparing adhesives is realized.
[0014] The present invention reacts the low eutectic solvent and lignin, the reaction temperature is 120°C to 140°C, and the reaction time is 8 h to 10 h. The present invention heats the reaction to 120 to 140°C to reach a temperature for the polymerization reaction of lignin and the natural small molecule hydroxy aromatic aldehyde in the low eutectic solvent, and the reaction is completed to obtain a lignin-based adhesive material with the best performance.
[0015] The present invention reacts the low eutectic solvent and lignin, specifically reacting the low eutectic solvent, lignin and alkali catalyst materials according to a mass ratio of (1.9~2.1):1:(0~0.05). In certain embodiments of the present invention, (19~21) g of low eutectic solvent, 10 g of lignin and (0~0.5) g of alkali catalyst are reacted. The alkali catalyst of the present invention includes at least one of sodium hydroxide, sodium carbonate or sodium bicarbonate. If the low eutectic solvent is too little, the lignin cannot be completely dispersed, resulting in incomplete reaction. If the low eutectic solvent is too much, the viscosity of the entire system will decrease, so that the produced adhesive is immersed in the low eutectic solvent, which affects its bonding strength. Therefore, when the mass ratio of the low eutectic solvent to lignin is close to 2:1, the obtained lignin-based adhesive material has the best performance.
[0016] The present invention also provides an adhesive, which is the lignin-based adhesive material described in any of the above technical solutions; or, it includes the above lignin-based adhesive material and an additive. The above lignin-based adhesive material of the present invention can be used directly as an adhesive, or it can be used together with an additive as an adhesive.
[0017] The present invention also provides a glued product, which is obtained from a wood raw material and an adhesive; the adhesive is the lignin-based adhesive material described in any of the above technical solutions; or the adhesive includes the lignin-based adhesive material described in any of the above technical solutions and an additive; the wood raw material is selected from bamboo powder or poplar wood board. The adhesive of the present invention is suitable for density board, plywood, particle board and bamboo winding products.
[0018] The present invention obtains a glued product after heat treatment of the wood raw material and the adhesive. The glued product prepared by the lignin-based adhesive material of the present invention has excellent water resistance; in one embodiment of the present invention, the glued product is a plywood, which has much better water resistance than moso bamboo board (MBB), bamboo flour board (BFB) and commercially available high-density fiberboard (HDF), and due to the presence of choline chloride and natural small molecule hydroxy aromatic aldehyde in the low eutectic solvent, it also has excellent mildew resistance. Therefore, the glued product obtained by the present invention is not only green and environmentally friendly, but also has stronger performance and lower cost.
[0019] In one embodiment of the present invention, bamboo powder and any of the above-mentioned lignin-based adhesive materials are mixed by banburying, then hot pressed, and cooled to obtain a high-performance density board. The hot pressing of the present invention is carried out at 110°C~130°C and a pressure of 20MPa~40 MPa for 20 min~40 min. The mass ratio of the bamboo powder and the lignin-based adhesive material of the present invention is 1:(1~3), and the preferred mass ratio is 1:2; the bonding strength of the lignin-based adhesive material to the bamboo board at room temperature is 4.24 (±0.26) MPa. Preliminary experiments have shown that if there is too much bamboo powder, its performance will decrease, and if there is too little bamboo powder, its performance will not be improved much, but the cost will increase. The density board obtained by the present invention has a bending strength of 43.21 (±2.45) MPa and an internal bonding strength of 6.8 (±0.4) MPa. The commercially available high-density fiberboard has a bending strength of 21.76 MPa and an internal bonding strength of 1.17 MPa. In comparison, the density board of the present invention has better performance, is greener and has lower cost.
[0020] In another embodiment of the present invention, a plurality of poplar wood boards are coated with the lignin-based adhesive material described in any of the above technical solutions and then hot-pressed, and high-strength plywood is obtained after cooling. The bonding strength of the lignin-based adhesive material described in the present invention to poplar wood is 5.08 (± 0.3) MPa at room temperature. The coating amount of the coating described in the present invention is 100 g / m 2 ~150g / m 2The hot pressing pressure of the present invention is 2 MPa~4 MPa, and the hot pressing time is 20 min~40 min; under the hot pressing condition of 2 MPa, the bending strength of the plywood is 68.14 (±4.2) MPa; under the hot pressing condition of 4 MPa, the bending strength of the plywood is 78.77 (±4.8) MPa. The bending strength of the plywood is much greater than 27.86 MPa of the poplar plywood sold on the market.
[0021] Based on the above technical solution, the lignin-based adhesive material provided by the present invention includes at least one of the following beneficial effects:
[0022] (1) The present invention first mixes choline chloride as a hydrogen bond acceptor and a natural small molecule hydroxy aromatic aldehyde as a hydrogen bond donor in a certain proportion to form a stable hydrogen bond, thereby obtaining a clear and transparent low eutectic solvent as a dispersant, and then adds lignin to the low eutectic solvent. After the lignin is evenly dispersed, the temperature is increased to polymerize the lignin with the natural small molecule hydroxy aromatic aldehyde in the low eutectic solvent to obtain a lignin-based adhesive. The lignin and natural small molecule hydroxy aromatic aldehyde in the raw materials of the present invention can all be derived from biomass raw materials, which are low in cost and easy to obtain. The natural small molecule hydroxy aromatic aldehyde is preferably vanillin. Vanillin is a food additive that is non-toxic and harmless and is an excellent substitute for formaldehyde, while lignin is an excellent substitute for phenol. Therefore, compared with phenolic resin and urea-formaldehyde resin adhesives, the lignin-based adhesive is more environmentally friendly, has a simple process, and is low in cost.
[0023] (2) The present invention uses a low eutectic solvent as a dispersant, which can reduce the damage of the solvent to the lignin structure and can also make lignin and vanillin fully contact, so that the reaction is relatively complete. In addition, the present invention prepares the lignin-based adhesive through a "one-pot three-step method", which is simple and efficient to operate, produces less three wastes, and is easy to industrialize. In addition, no toxic and harmful substances such as phenol and formaldehyde are introduced during the preparation process, which is a green and environmentally friendly adhesive processing technology.
[0024] (3) The high-performance density board obtained by the lignin-based adhesive material and bamboo powder of the present invention has performance far superior to the high-density fiberboard currently on the market, and is an excellent substitute for density board and plastic board. The high-performance plywood obtained by the lignin-based adhesive material and poplar board of the present invention also has performance superior to the common poplar plywood currently on the market. The lignin-based adhesive material of the present invention has high bonding strength to both poplar board and bamboo board, which far exceeds the national requirement standard for phenolic resin wood adhesive, which is bonding strength ≥0.7 MPa (GB / T 14732-2017). In addition, the preparation process is simple, the raw materials are non-toxic and harmless, the cost is low, no by-products are generated in the production process, and it is green and environmentally friendly. It is especially used as a safe, reliable and stable adhesive in furniture and industry, which can improve the quality of adhesives used in wood, has good economic and social benefits, and has broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A schematic diagram of the bonding strength of the lignin-based adhesive prepared in Example 1 of the present invention at room temperature;
[0026] Figure 2 This is an appearance diagram of a density board prepared in Example 2 of the present invention;
[0027] Figure 3 The bending strength and internal bonding strength test results of the density board prepared in Example 2 of the present invention are shown in FIG.
[0028] Figure 4 This is a comparison chart of the bending strength test results of the plywood prepared in Example 3 of the present invention;
[0029] Figure 5 This is a comparison chart of the mass expansion rate and thickness expansion rate results of the density board prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0030] The present invention discloses a lignin-based adhesive material, a preparation method thereof, an adhesive and an adhesive product. A person skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the above. It should be particularly noted that all similar substitutions and modifications are obvious to a person skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0031] The present invention will be further described below in conjunction with embodiments:
[0032] Example 1
[0033] Preparation of lignin-based adhesive: 3.0 g of choline chloride and 6.5 g of vanillin were mixed in a molar ratio of 1:2 and stirred at 90°C for 20 min to obtain a clear and transparent low eutectic solvent. 4.5 g of lignin was added to the low eutectic solvent, and 0.2 g of sodium carbonate as a catalyst was added. After stirring for 6 h, when the lignin was completely dispersed in the low eutectic solvent, the temperature was raised to 120°C and stirred for 8 h to obtain a lignin-based adhesive. The mass ratio of the low eutectic solvent to lignin was 2:1.
[0034] The bonding strength of the lignin adhesive obtained above on poplar board and bamboo board was tested, and the specific test process is as follows:
[0035] 1) Sample treatment: Take 0.2 g of the lignin-based adhesive prepared in Example 1 and apply it while hot on about one quarter (15×20 mm 2 ) on poplar wood chips and bamboo board samples (20 mm×60 mm×3 mm). A portion of the coated sample was placed in a hot press and the sample was hot pressed at 1.5 MPa and 120°C for 10 min, then slowly cooled to room temperature and continued cold pressing for 10 h.
[0036] 2) Room temperature (25°C) bonding performance test: The cold-pressed samples were placed at room temperature for 10 h, and then the samples were subjected to adhesion performance test using a tensile machine at a speed of 5 mm / min. The bonding strength was recorded as the maximum tensile strength.
[0037] like Figure 1 As shown, Figure 1 Schematic diagram of the bonding strength of the lignin-based adhesive prepared in Example 1 of the present invention at room temperature. The lignin-based adhesive has strong bonding strength. At room temperature, its bonding strength to the poplar board can reach 5.08 MPa, and its bonding strength to the bamboo board can also reach 4.24 MPa, which far exceeds the bonding strength (≥0.7 MPa) required by the national regulations on phenolic resin wood adhesives in GB / T 14732-2017, indicating that the lignin-based adhesive provided by the present invention meets the application needs of daily life.
[0038] Example 2
[0039] Preparation of high-performance density board: After the lignin-based adhesive prepared in Example 1 is mixed with bamboo powder in a mass ratio of 1:2, hot pressing is performed at 110°C and a pressure of 20 MPa for 20 min, and then naturally cooled to obtain a high-strength density board. The bending strength test method is the three-point bending method, and the internal bonding strength test method is tested according to GB / T31765-2015.
[0040] like Figure 2~Figure 3As shown, Figure 2 This is the appearance of the density board prepared in Example 2 of the present invention. Figure 3 The bending strength and internal bonding strength test results of the density board prepared in Example 2 of the present invention are shown in the figure. The bending strength is 43.21 (±2.45) MPa and the internal bonding strength is 6.8 (±0.4) MPa. The internal bonding strength of the density board far exceeds the 1 MPa required by the industry. This shows that the high-performance density board provided by the present invention can be used as an excellent substitute for high-density board.
[0041] Example 3
[0042] Preparation of high-performance plywood: The lignin-based adhesive prepared in Example 1 can be used to prepare plywood with poplar boards, with a coating amount of 100 g / m 2 The hot pressing conditions are 2 MPa or 4 MPa, hot pressing for 20 min, and after natural cooling, high-performance plywood can be obtained. The test method for the bending strength of the plywood is still the three-point bending method.
[0043] like Figure 4 As shown, Figure 4 The bending strength test results of the plywood prepared in Example 3 of the present invention are compared. Under 2MPa hot pressing conditions, the bending strength of the plywood is 68.14 (±4.2) MPa; under 4MPa hot pressing conditions, the bending strength of the plywood is 78.77 (±4.8) MPa. The bending strength of the plywood is much greater than 27.86MPa of the poplar plywood sold on the market. It meets the national standard of GB / T 9846-2015, indicating that the plywood meets the requirements of daily use. In addition, the plywood of the present invention does not contain formaldehyde, and its performance is better than the poplar plywood on the market, and it is an excellent substitute for it.
[0044] Example 4
[0045] Preparation of lignin-based adhesive: Choline chloride and ethyl vanillin were mixed in a molar ratio of 1:2 and stirred at 90°C for 20 min to obtain a clear and transparent low eutectic solvent. 4.5 g of lignin was added to the low eutectic solvent, and 0.1 g of sodium hydroxide as a catalyst was added. After stirring for 6 h, when the lignin was completely dispersed in the low eutectic solvent, the temperature was raised to 120°C and stirred for 8 h to obtain a lignin-based adhesive. The mass ratio of the low eutectic solvent to lignin was 2:1.
[0046] Example 5
[0047] Water resistance and mildew resistance test: The density board prepared in Example 2 was immersed in ultrapure water for 24 h, taken out and dried, and its mass increase rate (WA) and thickness increase rate (TS) were tested. Figure 5 As shown, Figure 5The comparison chart of the mass expansion rate and thickness expansion rate of the density board prepared in Example 2 of the present invention is shown in FIG. Figure 5 It can be seen that the water resistance of this density board is much higher than that of moso bamboo board (MBB), bamboo flour board (BFB) and commercially available high-density fiberboard (HDF).
[0048] In addition, due to the presence of choline chloride and at least one of hydroxy aromatic aldehydes such as vanillin, ethyl vanillin, o-vanillin, salicylaldehyde, and protocatechuic aldehyde, the board also has excellent mildew resistance. The bamboo board and the bamboo powder board will be moldy in 4 to 7 days in a humid environment, while the commercially available high-density fiberboard will also be moldy in 7 to 10 days, and the density board of Example 2 will not be moldy after 15 days.
[0049] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. Lignin-based adhesive material, characterized in that It is obtained from a deep eutectic solvent and lignin; The deep eutectic solvent comprises choline chloride and natural small molecule hydroxy aromatic aldehyde.
2. The lignin-based adhesive material according to claim 1, characterized in that The natural small molecule hydroxy aromatic aldehyde is selected from at least one of vanillin, ethyl vanillin, o-vanillin, salicylaldehyde or protocatechuic aldehyde.
3. The lignin-based adhesive material according to claim 1, characterized in that The molar ratio of the choline chloride to the natural small molecule hydroxy aromatic aldehyde is 1:(1-3).
4. The lignin-based adhesive material according to claim 1, characterized in that The lignin and the natural small molecule hydroxy aromatic aldehyde are both derived from biomass raw materials.
5. The method for preparing the lignin-based adhesive material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The low eutectic solvent and lignin are reacted to obtain a lignin-based adhesive material.
6. The preparation method according to claim 5, characterized in that The specific steps include: A low eutectic solvent, lignin and an alkali catalyst are reacted in a mass ratio of (1.9-2.1):1:(0-0.05) to obtain a lignin-based adhesive material.
7. The preparation method according to claim 5, characterized in that The reaction temperature is 120° C. to 140° C., and the reaction time is 8 h to 10 h.
8. The preparation method according to claim 5, characterized in that The deep eutectic solvent is obtained by mixing the choline chloride and a natural small molecule hydroxy aromatic aldehyde; The mixing temperature is 80° C. to 100° C., and the mixing time is 20 min to 40 min.
9. Adhesive, characterized in that It is the lignin-based adhesive material according to any one of claims 1 to 4; Alternatively, it comprises the lignin-based adhesive material according to any one of claims 1 to 4 and an additive.
10. Glued product, characterized in that It is obtained from wood raw materials and adhesives; The adhesive is the lignin-based adhesive material according to any one of claims 1 to 4; Alternatively, the adhesive comprises the lignin-based adhesive material according to any one of claims 1 to 4 and an additive.
Citation Information
Patent Citations
Method for preparing phenolic aldehyde adhesive based on lignin phenolized liquid and application thereof
CN101260283A
Method of producing aldehyde-free lignin-based wood adhesive by using lignin
CN107286905A
Preparation method and application of lignin-based biomass aldehyde-free adhesive
CN109868100A
Method for producing phenol-based resin adhesive
JP2007169491A
Cited By
Green, low-cost and high-performance lignin adhesive as well as preparation method and application thereof
CN120290136A