A solid phase reaction grinding disc for SiC wafer grinding and its preparation method and application

By introducing catalyst and hydrogen peroxide into the SiC wafer grinding disc to generate hydroxyl radicals with extremely strong oxidation properties, forming a soft oxide layer, solving the problems of low processing efficiency and large damage in the existing technology, and achieving high efficiency and low damage precision grinding effect.

CN113601390BActive Publication Date: 2024-11-22GUANGDONG NANOGRIND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110876310.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-31
Publication Date
2024-11-22
Estimated Expiration
2041-07-31

AI Technical Summary

Technical Problem

The lack of solid-phase reaction grinding discs suitable for silicon carbide (SiC) wafers in the prior art, resulting in low processing efficiency and large damage to SiC wafers, and the complexity of existing devices is not conducive to industrial applications.

Method used

Design a solid phase reaction grinding disc, consisting of a base plate, filler and abrasive block. The filler and abrasive block are distributed with catalysts. Combined with hydrogen peroxide abrasive liquid, it generates hydroxyl radicals with extremely strong oxidation properties, and forms a soft oxide layer. Reduce wafer damage.

Benefits of technology

It improves the processing efficiency and surface quality of SiC wafers, reduces damage to the wafer by the grinding disc, and is suitable for high-precision grinding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113601390B_ABST
    Figure CN113601390B_ABST
Patent Text Reader

Abstract

The present invention relates to a solid phase reaction grinding disc for grinding SiC wafers, and a preparation method and application thereof. The solid phase reaction grinding disc comprises a base disc, a filler stacked on the base disc, and a plurality of abrasive blocks embedded in the filler and flush with the surface of the filler; the filler is provided with pores penetrating the filler; the filler is composed of a catalyst and a grinding aid; the abrasive block is composed of a mixture of abrasive, catalyst and adhesive; the catalyst is iron-containing particles. The solid phase reaction grinding disc provided by the present invention is suitable for grinding SiC wafers, and can not only obtain a higher material removal rate and better surface quality, but also obtain a low-damage SiC wafer surface, and can be used for precision grinding of SiC wafers with higher surface requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of SiC wafer processing, and in particular relates to a solid phase reaction grinding disc for SiC wafer grinding and a preparation method and application thereof. Background Art

[0002] As a third-generation semiconductor material, silicon carbide (SiC) wafers have a large bandgap, high electron mobility, high breakdown electric field, high thermal conductivity and strong radiation resistance, and are one of the most promising semiconductor materials. In order to meet the requirements of epitaxial film growth of SiC wafers, their surface must be ultra-smooth, defect-free, and free of surface / subsurface damage. When there are tiny defects on the surface of the wafer, they will be transferred to the epitaxial growth film and become defects of the device. Therefore, the surface quality and precision of the SiC wafer directly determine the performance of SiC semiconductor devices. Silicon carbide wafers need to go through a series of process flows such as cutting, grinding, and polishing to produce qualified SiC substrates, but due to their high hardness, high brittleness physical properties and very stable chemical properties, high-quality and high-efficiency surface precision processing is very difficult. For this reason, some scholars have introduced chemical reactions in the processing process to reduce surface / subsurface damage, namely chemical mechanical polishing. Chemical reactions occur during the processing process to oxidize the wafer surface, which can obtain low surface roughness and damage-free surfaces. However, when chemical mechanical polishing is used to process SiC wafers, although a damage-free, low-roughness surface can be obtained, the processing efficiency is low and it can only be used for the final processing of SiC wafers.

[0003] In order to improve the processing efficiency, some scholars have proposed adding chemical reactions and solid-phase reaction grinding discs during the grinding process. The solid-phase reaction grinding disc combines the advantages of fixed abrasive grinding and chemical mechanical polishing, and uses the corresponding components in the grinding disc to react with the wafer surface under certain conditions to generate an oxide layer, thereby avoiding direct contact between the abrasive particles and the wafer surface, reducing the damage to the wafer surface, and at the same time, due to the presence of fixed abrasives, the processing efficiency is also guaranteed. However, due to the limitations of the solid-phase reaction, this type of grinding disc currently only has related abrasives used for materials such as sapphire and silicon wafers on the market; although there are reports of methods for using solid-phase reaction to achieve fine processing of silicon carbide (patent CN110355613A), the equipment involved is complex and the process is cumbersome, which is not conducive to the promotion of industrial applications.

[0004] Therefore, the development of solid phase reaction related grinding tools suitable for silicon carbide has important research significance and economic value. Summary of the invention

[0005] The purpose of the present invention is to overcome the lack of grinding tools for fine processing of SiC wafers using solid phase reaction in the prior art, and to provide a solid phase reaction grinding disc for grinding SiC wafers. The solid phase reaction grinding disc provided by the present invention is composed of a base disc, a filler, an abrasive block and pores, and any grinding surface of the solid phase reaction grinding disc is distributed with a specific catalyst; when it is ground with a grinding liquid containing hydrogen peroxide, the catalyst can react with H in the grinding liquid to form a catalyst. 2 O 2 The Fenton reaction occurs to generate highly oxidizing hydroxyl radicals (·OH). The hydroxyl radicals (·OH) react with the SiC wafer to form a soft oxide layer on the SiC surface. The oxide layer is then removed by the abrasive, which can improve the processing efficiency and reduce the damage of the grinding disc to the SiC wafer.

[0006] Another object of the present invention is to provide a method for preparing the solid phase reaction grinding disc.

[0007] Another object of the present invention is to provide application of the solid phase reaction grinding disc in grinding SiC wafers.

[0008] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:

[0009] A solid phase reaction grinding disc for grinding SiC wafers, comprising a base disc, a filler stacked on the base disc, and a plurality of abrasive blocks embedded in the filler and flush with the surface of the filler; the filler is provided with air holes penetrating the filler;

[0010] The filler is composed of a catalyst and a research aid;

[0011] The abrasive block is composed of a mixture of abrasive, catalyst and adhesive;

[0012] The catalyst is iron-containing particles.

[0013] The present invention introduces a specific catalyst into the grinding block and the filler so that any grinding surface of the entire solid phase reaction grinding disc is distributed with the specific catalyst, and the grinding efficiency can be improved by using a grinding aid; when grinding with a grinding liquid containing hydrogen peroxide, the catalyst can react with the H in the grinding liquid to form a hydrogen peroxide-containing grinding liquid. 2 O 2 The Fenton reaction occurs to generate highly oxidizing hydroxyl radicals (·OH). The hydroxyl radicals (·OH) react with the SiC wafer to form a soft oxide layer on the surface of the SiC. The oxide layer is then removed by the abrasive, which can improve the processing efficiency and reduce the damage of the grinding disc to the SiC wafer.

[0014] The solid phase reaction process is as follows:

[0015] (1)

[0016] (2)

[0017] (3).

[0018] The solid phase reaction grinding disc provided by the present invention is suitable for grinding SiC wafers, and can not only obtain a higher material removal rate and better surface quality, but also obtain a low-damage SiC wafer surface, and can be used for precision grinding processing of SiC wafers with higher surface requirements.

[0019] It should be understood that the solid phase reaction grinding disc can be prepared into different sizes according to the size of the machine tool; the content of the catalyst in the filler, and the content of the abrasive and the catalyst in the abrasive block can be selected and adjusted according to the grinding requirements.

[0020] Preferably, the weight percentage of the catalyst in the filler is 40-60%.

[0021] Preferably, the weight percentage of abrasive grains in the abrasive block is 10-30%, and the weight percentage of catalyst is 20-40%.

[0022] The content of abrasive and catalyst can also be adjusted according to specific requirements, and the type of abrasive, particle size, etc. can be reasonably selected.

[0023] Preferably, the abrasive blocks are evenly dispersed and arranged.

[0024] More preferably, the abrasive blocks are arranged in a shape of one or more of a spiral, annular, honeycomb or sunflower seed shape.

[0025] Preferably, the shape of the abrasive block is one or more of a cylinder, a cuboid or a polygonal prism.

[0026] Preferably, the upper and lower surfaces of the abrasive block are flush with the upper and lower surfaces of the filler block, respectively.

[0027] Preferably, the catalyst is one or more of ferroferric oxide, carbonyl iron powder or reduced iron powder.

[0028] Preferably, the particle size of the catalyst is 1-300 μm.

[0029] Preferably, the grinding aid is one or more of graphite powder, iron oxide powder, iron powder or stearic acid.

[0030] Preferably, the particle size of the grinding aid is 1-300 μm.

[0031] Conventional abrasives suitable for grinding silicon carbide in the art can be used in the present invention.

[0032] The types and particle sizes of abrasives can be of conventional types and particle size ranges, and can be reasonably selected and optimized according to grinding requirements.

[0033] Preferably, the abrasive is one or more of diamond, silicon carbide, cerium oxide or silicon oxide.

[0034] Preferably, the abrasive has a particle size of 1-300 μm.

[0035] Preferably, the adhesive is one or more of a resin bond, a ceramic bond or a metal bond.

[0036] Preferably, the air hole (eg, a circular hole) is disposed at the center of the filler.

[0037] Preferably, the pores penetrate the filler.

[0038] The method for preparing the solid phase reaction grinding disc comprises the following steps:

[0039] S1: mixing abrasive, catalyst and adhesive, hot pressing and curing, and demolding to obtain an abrasive block;

[0040] S2: bonding the abrasive block to the base plate;

[0041] S3: Add fillers into the gaps of the base disc and level it to obtain the solid phase reaction grinding disc.

[0042] Preferably, S1 further comprises the steps of mixing, grinding and sieving the abrasive and the catalyst before mixing.

[0043] The particle size of the abrasive and catalyst is controlled by grinding and screening.

[0044] The application of the above-mentioned solid phase reaction grinding disc in SiC wafer grinding is also within the protection scope of the present invention.

[0045] The present invention also seeks to protect a method for using the solid phase reaction grinding disc, comprising the following steps: using a grinding liquid containing hydrogen peroxide as a grinding liquid, and grinding a SiC wafer using the solid phase reaction grinding disc.

[0046] Preferably, the grinding pressure is 10-30 kPa (for example, 10 kPa, 20 kPa, 30 kPa), the grinding speed is 40-80 r / min (for example, 40 r / min, 60 r / min, 80 r / min), and the grinding time is 30-60 min (for example, 30 min, 45 min, 60 min).

[0047] Preferably, the concentration of hydrogen peroxide in the grinding liquid containing hydrogen peroxide is 5-20% wt. (for example, 5% wt., 10% wt., 15% wt., 20% wt.).

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] (1) The solid phase reaction grinding disc provided by the present invention is composed of a base disc, a filler, an abrasive block and pores. Any grinding surface of the solid phase reaction grinding disc is distributed with a specific catalyst. When the solid phase reaction grinding disc is used for grinding with a grinding liquid containing hydrogen peroxide, the catalyst can react with the H in the grinding liquid. 2 O 2 The Fenton reaction occurs, generating highly oxidizing hydroxyl radicals (·OH). The hydroxyl radicals (·OH) react with the SiC wafer to form a soft oxide layer on the surface of the SiC. The oxide layer is then removed by the abrasive, which can improve the processing efficiency and reduce the damage of the grinding disc to the SiC wafer.

[0050] (2) The solid phase reaction grinding disc provided by the present invention is suitable for grinding SiC wafers. It can not only obtain a higher material removal rate and better surface quality, but also obtain a low-damage SiC wafer surface, and can be used for precision grinding of SiC wafers with higher surface requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 A schematic diagram of the structure of the solid phase reaction grinding disc provided in Example 1;

[0052] Figure 2 A schematic diagram of the abrasive block preparation process provided in Example 1;

[0053] Figure 3 The surface morphology and surface roughness of the SiC wafer after grinding using the solid phase reaction grinding disc provided in Example 1;

[0054] Figure 4 The surface morphology and surface roughness of the SiC wafer after grinding using the solid phase reaction grinding disc provided in Example 2;

[0055] Figure 5 The surface morphology and surface roughness of the SiC wafer after grinding using the solid phase reaction grinding disc provided in Example 3;

[0056] Figure 6 The surface morphology and surface roughness of the SiC wafer after grinding using the grinding disc provided in Comparative Example 1;

[0057] Figure 7 The surface morphology and surface roughness of the SiC wafer after grinding using the grinding disk provided in Comparative Example 2.

[0058] Among them, 1 is an abrasive block, 2 is a filler, 3 is a base plate, and 4 is a mold. DETAILED DESCRIPTION

[0059] The present invention is further described below in conjunction with examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and substitutions made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention.

[0060] In each embodiment and comparative example, a white light interferometer was used to detect the surface roughness, the maximum peak-to-valley roughness Rt (defined as the sum of the absolute values ​​of the heights of the highest peak and the lowest valley of the surface morphology) and the surface morphology. Five points were taken for each piece and the average value was taken. An energy spectrometer was used to analyze the elemental composition of the wear debris and the workpiece surface. The workpiece mass was measured using an electronic analytical balance with an accuracy of 0.1 mg, and the material removal rate (MRR) was calculated using the mass difference and formula (4).

[0061] (4)

[0062] Where: MRR (nm / min) is the material removal rate; (mg) is the mass difference of SiC before and after processing; is the density of single crystal SiC, which is 3.2 g / cm 3 ; S (cm 2 ) is the area of ​​the workpiece to be processed; t (min) is the processing time.

[0063] Example 1

[0064] This embodiment provides a solid phase reaction grinding disc, comprising a base disc, a filler stacked on the base disc, and a plurality of abrasive blocks embedded in the filler and flush with the upper and lower surfaces of the filler; the filler is provided with pores penetrating the filler; and the solid phase reaction grinding disc is prepared by the following process:

[0065] (1) Weigh 20% by mass of diamond abrasive with a particle size of W5 (average particle size of 5 μm, the same below), 30% by mass of ferrosoferric oxide with a particle size of W3 (average particle size of 3 μm, the same below), and 50% by mass of phenolic resin;

[0066] (2) Mix diamond abrasive and ferroferric oxide in a drum for 30 min, then grind the mixture in a ball mill for 2-4 h, and then sieve through a 3000 mesh sieve to ensure the powder particle size; mix the sieved mixture with phenolic resin and add it to mold 4 (such as Figure 2 ), hot-pressed at 270°C and 10 MPa for 2 h, solidified and molded, and demolded to obtain an abrasive block;

[0067] 3) Weigh 50% by mass of ferroferric oxide with a particle size of W3, 5% by mass of graphite powder with a particle size of W3, and 45% by mass of epoxy resin liquid. First, mix the ferroferric oxide and graphite powder for 30 minutes, then mix the mixture with the epoxy resin liquid and stir it ultrasonically for 30 minutes to obtain the filler;

[0068] 4) The abrasive block obtained in step 2) is bonded to the base plate in a circular arrangement, leaving a circular air hole at the center of the base plate, and then fillers are added to the remaining gaps. After consolidation, the corresponding solid phase reaction grinding disc is obtained by leveling. Figure 1 .

[0069] The solid phase reaction grinding disc of this embodiment is used to grind single crystal SiC:

[0070] The grinding experiment was carried out using the grinding disc on a KD15BX single-sided grinding machine. The workpiece was a 2-inch 4H-SiC (0001) cutting disc produced by Beijing Tianke Heda Blue Light Semiconductor Co., Ltd. The original surface roughness Ra was 130nm and the thickness was (400±25)μm.

[0071] During grinding, the grinding disc rotates around the main shaft at a constant speed driven by the active motor. The SiC workpiece is evenly attached to the workpiece disc through paraffin and covered with a dressing ring. The pressure is adjusted by the counterweight block, and the center of the retaining pulley is on the concentric circle with the dressing ring. During the grinding process, the dressing ring and the workpiece disc rotate automatically under the friction of the retaining frame and the grinding disc, and the SiC workpiece is processed through relative motion.

[0072] The grinding liquid used was 5 wt.% hydrogen peroxide, the grinding liquid flow rate was 20 mL / min, the grinding pressure was 10 kPa, the rotation speed was 60 r / min, and after processing for 60 min, the Ra of the SiC wafer was 10 nm and the material removal rate was 1.6 μm / min.

[0073] The surface morphology and surface roughness of the polished wafer were tested using white light interferometer. Figure 3 .

[0074] Example 2

[0075] This embodiment provides a solid phase reaction grinding disc, comprising a base disc, a filler stacked on the base disc, and a plurality of abrasive blocks embedded in the filler and flush with the upper and lower surfaces of the filler; the filler is provided with pores penetrating the filler; and the solid phase reaction grinding disc is prepared by the following process:

[0076] (1) Weigh 15% by mass of diamond abrasive with a particle size of W3, 35% by mass of carbonyl iron powder with a particle size of W1, and 50% by mass of phenolic resin;

[0077] (2) Mix and stir the diamond abrasive and carbonyl iron powder in a drum for 30 min, then grind the mixture in a ball mill for 2-4 h, and then sieve through a 5000 mesh sieve to ensure the powder particle size; mix the sieved mixture with phenolic resin and add it into mold 4, hot press it at 270°C and 10 MPa for 2 h, solidify it into a mold, and demold it to obtain an abrasive block;

[0078] 3) Weigh 55% by mass of carbonyl iron powder with a particle size of W1 (average particle size of 1 μm, the same below), 5% by mass of graphite powder with a particle size of W1, and 40% by mass of epoxy resin liquid. First, mix the carbonyl iron powder and graphite powder for 30 minutes, then mix the mixture with the epoxy resin liquid and ultrasonically stir for 30 minutes to obtain the filler;

[0079] 4) The abrasive block obtained in step 2) is bonded to the base plate in a sunflower seed arrangement, leaving a circular air hole at the center of the base plate, and then fillers are added to the remaining gaps. After consolidation, the solid phase reaction grinding disc is obtained by leveling.

[0080] The single crystal SiC is ground using the solid phase reaction grinding disc with oriented abrasive grains of this embodiment:

[0081] The grinding experiment was carried out using the grinding disc on a KD15BX single-sided grinding machine. The workpiece was a 2-inch 6H-SiC (0001) cutting disc produced by Beijing Tianke Heda Blue Light Semiconductor Co., Ltd. The original surface roughness Ra was 130nm and the thickness was (400±25)μm.

[0082] During grinding, the grinding disc rotates around the main shaft at a constant speed driven by the active motor. The SiC workpiece is evenly attached to the workpiece disc through paraffin and covered with a dressing ring. The pressure is adjusted by the counterweight block, and the center of the retaining pulley is on the concentric circle with the dressing ring. During the grinding process, the dressing ring and the workpiece disc rotate automatically under the friction of the retaining frame and the grinding disc, and the SiC workpiece is processed through relative motion.

[0083] The grinding liquid was 10wt.% hydrogen peroxide, the grinding liquid flow rate was 30 mL / min, the grinding pressure was 10 kPa, the rotation speed was 40 r / min, and after 60 min of processing, the Ra of the SiC wafer was 5 nm. The material removal rate was 1.1 μm / min.

[0084] The surface morphology and surface roughness of the polished wafer were tested using a white light interferometer. Figure 4 .

[0085] Example 3

[0086] This embodiment provides a solid phase reaction grinding disc, comprising a base disc, a filler stacked on the base disc, and a plurality of abrasive blocks embedded in the filler and flush with the upper and lower surfaces of the filler; the filler is provided with pores penetrating the filler; and the solid phase reaction grinding disc is prepared by the following process:

[0087] (1) Weigh 20% by mass of W1-sized silicon oxide abrasive, 30% by mass of W1-sized ferrosoferric oxide, and 50% by mass of phenolic resin;

[0088] (2) Mix diamond abrasive and ferroferric oxide in a drum for 30 min, then grind the mixture in a ball mill for 2-4 h, and then sieve through an 8000 mesh sieve to ensure the powder particle size; mix the sieved mixture with phenolic resin and add it into mold 4, hot press at 270°C and 10 MPa for 2 h, solidify and mold, and demold to obtain an abrasive block;

[0089] 3) Weigh 60% by mass of ferroferric oxide with a particle size of W1, 5% by mass of graphite powder with a particle size of W1, and 35% by mass of epoxy resin liquid, first mix the ferroferric oxide and graphite powder and stir for 30 min, then mix the mixture with the epoxy resin liquid and stir ultrasonically for 30 min to obtain the filler;

[0090] 4) The abrasive block obtained in step 2) is bonded to the base plate in an Archimedean spiral arrangement, leaving a circular air hole at the center of the base plate, and then fillers are added to the remaining gaps. After consolidation, the solid phase reaction grinding disc is obtained by leveling.

[0091] The single crystal SiC is ground using the solid phase reaction grinding disc with oriented abrasive grains of this embodiment:

[0092] The grinding experiment was carried out using the grinding disc on a KD15BX single-sided grinding machine. The workpiece was a 2-inch 6H-SiC (0001) cutting disc produced by Beijing Tianke Heda Blue Light Semiconductor Co., Ltd. The original surface roughness Ra was 130nm and the thickness was (400±25)μm.

[0093] During grinding, the grinding disc rotates around the main shaft at a constant speed driven by the active motor. The SiC workpiece is evenly attached to the workpiece disc through paraffin and covered with a dressing ring. The pressure is adjusted by the counterweight block, and the center of the retaining pulley is on the concentric circle with the dressing ring. During the grinding process, the dressing ring and the workpiece disc rotate automatically under the friction of the retaining frame and the grinding disc, and the SiC workpiece is processed through relative motion.

[0094] The grinding liquid used was 20wt.% hydrogen peroxide, the grinding liquid flow rate was 25mL / min, the grinding pressure was 10 kPa, the rotation speed was 60r / min, and after 60 minutes of processing, the Ra of the SiC wafer was 2 nm. The material removal rate was 0.05 μm / min.

[0095] The surface morphology and surface roughness of the polished wafer were tested using a white light interferometer. Figure 5 .

[0096] Comparative Example 1

[0097] This comparative example provides a conventional diamond grinding disc, which is commercially available.

[0098] The grinding was carried out using the same grinding equipment and conditions as in Example 1. The Ra of the SiC wafer was 98 nm and the material removal rate was 1.5 μm / min. The surface morphology and surface roughness of the wafer after grinding were detected by white light interferometry. Figure 6 .

[0099] Comparative Example 2

[0100] This comparative example provides a grinding disc. In the preparation method thereof, the grinding liquid is deionized water, and the rest is consistent with Example 1.

[0101] The grinding was carried out using the same grinding equipment and conditions as in Example 1. The Ra of the SiC wafer was 50 nm and the material removal rate was 1.3 μm / min. The surface morphology and surface roughness of the wafer after grinding were detected by white light interferometry. Figure 7 .

[0102] Those skilled in the art will appreciate that the embodiments herein are intended to help readers understand the principles of the present invention, and should be understood that the protection scope of the present invention is not limited to such specific statements and embodiments. Those skilled in the art can make various other specific variations and combinations that do not deviate from the essence of the present invention based on the technical revelations disclosed by the present invention, and these variations and combinations are still within the protection scope of the present invention.

Claims

1. A solid phase reaction grinding disc for SiC wafer grinding, characterized in that: It comprises a base plate, a filler stacked on the base plate, and a plurality of abrasive blocks embedded in the filler and flush with the surface of the filler; the filler is provided with an air hole, which is arranged at the center of the filler and penetrates the filler; The filler is composed of a catalyst and a research aid; The abrasive block is composed of a mixture of abrasive, catalyst and adhesive; The catalyst is iron-containing particles; The weight percentage of the catalyst in the filler is 40-60%, the weight percentage of the abrasive in the abrasive block is 10-30%, and the weight percentage of the catalyst is 20-40%.

2. The solid phase reaction grinding disc according to claim 1, characterized in that: The abrasive blocks are evenly dispersed and arranged; the abrasive blocks are in the shape of cylinders and / or polygonal prisms.

3. The solid phase reaction grinding disc according to claim 2, characterized in that: The abrasive blocks are arranged in a shape of one or more of a spiral, a ring, a honeycomb or a sunflower seed.

4. The solid phase reaction grinding disc according to claim 1, characterized in that: The catalyst is one or more of ferroferric oxide, carbonyl iron powder or reduced iron powder; the grinding aid is one or more of graphite powder, iron oxide powder, iron powder or stearic acid.

5. The solid phase reaction grinding disc according to claim 1, characterized in that: The abrasive is one or more of diamond, silicon carbide, cerium oxide or silicon oxide.

6. The solid phase reaction grinding disc according to claim 1, characterized in that: The adhesive is one or more of a resin binder, a ceramic binder or a metal binder.

7. The method for preparing a solid phase reaction grinding disc according to any one of claims 1 to 6, characterized in that: The steps include: S1: mixing abrasive, catalyst and adhesive, hot pressing and curing, and demolding to obtain an abrasive block; S2: bonding the abrasive block to the base plate; S3: Add fillers into the gaps of the base disc and level it to obtain the solid phase reaction grinding disc.

8. The method for preparing a solid phase reaction grinding disc according to claim 7, characterized in that: S1 also includes the steps of mixing, grinding and sieving the abrasive and the catalyst before mixing.

9. Use of the solid phase reaction grinding disc according to any one of claims 1 to 6 in grinding SiC wafers.