Inductive structural element and method for producing an inductive structural element

By combining the wrapping material of high-aluminum cement and other materials in the transformer with the copper wire winding, the magnetic permeability and thermal conductivity are improved, the problems of power density and material cost of traditional transformers are solved, and efficient and low-cost induction structural components are realized.

CN113614862BActive Publication Date: 2024-11-08ROBERT BOSCH GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080027147.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-08
Filing Date
2020-03-11
Publication Date
2024-11-08
Estimated Expiration
2040-03-11

AI Technical Summary

Technical Problem

The power density of traditional transformers is affected by the loss power discharge caused by the wrapping material, resulting in reduced magnetic permeability and efficiency, and high material cost.

Method used

Using a wrapping material of matrix and soft magnetic powder including high-aluminum cement, phosphate cement, SiO2 and reactive alumina, combined with copper wire winding, improve magnetic permeability and thermal conductivity and reduce dielectric by adjusting the proportion and structural design of the filling material. Constant, achieving high power density and mechanical stability.

Benefits of technology

High power density and thermal conductivity are achieved, structural space requirements are reduced, material costs are saved, and leakage inductance and resonant inductance are improved without affecting efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113614862B_ABST
    Figure CN113614862B_ABST
Patent Text Reader

Abstract

The invention relates to an inductive structural element (1, 10), comprising a copper wire winding (3) and a wrapping material (8) surrounding the copper wire winding (3), wherein the wrapping material (8) comprises a matrix (5) and at least one first filling material (6), wherein the matrix (5) comprises at least one selected from high-alumina cement, phosphate cement, SiO 2 , MgO and reactive alumina, and wherein the first filler material (6) comprises at least one soft magnetic powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an inductive component having a high power density and a method for producing an inductive component having good inductivity with good thermal conductivity. Background Art

[0002] When manufacturing conventional transformers, a magnetic core is surrounded in a known manner by two electrical conductors with unequal numbers of windings, such as copper wire windings. Subsequently, the electrical conductors are surrounded by a sheathing material, which establishes a connection between the magnetic core surrounded by the windings and the housing. During operation of the transformer, the power losses generated in the magnetic core or in the windings are dissipated to the housing via the sheathing material. The power density of conventional transformers is thereby reduced. Summary of the invention

[0003] The invention is improved by an inductive structural element, which comprises a copper wire winding and a sheathing material surrounding the copper wire winding, wherein the sheathing material comprises a matrix and at least one first filling material, wherein the matrix comprises at least one material selected from high-alumina cement, phosphate cement, SiO2, MgO and reactive alumina, and wherein the first filling material comprises at least one soft-magnetic powder, and further comprises at least one second filling material, wherein the total mass of the first filling material is 1 to 50 mass percent relative to the total mass of the first and second filling materials, wherein the total mass of the second filling material is 50 to 99 mass percent relative to the total mass of the first and second filling materials. The inductive structural element according to the invention is distinguished by a high power density. This is achieved in that a high magnetic permeability (μ) can be achieved due to the structural design of the inductive structural element. R =2 to 4 or 10 to 500) and thereby also the leakage inductance can be increased, thereby also enabling the integration of a resonant inductance, without significantly affecting the efficiency of the inductive component and thereby the power density. In addition, the installation space of the inductive component can be reduced with high thermal conductivity and good power density.

[0004] As described above, according to the invention, the inductive component comprises a copper wire winding and a sheathing material surrounding the copper wire winding. According to the invention, two or more copper wire windings or only one copper wire winding and at least one further winding of an electrically conductive material can also be used. The number of windings depends on the use of the inductive component. The copper wire winding can be present, for example, as a free-form copper wire winding and is essentially unlimited in shape and form. A particularly suitable form is a winding in the form of a ring.

[0005] The encapsulating material comprises a matrix and at least one first filling material. This means that not only the first filling material can be present alone or a mixture of the first filling material and one or more other filling materials can be present. The first filling material and, if necessary, other filling materials are distributed in the matrix, wherein a certain mechanical stability is obtained by the composite material produced and the matrix provides a connection between the copper wire winding and, for example, surrounding components. The matrix comprises at least one material selected from high-aluminum cement, phosphate cement, SiO2, MgO and reactive alumina. This involves a chemical compound or a mixture of these compounds solidified with water and does not involve a sintered ceramic material. It is assumed here that the increase in the dielectric constant can be prevented by a high magnetic permeability. The inductance can be provided by the first filling material contained in the matrix, the first filling material comprising at least one soft magnetic powder. The first filling material can comprise a soft magnetic powder alone or a mixture consisting of two or more soft magnetic powders.

[0006] In addition to good magnetic properties, the inductive component also has high thermal conductivity and a low loss factor for the magnetic permeability. For example, the thermal conductivity of the encapsulation material used according to the invention is 5 to 8 W / m·K, which is due in particular to the use of high-alumina cement, phosphate cement, SiO2, MgO or reactive alumina. In addition, the inductive component can be formed without a conventional magnetic core, which saves material costs and costs for manufacturing the component.

[0007] The dependent claims describe preferred embodiments of the invention.

[0008] Due to the very good inductive properties, the soft magnetic powder is advantageously selected from carbonyl iron and ferrite powders. This means that carbonyl iron and ferrite powders can be used individually or in the form of a mixture.

[0009] According to another advantageous refinement, the encapsulation material comprises at least one polymer. By using one or more polymers, for example, the thermal properties of the encapsulation material, such as shrinkage or thermal conductivity, etc., can be advantageously influenced. The use of polymers can also improve the adhesion of the encapsulation material to surrounding components, such as, for example, a housing. Particularly suitable polymers are thermoplastic polymers. Preferred polymers are copolymers of acrylates, ethylene and vinyl esters, copolymers of acrylates, methacrylates and styrene, copolymers of ethylene and vinyl esters and polymethyl silicone resins.

[0010] In order to improve the properties of the encapsulation material, the encapsulation material advantageously comprises at least one second filling material. This second filling material can add further functions to the encapsulation material. In this case, only a second filling material can be used or two or more second filling materials can be used. Due to the very good thermal conductivity, the second filling material preferably contains Al2O3.

[0011] In order to provide good mechanical stability with simultaneously high thermal conductivity and good magnetic permeability, the total mass of the matrix is ​​5 to 25 mass percent relative to the total mass of the encapsulating material. In this case, high-alumina cement, phosphate cement, SiO2, MgO or reactive alumina forms a very fine microstructure with a particle size of up to 200 μm, which contributes to the high stability of the matrix and the very good thermal conductivity.

[0012] In order to optimize the function of the encapsulation material and in particular to improve the inductive and thermal conductivity, the total mass of the first and second filling materials is in particular 75 to 95 percent by mass relative to the total mass of the encapsulation material.

[0013] In particular, when using a free-form copper wire winding without a magnetic core surrounded by the copper wire winding, the total mass of the first filling material relative to the total mass of the first and second filling materials is advantageously 75 to 95 mass percent in order to maximize the inductive properties of the inductive component. This means that, in addition to the first filling material, only a small proportion of the second filling material is contained in the matrix and thus also in the encapsulating material. The proportion of soft magnetic powder is thus very high. This results in very good magnetic permeability.

[0014] According to another advantageous development, the inductive component comprises a magnetic core. The copper wire winding thus surrounds the magnetic core at least partially or at least in sections. The magnetic core can be, for example, a ferrite core or a magnetic powder core with a polymer matrix or also a sintered magnetic powder core and is in particular designed as a ferrite core.

[0015] In the aforementioned embodiment with a magnetic core, it is preferred that the total mass of the soft magnetic powder is 1 to 50 mass percentage points relative to the total mass of the first and second filling materials. As a result, a high magnetic permeability can nevertheless be provided in the inductive structural element while reducing the total mass of the soft magnetic powder. The leakage inductance can be increased and a resonant inductor can be integrated while maintaining the same low dielectric constant.

[0016] Furthermore, in embodiments with a magnetic core, with regard to the thermal conductivity of the encapsulating material and thus also the inductive component, it is advantageous if the total mass of the second filler material and in particular Al2O3 is 50 to 99 mass percent relative to the total mass of the first and second filler materials.

[0017] The inductive structural element and in particular the encapsulation material advantageously do not contain Portland cement. This means that no Portland cement is added or used when producing the inductive structural element. The total mass of the Portland cement is therefore essentially 0 mass percent relative to the total mass of the encapsulation material and therefore also relative to the total mass of the inductive structural element. Portland cement has the disadvantage relative to the matrix according to the invention that it contains many impurities, which, although tolerable for load-bearing components, bring about significant performance impairments for electronic applications and in particular for inductive components. In addition, Portland cement has a significantly lower thermal conductivity than high-alumina cement, phosphate cement, SiO2, MgO or reactive alumina, which can probably be attributed to the chemical structure of the individual matrix phases.

[0018] It is also advantageous if the first filler material and the second filler material are not sintered, which brings advantages not only in terms of energy-saving production but also from the perspective of high magnetic permeability and high thermal conductivity.

[0019] The inductive component can be designed, for example, as a coil and for this purpose can include in particular a copper wire winding. Due to the very good inductive and thermally conductive properties, the inductive component according to the invention is designed in particular as a transformer and for this purpose can include a copper wire winding and at least one further electrically conductive winding, which can also be designed as a copper wire winding.

[0020] According to the invention, a method for producing an inductive component is also described. The method comprises the step of mixing a matrix material with at least one first filler material, water and optionally at least one solvent when producing slip. "Slip" is understood here to be an uncured and unsolidified, more or less flowable or at least formable material.

[0021] Solvents within the meaning of the present invention may be, for example, modified polycarboxylic acid ethers and may be used, for example, in an amount of 0.1 to 2 percent by mass, relative to the total mass of the slip.

[0022] The matrix material contains at least one material selected from unsolidified high-alumina cement, unsolidified phosphate cement, unsolidified SiO2, unsolidified MgO and unsolidified reactive alumina. In addition, the first filling material includes at least one soft magnetic powder. The mixing can be accomplished, for example, by stirring with a suitable stirrer. The resulting slip is then arranged around the copper wire winding so that the slip surrounds the copper wire winding as completely as possible but at least on the outer circumference of the copper wire winding. Subsequently, the slip is solidified by at least partially solidifying the matrix material with water at a temperature in the range of 50 to 150° C. This solidification step can be carried out, for example, in a furnace. Sintering is not carried out at a temperature greater than 200° C. By this solidification, the solvent previously used is largely removed and can basically no longer be confirmed thereafter.

[0023] As described above according to the invention, a coating material in the sense of the invention is produced. The degree of solidification of the matrix material can be adjusted by the amount of water added. The appropriate amount of water can be determined by simple experiments.

[0024] The method according to the invention can be easily and cost-effectively implemented and can produce dielectric materials with a high magnetic permeability (μ) with little or no increase in the dielectric constant. R =2 to 4 or 10 to 500), high leakage inductance and integrated resonant inductance. In addition, the components produced according to the invention are also distinguished by high thermal conductivity, making the inductive components highly efficient and having an outstanding power density.

[0025] The advantages, advantageous effects and developments described for the inductive component according to the invention also apply to the method according to the invention for producing an inductive component.

[0026] In order to improve the mechanical properties, the method can furthermore include a step of annealing immediately after solidification of the matrix material. The annealing is preferably carried out at a temperature in the range of 100 to 150° C.

[0027] It is also advantageous that the method can also provide a step of surrounding a magnetic core, in particular in the form of a ferrite core, with a copper wire winding. In this embodiment, the copper wire winding is therefore not present as a free-form copper wire winding, but surrounds the magnetic core. Thus, the encapsulation material is arranged around the copper wire winding surrounding the magnetic core and in particular is not arranged inside the copper wire winding. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0029] Figure 1shows a cross-sectional view of an inductive structural element according to a first embodiment; and

[0030] Figure 2 A sectional view of an inductive component according to a second specific embodiment is shown.

[0031] Only the main features of the present invention are shown in the accompanying drawings. All other features are omitted for the sake of simplicity. In addition, the same reference numerals represent the same components. DETAILED DESCRIPTION

[0032] Figure 1 An inductive component 1 according to a first embodiment is shown in section. The inductive component 1 comprises a housing 2 in which a magnetic core 4 is arranged which is surrounded on all sides by a copper wire winding 3. The copper wire winding 3 is wound directly around the magnetic core 4 in this case.

[0033] The magnetic core 4 is configured, for example, as a ferrite core or as a magnetic powder core with a polymer matrix or as a sintered magnetic powder core, wherein the configuration as a ferrite core is preferred. The magnetic core 4 and the copper wire winding 3 surrounding the magnetic core 4 are arranged in a housing 2. A wrapping material 8 is arranged between the housing 2 and the copper wire winding 3, which provides a connection between the copper wire winding 3 and the housing 2.

[0034] The encapsulating material 8 comprises a matrix 5 and a first filler material 6 and a second filler material 7, wherein the first filler material 6 is a soft magnetic powder, such as carbonyl iron or ferrite powder, and wherein the second filler material 7 is Al2O3. The first filler material 6 and the second filler material 7 are distributed in the matrix 5 and exist in a non-sintered form.

[0035] The matrix 5 comprises at least one material selected from high-alumina cement, phosphate cement, SiO2, MgO and reactive alumina. These compounds or mixtures of these compounds are present in a form at least partially solidified with water at 50 to 150° C. and are not sintered. The matrix 5 thus forms a microcrystalline network structure of particles with a particle size of up to 200 μm, in which the filler materials 6, 7 are uniformly distributed. The encapsulating material 8 and thus the inductive structural element 1 also do not contain Portland cement.

[0036] The total mass of the base body 5 is 5 to 25 mass percent relative to the total mass of the wrapping material 8 .

[0037] The total mass of the first and second filling materials 6, 7 is 75 to 95 mass percent relative to the total mass of the encapsulating material 8, wherein the proportion of the first filling material 6, i.e. the soft magnetic powder, is advantageously 1 to 50 mass percent relative to the total mass of the first filling material 6 and the second filling material 7. As a result, a particularly high thermal conductivity is achieved with good magnetic properties due to the high proportion of the second filling material 7.

[0038] The inductive structural element 1 is distinguished by a high power density and a high efficiency due to the use of the encapsulating material 8. This means that the inductive structural element 1 has a high magnetic permeability (μ R =2 to 4 or 10 to 500) and have high leakage inductance and resonance inductance, while the dielectric constant is not significantly increased. In addition, the encapsulating material 8 has a high thermal conductivity, which further increases the power density of the inductive component 1.

[0039] Figure 2 An inductive structural element 10 according to a second embodiment is shown in section. Figure 1 The inductive component 1 differs from the inductive component 1 in that it has no magnetic core. The copper wire winding 3 is therefore in the form of a free-form copper wire winding which has been produced beforehand on a substrate, for example.

[0040] Here too, the total mass of the base body 5 is 5 to 25 mass percent relative to the total mass of the encapsulating material 8 .

[0041] The total mass of the first filling material 6 and the second filling material 7 is 75 to 95 mass percent relative to the total mass of the packaging material 8, wherein the proportion of the first filling material 6, that is, the soft magnetic powder, is 75 to 95 mass percent. Figure 1 The content of the second filler material 7, that is, in particular Al2O3, is thus smaller in the matrix of the inductive component 10 and is in particular 75 to 95 percent by mass relative to the total mass of the first filler material 6 and the second filler material 7. The higher content of the soft magnetic powder is advantageous in view of the magnetic properties of the inductive component 10.

[0042] The inductive structural element 10 is also distinguished by a high power density and a high efficiency due to the use of the encapsulation material 8. A high magnetic permeability (μ R =2 to 4 or 10 to 500) and also obtain high leakage inductance and resonance inductance. In addition, the encapsulation material 8 has good thermal conductivity, which further increases the power density of the inductive structural element 10.

Claims

1. An inductive structural element, comprising a copper wire winding (3) and a sheathing material (8) surrounding the copper wire winding (3), wherein the sheathing material (8) comprises a base body (5) and at least one first filling material (6), - wherein the matrix (5) comprises at least one material selected from high-alumina cement, phosphate cement, SiO2, MgO and reactive alumina, and - wherein the first filling material (6) comprises at least one soft magnetic powder, Furthermore, it comprises at least one second filling material (7), The total mass of the first filling material (6) is 1 to 50 mass percent relative to the total mass of the first and second filling materials (6, 7), The total mass of the second filling material (7) is 50 to 99 mass percent relative to the total mass of the first and second filling materials (6, 7).

2. The inductive structural element according to claim 1, wherein the soft magnetic powder is selected from carbonyl iron powder and ferrite powder.

3. The inductive structural element according to claim 1 or 2, wherein the encapsulation material (8) comprises at least one polymer.

4. The inductive structural element according to claim 1 or 2, wherein the total mass of the base body (5) relative to the total mass of the encapsulating material (8) is 5 to 25 mass percentage points.

5. The inductive structural element according to claim 1 or 2, wherein the total mass of the first and second filling materials (6, 7) relative to the total mass of the encapsulating material (8) is 75 to 95 mass percent.

6. The inductive structural element according to claim 1 or 2, further comprising a magnetic core (4), wherein the copper wire winding (3) at least partially surrounds the magnetic core (4).

7. The inductive structural element according to claim 1 or 2, wherein the structural element (1, 10) is free of Portland cement.

8. The inductive structural element according to claim 1 or 2, wherein the first filler material (6) and the second filler material (7) are not sintered.

9. The inductive structural element according to claim 1 or 2, which is designed as a transformer.

10. A method for producing an inductive structural element (1, 10), comprising the following steps: - in the production of slip, a base material is mixed with at least one first filler material (6), water and optionally at least one solvent, wherein the base material comprises at least one material selected from the group consisting of uncured high-alumina cement, uncured phosphate cement, uncured SiO2, uncured MgO and uncured reactive alumina, and the first filler material (6) comprises at least one soft magnetic powder, - using the slip to surround the copper wire winding (3) and The matrix material is at least partially solidified by water at a temperature in the range of 50 to 150°C.

11. The method according to claim 10, further comprising the step of annealing immediately after solidification of the matrix material, wherein the annealing is performed at a temperature in the range of 100 to 150°C.

12. A method according to claim 10 or 11, comprising the step of surrounding the magnetic core (4) with a copper wire winding (3).