Metal foil for printed wiring board, metal foil with carrier, metal-clad laminate, and method for producing printed wiring board using the same
By using a metal foil with a first etching sacrificial layer with an etching rate higher than Cu and a second etching sacrificial layer with an etching rate lower than Cu, combined with a local cell reaction and an anti-diffusion layer, the problem of ultra-thin copper foil microstructure in printed circuit board manufacturing is solved. Defects and circuit breakage issues under etching and high-temperature pressing enable more efficient circuit manufacturing and stability.
Patent Information
- Application Number
- CN202080023976.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-27
- Filing Date
- 2020-03-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-03-09
AI Technical Summary
In the manufacturing process of printed circuit boards, ultra-thin copper foil is prone to defects and circuit dents during the micro-etching process, and the difference in thermal expansion between the copper foil and the insulating resin material after high-temperature pressing causes circuit breakage. The existing etched sacrificial layer cannot be treated with chemical solutions. Not effective at high temperatures.
Using a metal foil with a first etching sacrificial layer and a second etching sacrificial layer that are easier to etch than Cu, the first etching sacrificial layer has a higher etching rate than Cu, and the second etching sacrificial layer has a lower etching rate than Cu, through local cell reactions Inhibits dissolution of the seed layer and prevents metal diffusion at high temperatures.
It effectively suppresses the occurrence of seed layer defects and circuit dents, ensures the miniaturization of printed circuit boards and the stability of circuits, prevents metal from diffusing into the copper layer, and improves productivity and circuit reliability.
Smart Images

Figure CN113646469B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a metal foil for producing a printed wiring board, a metal foil with a carrier, a metal-clad laminate, and a method for producing a printed wiring board using the same. Background Art
[0002] In recent years, the MSAP method (modified semi-additive process) has been widely used as a method for manufacturing printed circuit boards suitable for miniaturization of circuits. The MSAP method is a method suitable for forming extremely fine circuits. In order to fully utilize this feature, it is carried out using copper foil with a carrier. For example, Figure 6 and 7 As shown, using prepreg 112 and primer 113, ultra-thin copper foil 110 is pressed and bonded to insulating resin substrate 111 having lower circuit 111b on base substrate 111a (process (a)); after peeling off the carrier (not shown), via 114 is formed by laser perforation as needed (process (b)). Then, after chemical copper plating 115 (process (c)), exposure and development of dry film 116 are used, masking is performed in a predetermined pattern (process (d)), and electroplating 117 is performed (process (e)). After the dry film 116 is removed and wiring portion 117a is formed (process (f)), unnecessary ultra-thin copper foil between adjacent wiring portions 117a, 117a is removed by etching over their entire thickness (process (g)), thereby obtaining wiring 118 formed with a predetermined pattern.
[0003] Here, after forming the via hole 114 (process (b)) and before forming the chemical copper plating 115 (process (c)), micro-etching (Cu etching) is sometimes performed for the purpose of cleaning the lower layer circuit 111b on the bottom surface of the via hole and removing the spatter attached to the periphery of the via hole. In recent years, from the viewpoint of miniaturizing the circuit, it is ideal to make the thickness of the ultra-thin copper foil 110 thinner than before in advance, so that the seed layer (ultra-thin copper foil 110) at the moment of the aforementioned micro-etching is about 0.3 μm thick. However, if an attempt is made to micro-etch the laminate of the ultra-thin copper foil 110 and the insulating resin substrate 111 thus thinned, as shown in FIG. Figure 8 As schematically shown, during the micro-etching process, defects 110 a may be locally generated in the ultra-thin copper foil 110 (seed layer) due to in-plane deviation of the micro-etching.
[0004] Therefore, a method has been proposed to significantly reduce the in-plane deviation of micro-etching by using an extremely thin copper foil having an etching sacrificial layer that is easier to etch than Cu. For example, Patent Document 1 (International Publication No. 2017 / 141985) discloses a copper foil for printed circuit board manufacturing, which sequentially comprises a first copper layer, an etching sacrificial layer composed of a Cu-Zn alloy, etc., and a second copper layer (seed layer), wherein the ratio r of the etching rate of the etching sacrificial layer to the etching rate of Cu is higher than 1.0. According to the above copper foil, Fig. 9 As schematically shown, since the etching sacrificial layer 212 is sandwiched between the two copper layers 213 and 211, during the micro-etching process of the laminate of the metal foil 210 and the insulating layer 228, even if the etching sacrificial layer 212 is dissolved unevenly and the second copper layer (seed layer) 213 is partially exposed, the etching sacrificial layer 212 is still preferentially dissolved. As a result, it is believed that the thickness of the second copper layer (seed layer) 213 is substantially uniformly maintained and becomes less likely to be damaged.
[0005] On the other hand, Patent Document 1 also discloses that in the manufacture of printed circuit boards based on the coreless build-up method, copper foil having the above-mentioned etched sacrificial layer can be preferably used. The coreless build-up method is a method in which a wiring layer (first wiring layer) is formed on a metal layer on the surface of a support body (core), and then a build-up layer is formed, and then the support body (core) is removed to form a wiring board only from the build-up layer. The printed circuit board manufactured using the above method is a type in which the circuit pattern is buried in the insulating layer, so this method is called ETS (Embedded Trace Substrate). According to Patent Document 1, Fig.10 As schematically shown in (b) and (c), when Cu etching is performed, even if Cu (Cu of the second copper layer 213 or the first wiring layer 226) is partially exposed due to uneven dissolution of the etching sacrificial layer 212 and / or pinholes that may accidentally exist in the etching sacrificial layer 212, the dissolution of the second copper layer 213 or the first wiring layer 226 (copper layer) of the substrate can be suppressed by local battery reaction. As a result, it is believed that the second copper layer 213 can be uniformly etched in the plane and the occurrence of local circuit depressions in the first wiring layer 226 can be suppressed. In addition, according to this method, since the etching sacrificial layer 212 is dissolved and removed along with the Cu etching, an additional process for removing the etching sacrificial layer 212 is no longer required, and productivity is also improved.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2017 / 141985 Summary of the invention
[0009] Thus, in the manufacture of printed circuit boards, copper foil having an etched sacrificial layer is highly useful from the viewpoint of being able to significantly suppress the occurrence of seed layer defects and circuit depressions. Figure 6 and 7 ), since the via hole 114 is formed by laser drilling or the like (step (b)), resin residue (drill smear) may be generated at the bottom of the via hole 114, etc., and a desmear treatment using a chemical solution is performed as a treatment to remove the resin residue. This desmear treatment can also be performed when the build-up layer is formed in the above-mentioned ETS method. On the other hand, when a copper foil having an etching sacrificial layer is used as an ultra-thin copper foil, such as Figure 3 As shown schematically, after drilling, the etching sacrificial layer 212 is exposed from the side of the via hole 214. When desmear treatment is performed in this state, although the etching sacrificial layer 212 is protected by the first copper layer 211 in the portion other than the side of the via hole 214, the chemical solution may start to corrode from the exposed portion of the etching sacrificial layer 212 on the side of the via hole 214. Therefore, there is a concern that the etching sacrificial layer 212 has disappeared at the beginning of micro-etching. As a result, the sacrificial effect of the etching sacrificial layer 212 being dissolved preferentially over the seed layer (second copper layer 213) during micro-etching cannot be fully exerted, and a defect 213a may be generated in the seed layer.
[0010] On the other hand, as the circuits of printed circuit boards have been required to be further miniaturized in recent years, low CTE substrates with low coefficient of thermal expansion (CTE) are widely used as insulating substrates to prevent circuit breakage and other undesirable conditions caused by the difference in thermal expansion between copper wiring and insulating resin materials. However, low CTE substrates generally have high curing temperatures, so the pressing temperature when they are closely attached to copper foil is likely to be high (e.g., above 220°C). In this regard, when high-temperature pressing is performed using copper foil having an etched sacrificial layer of Cu-Zn alloy, etc., Figure 5 As schematically shown, metal (e.g., Zn) and the like diffuse from the etching sacrificial layer 212 to the copper layers 211 and 213, and as a result, these layers as a whole may become an alloy layer 220 having a composition similar to that of the etching sacrificial layer 212. Therefore, when micro-etching is performed, the sacrificial effect of the etching sacrificial layer 212 cannot be fully exerted, and there is a concern that the etching sacrificial layer 212 and the seed layer (second copper layer 213) become one and are removed.
[0011] The inventors of the present invention have obtained the following insight: in the manufacture of printed circuit boards, by using a metal foil having a second etching sacrificial layer with an etching rate higher than Cu and lower than the first etching sacrificial layer sandwiched between the seed layer (copper layer) and the first etching sacrificial layer, the occurrence of seed layer defects can be suppressed even in the case of chemical solution treatment after perforation. In addition, the inventors of the present invention have obtained the following insight: by sandwiching the second etching sacrificial layer between the seed layer (copper layer) and the first etching sacrificial layer, the diffusion of metals etc. from the first etching sacrificial layer to the seed layer can be effectively prevented even in the case of high temperature pressing, and as a result, the sacrificial effect originally possessed by the etching sacrificial layer can be exerted.
[0012] Therefore, the first object of the present invention is to provide a metal foil for manufacturing a printed circuit board, which can suppress the occurrence of seed layer defects even when a chemical solution treatment is performed after perforation. In addition, the second object of the present invention is to provide a metal foil for manufacturing a printed circuit board, which can effectively prevent the diffusion of metals, etc. from the first etching sacrificial layer to the seed layer even when a high-temperature pressing process is performed, and as a result, the sacrificial effect originally possessed by the etching sacrificial layer can be exerted.
[0013] According to one embodiment of the present invention, a metal foil for printed circuit board manufacturing is provided, which comprises a first etching sacrificial layer, a second etching sacrificial layer and a copper layer in sequence, and when the ratio of the etching rate of the first etching sacrificial layer to the etching rate of Cu is set to r1 and the ratio of the etching rate of the second etching sacrificial layer to the etching rate of Cu is set to r2, r1>r2>1.0 is satisfied.
[0014] According to another aspect of the present invention, there is provided a metal foil with a carrier, comprising a carrier, a release layer, and the metal foil in this order.
[0015] According to another aspect of the present invention, there is provided a metal-clad laminate including the metal foil described above.
[0016] According to another aspect of the present invention, there is provided a method for manufacturing a printed wiring board, characterized by using the above-mentioned metal foil or the above-mentioned metal foil with a carrier. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a schematic cross-sectional view showing an example of a metal foil with a carrier including the metal foil of the present invention.
[0018] Figure 2 This is a schematic cross-sectional view for explaining chemical solution corrosion after drilling in a laminated body having two etching sacrificial layers.
[0019] Figure 3This is a schematic cross-sectional view for explaining chemical solution corrosion after drilling in a laminated body having a single etching sacrifice layer.
[0020] Figure 4 This is a schematic cross-sectional view for explaining diffusion during high-temperature pressing in a laminate having two etching sacrificial layers.
[0021] Figure 5 This is a schematic cross-sectional view for explaining diffusion during high-temperature pressing in a laminated body having a single etching sacrifice layer.
[0022] Figure 6 It is a diagram showing the first half of the process in a conventional example of a method for manufacturing a printed wiring board using the MSAP method.
[0023] Figure 7 A conventional example of a method for manufacturing a printed wiring board using the MSAP method is shown. Figure 6 The second half of the process shown.
[0024] Figure 8 This is a schematic cross-sectional view for explaining uneven etching of a seed layer (ultra-thin copper foil) in the MSAP method using a conventional copper foil.
[0025] Fig. 9 This is a schematic cross-sectional view for explaining the function of the etching sacrificial layer in the MSAP method.
[0026] Fig.10 This is a schematic cross-sectional view for explaining the function of the etching sacrifice layer in the coreless build-up method (ETS method).
[0027] Fig.11 This is a diagram showing the first half of the process in an example of a method for producing a printed wiring board by a coreless build-up method (ETS method) using the metal foil of the present invention.
[0028] Fig.12 An example of a method for producing a printed wiring board by a coreless build-up method (ETS method) using the metal foil of the present invention is shown. Fig.11 The second half of the process shown.
[0029] Fig.13 It is a diagram for explaining the etching process when the seed layer is not damaged.
[0030] Fig.14 This is a diagram schematically illustrating an etching process when a seed layer is damaged due to a residue of an additional copper layer. DETAILED DESCRIPTION
[0031] Metal foil for printed circuit board manufacturing
[0032] The metal foil according to the present invention is a metal foil used in the manufacture of printed circuit boards. Figure 1 FIG. 2 is a schematic cross-sectional view of the metal foil of the present invention. Figure 1 As shown, the metal foil 10 includes a first etching sacrificial layer 11, a second etching sacrificial layer 12, and a copper layer (seed layer) 13 in this order. The metal foil 10 may further include an additional copper layer 14 on the surface of the first etching sacrificial layer 11 on the opposite side to the second etching sacrificial layer 12 as needed. In addition, the metal foil 10 may further include a diffusion prevention layer 15 between the additional copper layer 14 and the first etching sacrificial layer 11. Usually, when the metal foil 10 and the insulating resin are laminated, the copper layer that is not in close contact with the insulating resin is the "additional copper layer 14", and the copper layer that is in close contact with the insulating resin is the "copper layer 13". It should be noted that when the metal foil 10 of the present invention is applied to the ETS method, the copper layer on the side where the circuit pattern is not formed is the "additional copper layer 14", and the copper layer on the side where the circuit pattern is to be formed is the "copper layer 13". In this specification, the "copper layer 13" is a layer specifically used to form a circuit pattern, and focusing on this function, the "copper layer 13" is sometimes referred to as the "seed layer 13".
[0033] Even though the first etching sacrificial layer 11 and the second etching sacrificial layer 12 may be copper alloy layers, since they are not metal copper layers, the metal foil 10 includes a metal or alloy other than copper as its inner layer / outer layer. Therefore, in the present invention, although the metal foil 10 is referred to as "metal foil for printed circuit board manufacturing", the metal foil 10 can be used for the same purpose as copper foil generally regarded as copper foil for printed circuit board manufacturing. In addition, regarding the counting order included in the names of "first etching sacrificial layer" and "second etching sacrificial layer", when there is a carrier, it is based on the order of counting from the carrier side. For example, as in Figure 1 When the metal foil 10 is provided in the form of the metal foil 16 with a carrier shown, it is composed in the order of a carrier 17, a peeling layer 18, an additional copper layer 14 (if present), an anti-diffusion layer 15 (if present), a first etching sacrificial layer 11, a second etching sacrificial layer 12, and a copper layer 13 (seed layer).
[0034] In addition, the first etching sacrificial layer 11 and the second etching sacrificial layer 12 are characterized in that when the ratio of the etching rate of the first etching sacrificial layer 11 to the etching rate of Cu is set to r1 and the ratio of the etching rate of the second etching sacrificial layer 12 to the etching rate of Cu is set to r2, r1>r2>1.0 is satisfied. In this way, in the manufacture of printed circuit boards, by using a metal foil in which the second etching sacrificial layer 12 having a lower etching rate ratio than the first etching sacrificial layer 11 is sandwiched between the copper layer 13 and the first etching sacrificial layer 11, it is possible to suppress the occurrence of seed layer defects, etc. even when a chemical solution treatment is performed after perforation.
[0035] As mentioned above, Figure 3 As shown schematically, in a conventional laminate of a metal foil 210 and an insulating layer 228 in which a layer of an etching sacrificial layer 212 is sandwiched between copper layers 211 and 213, after perforation, the etching sacrificial layer 212 will be exposed from the side of the via hole 214. When desmear treatment is performed in this state, although the etching sacrificial layer 212 is protected by the first copper layer 211 in the portion other than the side of the via hole 214, the chemical solution may start to corrode from the exposed portion of the etching sacrificial layer 212 on the side of the via hole 214. In particular, since the etching sacrificial layer 212 is a layer that is more easily etched than the copper layers 211 and 213, it can be said that chemical solution corrosion is prone to occur. Therefore, there is a concern that the etching sacrificial layer 212 has disappeared at the moment when micro-etching starts. As a result, the sacrificial effect that the etching sacrificial layer 212 is preferentially dissolved over the seed layer (second copper layer 213) during micro-etching cannot be fully exerted, and the seed layer may have a defect 213a.
[0036] In contrast, the above technical problems can be easily solved by using the metal foil 10 of the present invention. Figure 2 As shown schematically, in the laminate of the metal foil 10 (having the additional copper layer 14, the first etching sacrificial layer 11, the second etching sacrificial layer 12, and the copper layer 13) and the insulating layer 28, even when the desmear treatment is performed after the via hole 54 is formed by perforation, the second etching sacrificial layer 12 remains on the seed layer (copper layer 13). In other words, since the etching rate ratio r2 of the second etching sacrificial layer 12 is lower than the etching rate ratio r1 of the first etching sacrificial layer 11, when the chemical solution treatment such as desmear treatment is performed, the first etching sacrificial layer 11 is preferentially dissolved than the second etching sacrificial layer 12 by the local battery reaction. In this way, the chemical solution erosion of the second etching sacrificial layer 12 can be suppressed, and at the time of starting micro-etching, not only the seed layer 13 but also at least the second etching sacrificial layer 12 remain on the laminate. Thus, even if Cu is partially exposed during micro-etching, the second etching sacrificial layer 12 can be preferentially dissolved by local battery reaction, and as a result, the dissolution of the underlying seed layer 13 can be suppressed, making it difficult for defects to occur.
[0037] In addition, by interposing the second etching sacrificial layer 12 between the copper layer 13 and the first etching sacrificial layer 11, even when a high-temperature pressing process is performed at, for example, 220°C or higher, it is possible to effectively prevent the diffusion of metals or the like from the first etching sacrificial layer 11 to the seed layer (copper layer 13). As described above, when a copper foil having an etching sacrificial layer made of a Cu-Zn alloy or the like is subjected to high-temperature pressing, Figure 5As shown schematically, metal (e.g., Zn) and the like diffuse from the etching sacrificial layer 212 to the copper layers 211 and 213, and as a result, these layers as a whole may become an alloy layer 220 having a composition similar to that of the etching sacrificial layer 212. Therefore, during micro-etching, the sacrificial effect of the etching sacrificial layer 212 cannot be fully exerted, and there is a concern that the etching sacrificial layer 212 and the seed layer (second copper layer 213) may be integrated and removed. In contrast, in the metal foil 10 of the present invention, as shown in FIG. Figure 4 As shown schematically, the second etching sacrificial layer 12 is sandwiched between the first etching sacrificial layer 11 and the copper layer 13. In addition, the diffusion prevention layer 15 can be sandwiched between the first etching sacrificial layer 11 and the additional copper layer 14 as needed. Therefore, the diffusion of metal from the first etching sacrificial layer 11 can be prevented by the second etching sacrificial layer 12 and / or the diffusion prevention layer 15 (if present). As a result, the alloying of the seed layer 13 and the additional copper layer 14 (if present) can be suppressed, and the above-mentioned technical problems can be eliminated. As a result, a low CTE substrate having a low coefficient of thermal expansion (CTE) but a high curing temperature can be used as an insulating substrate, and as a result, further miniaturization of the circuit in the manufacture of the printed circuit board can be achieved.
[0038] Since the metal foil 10 is subjected to processes such as high-temperature pressing, it is preferred that diffusion from the first etching sacrificial layer 11 to the seed layer 13 does not occur even after heating at 220° C. for 2 hours in a vacuum. In this specification, “no diffusion occurs” means that (i) the copper layer 13 before the metal foil 10 is heated contains only 1 wt% or less (including 0 wt%), and (ii) an element (hereinafter referred to as “diffusion confirmation element”) contained in at least one of the first etching sacrificial layer 11 and the second etching sacrificial layer 12 before the metal foil 10 is heated has a content of 1 wt% or less at a predetermined measurement point of the copper layer 13 after the metal foil 10 is heated. Therefore, for example, even if the carbon content before and after heating in the copper layer 13 is 0.5 wt% and 2 wt%, respectively, if the carbon content before heating in any of the first etching sacrificial layer 11 and the second etching sacrificial layer 12 is less than 1 wt%, since carbon is not a diffusion confirmation element (does not satisfy the above (ii)), it is considered that no diffusion occurs. Here, "the measurement site of the copper layer 13 after the metal foil 10 is heated" refers to: among the sites (a) on the surface of the copper layer 13 on the side opposite to the second etching sacrificial layer 12, or (b) in the depth direction of the copper layer 13, the sites close to the second etching sacrificial layer 12 are 0.3 μm away from the boundary surface between the copper layer 13 and the second etching sacrificial layer 12. That is, when the thickness of the copper layer 13 is less than 0.3 μm, the above (a) becomes the measurement site; when the thickness of the copper layer 13 exceeds 0.3 μm, the above (b) becomes the measurement site. In the case where the boundary between the copper layer 13 and the second etching sacrificial layer 12 cannot be distinguished in the heated metal foil 10, it is considered that diffusion has occurred. It should be noted that when the metal foil 10 is heated, other components (such as a support body, etc.) that do not substantially contain a diffusion confirmation element can be bonded to the surface of the copper layer 13 on the side opposite to the second etching sacrificial layer 12. As described in Examples below, the element content of each layer adopts a value determined by performing element analysis in the depth direction of the metal foil 10 using a glow discharge optical emission spectrometer (GD-OES).
[0039] As long as the etching rate of the first etching sacrificial layer 11 is higher than that of Cu and the second etching sacrificial layer 12, there is no particular limitation. In other words, the ratio r1 of the etching rate of the first etching sacrificial layer 11 to the etching rate of Cu (hereinafter referred to as the etching rate ratio r1), and the ratio r2 of the etching rate of the second etching sacrificial layer 12 to the etching rate of Cu (hereinafter referred to as the etching rate ratio r2) satisfy r1>r2>1.0. By satisfying this relationship, the first etching sacrificial layer 11 and the seed layer 13 can be dissolved and removed simultaneously by Cu etching, and even if the first etching sacrificial layer 11 and the second etching sacrificial layer 12 are unevenly dissolved and Cu is partially exposed, the dissolution of the copper layer (seed layer) of the base is suppressed by the local battery reaction. As a result, the etching of the seed layer can be carried out uniformly within the surface, and the defects of the seed layer, local circuit depressions, and defects can be suppressed. Furthermore, by satisfying the above relationship, when chemical solution treatment is performed in a state where both the first etching sacrificial layer 11 and the second etching sacrificial layer 12 are partially exposed, such as in desmear treatment after drilling, the first etching sacrificial layer 11 is dissolved preferentially over the second etching sacrificial layer 12 by local battery reaction. As a result, at the time of starting micro-etching, the second etching sacrificial layer 12 can be left in a state where dissolution is suppressed, and as a result, even when chemical solution treatment is performed after drilling, the occurrence of seed layer defects can be suppressed.
[0040] The etching rate of the first etching sacrificial layer 11 is calculated as follows: a foil sample made of the same material as the first etching sacrificial layer 11 and a copper foil sample as a reference sample are treated for the same time in the etching process, and the thickness change of each sample caused by etching is divided by the dissolution time to calculate. It should be noted that the thickness change can be determined by measuring the weight loss of the two samples and converting the density of each metal into thickness. From the perspective of obtaining a high sacrificial effect, the preferred etching rate ratio r1 is 1.2 or more, more preferably 1.25 or more, and further preferably 1.3 or more. The upper limit of the etching rate ratio r1 is not particularly limited, but in order to uniformly maintain the dissolution rate of the first etching sacrificial layer 11 in the plane and make the local battery reaction with the second etching sacrificial layer 12 and / or the copper layer 13 uniformly act in the plane, the etching rate ratio r1 is preferably 5.0 or less, more preferably 4.5 or less, more preferably 4.0 or less, particularly preferably 3.5 or less, and most preferably 3.0 or less. Here, as an etching solution, a known liquid that can dissolve copper by a redox reaction can be used. As examples of etching solutions, aqueous solutions of copper chloride (CuCl2), ferric chloride (FeCl3), ammonium persulfate, sodium persulfate, potassium persulfate, sulfuric acid / hydrogen peroxide, etc. can be cited. Among them, from the perspective of being able to precisely control the etching rate of Cu and being suitable for ensuring the etching time difference with the first etching sacrificial layer 11, sodium persulfate, potassium persulfate and sulfuric acid / hydrogen peroxide are preferred, among which sulfuric acid / hydrogen peroxide is most preferred. As an etching method, a spray method, an immersion method, etc. can be used. In addition, as an etching temperature, it can be appropriately set within a range of more than 25°C and less than 70°C. The etching rate in the present invention can be adjusted by a combination of the above-mentioned etching solution, etching method, etc., and the selection of the material of the first etching sacrificial layer 11 shown below.
[0041] The material constituting the first etching sacrificial layer 11 is preferably a metal that is electrochemically lower than Cu. Examples of such preferred metals include Cu-Zn alloys, Cu-Sn alloys, Cu-Mn alloys, Cu-Al alloys, Cu-Mg alloys, Fe metals, Zn metals, Co metals, Mo metals and oxides thereof, and combinations thereof, and Cu-Zn alloys are particularly preferred. For the Cu-Zn alloy that can constitute the first etching sacrificial layer 11, from the viewpoint of obtaining a high sacrificial effect, the Zn content is preferably 40% by weight or more, more preferably 50% by weight or more, further preferably 60% by weight or more, and particularly preferably 70% by weight or more. In addition, from the viewpoint of maintaining the uniformity of the in-plane dissolution rate of the first etching sacrificial layer 11 and the in-plane uniformity of the local battery reaction with the second etching sacrificial layer 12 and / or the copper layer 13, the Zn content in the Cu-Zn alloy is preferably 98% by weight or less, more preferably 96% by weight or less, and further preferably 94% by weight or less. The first etching sacrificial layer 11 preferably has a thickness d1 of 0.1 μm to 5 μm, more preferably 0.1 μm to 4.5 μm, further preferably 0.2 μm to 4 μm, particularly preferably 0.2 μm to 3.5 μm, and most preferably 0.3 μm to 3 μm.
[0042] As long as the etching rate of the second etching sacrificial layer 12 is higher than Cu and lower than the first etching sacrificial layer 11 (i.e., the aforementioned relationship of r1>r2>1.0 is satisfied), there is no particular limitation. If the etching rate is higher than Cu (the etching rate ratio r2 is higher than 1.0), not only can it be dissolved and removed simultaneously by Cu etching, but even if the second etching sacrificial layer 12 is unevenly dissolved and Cu is partially exposed, the dissolution of the copper layer (seed layer) of the substrate is suppressed by local battery reaction, thereby evenly etching the seed layer in the surface, and the defects of the seed layer, local circuit depressions, and defects can be suppressed. In addition, since the etching rate ratio r2 is lower than the etching rate ratio r1, when the chemical solution treatment is performed in a state where both the first etching sacrificial layer 11 and the second etching sacrificial layer 12 are partially exposed, the first etching sacrificial layer 11 is preferentially dissolved than the second etching sacrificial layer 12 by local battery reaction. Thus, at the moment of micro-etching, the second etching sacrificial layer 12 can remain in a state where dissolution is suppressed. As a result, even when a chemical solution treatment is performed after perforation, the generation of seed layer defects and the like can be suppressed. As for the etching rate of the second etching sacrificial layer 12, as described above with respect to the first etching sacrificial layer 11, the preferred methods such as etching solution and etching method are also directly applicable to the second etching sacrificial layer 12. From the viewpoint of obtaining a high sacrificial effect, the preferred etching rate ratio r2 is 1.2 or more, more preferably 1.25 or more. The upper limit of the etching rate ratio r2 is not particularly limited. In order to uniformly maintain the dissolution rate of the second etching sacrificial layer 12 in the plane and make the local battery reaction with the copper layer 13 uniformly act in the plane, the etching rate ratio r2 is preferably 5.0 or less, more preferably 4.5 or less, more preferably 4.0 or less, more preferably 3.5 or less, particularly preferably 3.0 or less, and most preferably 2.7 or less.
[0043] From the viewpoint of obtaining a high sacrificial effect, the material constituting the second etching sacrificial layer 12 is preferably a metal that is electrochemically inferior to Cu. Examples of such preferred metals include Cu-Zn alloys, Cu-Sn alloys, Cu-Mn alloys, Cu-Al alloys, Cu-Mg alloys, Fe metals, Zn metals, Co metals, Mo metals, and oxides thereof, and combinations thereof. More preferred examples include Cu-Zn alloys, Fe metals, and oxides thereof, and combinations thereof, and Cu-Zn alloys are particularly preferred. For the Cu-Zn alloy that can constitute the second etching sacrificial layer 12, from the viewpoint of obtaining a high sacrificial effect, the Zn content is preferably 40% by weight or more, more preferably 50% by weight or more, and further preferably 60% by weight or more. In addition, from the perspective of maintaining the uniform in-plane dissolution rate of the above-mentioned second etching sacrificial layer 12 and the uniform in-plane effect of the local battery reaction with the copper layer 13, the Zn content in the Cu-Zn alloy is preferably 98 weight % or less, more preferably 96 weight % or less, further preferably 94 weight % or less, and particularly preferably 92 weight % or less.
[0044] From the viewpoint of obtaining a high diffusion prevention effect, the second etching sacrificial layer 12 is also preferably composed of at least one selected from Fe metal, Fe-W alloy, Co metal, Co-W alloy, Co-Ni alloy and their oxides, and combinations thereof. As more preferred examples, Fe metal, Fe-W alloy and their oxides, and combinations thereof can be cited, and Fe metal is particularly preferred. The second etching sacrificial layer 12 preferably has a thickness d2 of 0.05 μm or more and 2.5 μm or less, and a more preferred thickness d2 is 0.06 μm or more and 2.0 μm or less, further preferably 0.06 μm or more and 1.5 μm or less, particularly preferably 0.07 μm or more and 1.0 μm or less, and most preferably 0.07 μm or more and 0.5 μm or less. When the thickness d2 is within such a range, the desired sacrificial effect can be obtained, and a further excellent diffusion prevention effect can be exerted.
[0045] The first etching sacrificial layer 11 and the second etching sacrificial layer 12 may be selected from any combination of the above-mentioned metals and / or alloys, for example, to satisfy the above-mentioned relationship of r1>r2>1.0. The first etching sacrificial layer 11 and the second etching sacrificial layer 12 may be alloys of the same type or metals and / or alloys of different types. When the first etching sacrificial layer 11 and the second etching sacrificial layer 12 are composed of the same type of alloy, it is preferred to adjust the ratio of the elements constituting the respective alloys so as to satisfy the relationship of r1>r2>1.0. For example, the first etching sacrificial layer 11 and the second etching sacrificial layer 12 may each be composed of a Cu-Zn alloy, and when the Zn content of the first etching sacrificial layer 11 is set to x and the Zn content of the second etching sacrificial layer 12 is set to y, from the viewpoint of obtaining a high sacrificial effect, it is preferred to satisfy x>y≥50 weight %. In addition, it is also preferable that the first etching sacrificial layer 11 is composed of a Cu—Zn alloy or Zn metal, and the second etching sacrificial layer 12 is composed of Fe metal. This can further effectively prevent diffusion of Zn from the first etching sacrificial layer 11 through the second etching sacrificial layer 12 .
[0046] The copper layer 13 may be a known structure, and is not particularly limited. For example, the copper layer 13 may be a copper layer formed by a wet film forming method such as chemical plating and electrolytic plating, a dry film forming method such as sputtering and chemical vapor deposition, or a combination thereof. The copper layer 13 preferably has a thickness d3 of 0.1 μm or more and 2.5 μm or less, and a more preferred thickness d3 is 0.1 μm or more and 2 μm or less, further preferably 0.1 μm or more and 1.5 μm or less, particularly preferably 0.2 μm or more and 1 μm or less, and most preferably 0.2 μm or more and 0.8 μm or less. When the thickness d3 is within such a range, it is a sufficient thinness suitable for forming a circuit, and can more effectively prevent defects such as defects during Cu etching.
[0047] The surface of the copper layer 13 is preferably roughened. Since roughened particles formed by the roughening treatment are attached to the surface of the copper layer, the adhesion with the insulating resin layer during the manufacture of the metal-clad laminate and the printed circuit board can be improved. In addition, in the ETS method, image detection is easy to perform after the wiring pattern is formed and the adhesion with the photoresist pattern 20 can be improved. The average particle size D of the roughened particles by image analysis is preferably 0.04 μm or more and 0.53 μm or less, more preferably 0.08 μm or more and 0.13 μm or less, and further preferably 0.09 μm or more and 0.12 μm or less. When it is within the above preferred range, in the ETS method, the roughened surface will have a moderate roughness to ensure excellent adhesion with the photoresist, and the opening of the area where the photoresist is not required can be well achieved when the photoresist is developed. As a result, it is possible to effectively prevent the line defects of the pattern plating layer 22 that may be caused by the difficulty of plating due to the photoresist that is not fully opened. Therefore, when it is within the above preferred range, it can be said that the photoresist has excellent developability and pattern plating properties, and therefore, it is suitable for the fine formation of the wiring pattern 24. It should be noted that the average particle size D of the roughened particles based on image analysis is preferably measured in the following manner: an image is taken at a magnification of a predetermined number of particles (for example, more than 1000 and less than 3000) in one field of view of a scanning electron microscope (SEM), and the image is processed using commercially available image analysis software to measure, for example, 200 particles selected at random are taken as the object, and the average diameter of these particles can be used as the average particle size D.
[0048] The particle density ρ of the roughening particles based on image analysis is preferably 4 particles / μm. 2 More than 200 pieces / μm 2 Below, more preferably 40 / μm 2 More than 170 / μm 2 Below, 70 / μm 2 More than 100 / μm 2Below. In addition, when the roughening particles on the surface of the copper layer are densely present, in the ETS method, it is easy to generate the development residue of the photoresist, but when it is within the above preferred range, it is not easy to generate such development residue, so the developability of the photoresist pattern 20 is also excellent. Therefore, when it is within the above preferred range, it can be said that it is suitable for the fine formation of the wiring pattern 24. It should be noted that the particle density ρ of the roughening particles based on image analysis is preferably measured in the following manner: an image is taken at a magnification of a predetermined number of particles (for example, more than 1000 and less than 3000) in a field of view of a scanning electron microscope (SEM), and the image is processed using commercially available image analysis software to measure, for example, the value obtained by dividing the number of these particles (for example, 200) in a field of view where 200 particles exist by the field of view area can be used as the particle density ρ.
[0049] In addition to the above-mentioned roughening treatment for the attachment of roughening particles, the surface of the copper layer 13 is preferably subjected to rust prevention treatment such as nickel-zinc / chromate treatment, coupling treatment based on a silane coupling agent, etc. These surface treatments can improve the chemical stability of the copper layer surface and improve the adhesion when the insulating layer is stacked.
[0050] The additional copper layer 14 to be set as desired can be a known copper foil composition, without special limitation. By having the additional copper layer 14, the following advantages are achieved: the first etching sacrificial layer 11 with a fast dissolution rate in the pretreatment of the Cu etching process can be controlled so that it is not exposed, and the peeling with the following peeling layer is easy. The additional copper layer 14 can be an additional copper layer formed by a wet film forming method such as chemical plating and electrolytic plating, a dry film forming method such as sputtering and chemical evaporation, or a combination thereof. The additional copper layer 14 preferably has a thickness d3' of 0.1 μm or more and 2.5 μm or less, more preferably 0.1 μm or more and 2 μm or less, further preferably 0.2 μm or more and 1.5 μm or less, particularly preferably 0.2 μm or more and 1 μm or less, and most preferably 0.3 μm or more and 0.8 μm or less. When the thickness d3' is within such a range, the first etching sacrificial layer 11 can be more effectively protected in the process before Cu etching (for example, a chemical solution process such as desmearing), and the conditions of d1 / r1+d2 / r2≥d3'+d2' / r2' and / or d1+d2+d3+d3'+d2'≤3.0μm described later can be easily satisfied. As a result, defects and other undesirable conditions during Cu etching can be more effectively prevented.
[0051] The diffusion prevention layer 15 set as desired is a layer having the function of preventing metals and the like from diffusing from the first etching sacrificial layer 11 to the additional copper layer 14, and can be set to a configuration based on the second etching sacrificial layer 12. Therefore, from the viewpoint of obtaining a high diffusion prevention effect, the diffusion prevention layer 15 is preferably composed of at least one selected from Fe metal, Fe-W alloy, Co metal, Co-W alloy, Co-Ni alloy, their oxides, and combinations thereof, and more preferably Fe metal, Fe-W alloy, their oxides, and combinations thereof can be cited as more preferred examples, and Fe metal is particularly preferred. The diffusion prevention layer 15 preferably has a thickness d2' of 0.05 μm or more and 2.5 μm or less, more preferably 0.06 μm or more and 2.0 μm or less, further preferably 0.06 μm or more and 1.5 μm or less, particularly preferably 0.07 μm or more and 1.0 μm or less, and most preferably 0.07 μm or more and 0.5 μm or less. When the thickness d2' is within such a range, the diffusion of metals etc. from the first etching sacrificial layer 11 can be more effectively prevented, and the conditions of d1 / r1+d2 / r2≥d3'+d2' / r2' and / or d1+d2+d3+d3'+d2'≤3.0μm described later can be easily satisfied. As a result, defects such as defects during Cu etching can be more effectively prevented.
[0052] However, the additional copper layer 14 and the diffusion prevention layer 15 can protect the first etching sacrificial layer 11 from being dissolved by the chemical solution in the subsequent process of Cu etching (e.g., chemical solution process such as desmearing) or can prevent the diffusion of metals etc. from the first etching sacrificial layer 11. On the other hand, if the thickness is too thick, the copper layer 13 (seed layer) after etching may be defective. From the viewpoint of effectively preventing the above-mentioned defect, when the ratio of the etching rate of the diffusion prevention layer 15 to the etching rate of Cu is set to r2', the ratio d1 / r1 of the thickness d1 of the first etching sacrificial layer 11 to the etching rate ratio r1, the ratio d2 / r2 of the thickness d2 of the second etching sacrificial layer 12 to the etching rate ratio r2, the thickness d3' of the additional copper layer 14, and the ratio d2' / r2' of the thickness d2' of the diffusion prevention layer 15 (when the diffusion prevention layer exists) to the etching rate ratio r2' preferably satisfy d1 / r1+d2 / r2≥d3'+d2' / r2'. Regarding this situation, refer to Fig.13 and 14 The stacked body of the metal foil 10, 10' and the insulating layer 28 schematically shown in FIG. 1 is described as follows. It should be noted that for the sake of convenience, Fig.13 and 14In the following description, the first etching sacrificial layer 11 and the second etching sacrificial layer 12 are sometimes referred to as "etching sacrificial layers 11, 12", or the additional copper layers 14, 14' and the diffusion prevention layer are sometimes referred to as "additional copper layers 14, 14', etc." Fig.14 As shown in (a), when the additional copper layer 14' is too thick, the additional copper layer 14' is unevenly dissolved to expose the etching sacrifice layers 11 and 12 ( Fig.14 (b)), the exposed etching sacrificial layers 11 and 12 are immediately dissolved (prioritized over the remaining additional copper layer 14' etc.) to expose the seed layer 13 ( Fig.14 As a result, while the remaining additional copper layer 14' and the like are being dissolved, the exposed seed layer 13 is also being dissolved ( Fig.14 (d)), the seed layer 13 may have defects 13a (refer to Fig.14 (e)). In contrast, Fig.13 As shown in (a), when the additional copper layer 14 is moderately thin, the additional copper layer 14 is thin, so the deviation during dissolution is small ( Fig.13 (b)), the additional copper layer 14 etc. will be completely dissolved before the etching sacrificial layers 11 and 12 are dissolved and the seed layer 13 is exposed ( Fig.13 As a result, the etching sacrificial layers 11 and 12 and the seed layer 13 are simultaneously exposed to the etching solution, thereby exhibiting a sacrificial effect brought about by the etching sacrificial layers 11 and 12 ( Fig.13 (d)), the seed layer 13 will not have defects ( Fig.13 (e)). Thus, from the viewpoint of preventing defects, it is desirable that the time for the additional copper layer 14 and the diffusion prevention layer 15 to be completely dissolved is shorter than the time for the first etching sacrificial layer 11 and the second etching sacrificial layer 12 to be completely dissolved. Therefore, when the etching rate of the first etching sacrificial layer 11 is set to v1, the etching rate of the second etching sacrificial layer 12 is set to v2, the etching rate of the additional copper layer 14 is set to v3', and the etching rate of the diffusion prevention layer 15 is set to v2', it can be said that the following relationship is ideally satisfied:
[0053] d1 / v1+d2 / v2≥d3' / v3'+d2' / v2'
[0054]
[0055]
[0056] That is, since the etching rate v3' of the additional copper layer 14 is only the etching rate relative to Cu, when the etching rate ratio r is used, v1 / v3'=r1, v2 / v3'=r2, v2' / v3'r2'. Therefore, as described above, it can be said that d1 / r1+d2 / r2≥d3'+d2' / r2' is preferably satisfied.
[0057] The number of pinholes per unit area of the metal foil 10 is preferably 2 / mm. 2 As a result, defects such as defects caused by chemical solution corrosion during Cu etching can be further reduced. In particular, the number of pinholes per unit area of the additional copper layer 14 (the first etching sacrificial layer 11 when the additional copper layer 14 is not present) is preferably 2 / mm 2 This is because if the number of pinholes in the additional copper layer 14 is as small as described above, the number of pinholes that may appear in the diffusion prevention layer 15 plated on the additional copper layer 14, the first etching sacrificial layer 11, the second etching sacrificial layer 12, and the copper layer 13 during the manufacturing process of the metal foil 10 will also be reduced.
[0058] In the metal foil 10, the total thickness d1+d2+d3+d2'+d3' of the thickness d1 of the first etching sacrificial layer 11, the thickness d2 of the second etching sacrificial layer 12, the thickness d3 of the copper layer 13, the thickness d2' of the diffusion prevention layer 15 (if present), and the thickness d3' of the additional copper layer 14 (if present) is preferably 3.0 μm or less, more preferably 0.3 μm or more and 2.8 μm or less, further preferably 0.6 μm or more and 2.8 μm or less, and particularly preferably 0.9 μm or more and 2.6 μm or less. The total thickness within such a range means that the thickness of the metal foil 10 is sufficiently thin, and the direct laser opening property of the metal foil 10 is improved.
[0059] As long as the sacrificial effect of the first etching sacrificial layer 11 and the second etching sacrificial layer 12 is not hindered, other layers may be present between the additional copper layer 14 and the anti-diffusion layer 15, between the anti-diffusion layer 15 and the first etching sacrificial layer 11, between the first etching sacrificial layer 11 and the second etching sacrificial layer 12, and / or between the second etching sacrificial layer 12 and the copper layer 13 as desired.
[0060] Metal foil with carrier
[0061] The metal foil 10 (i.e., the laminate of the copper layer 13, the second etching sacrificial layer 12, the first etching sacrificial layer 11, the diffusion prevention layer 15 if present, and the additional copper layer 14 if present) can be provided in the form of a metal foil without a carrier, such as Figure 1As shown, it can also be provided in the form of a metal foil 16 with a carrier, but it is preferably provided in the form of a metal foil 16 with a carrier. In this case, the metal foil 16 with a carrier may include a carrier 17, a peeling layer 18, an additional copper layer 14 (if present), a diffusion prevention layer 15 (if present), a first etching sacrificial layer 11, a second etching sacrificial layer 12, and a copper layer 13 in this order, or it may include a carrier 17, an additional copper layer 14 (if present), a diffusion prevention layer 15 (if present), a first etching sacrificial layer 11, a second etching sacrificial layer 12, and a copper layer 13 in this order. That is, the peeling layer 18 may be included, or the peeling layer 18 may not be included in the form of a separate layer. A preferred metal foil with a carrier includes a carrier 17, a peeling layer 18, and a metal foil 10 in this order.
[0062] The carrier 17 is a layer (typically a foil) for supporting the metal foil and improving its handling properties. Examples of the carrier include aluminum foil, copper foil, stainless steel foil, resin film, resin film with a metal coating on the surface, glass plate, etc., preferably copper foil. The copper foil can be any of rolled copper foil and electrolytic copper foil. The thickness of the carrier is typically 250 μm or less, preferably 12 μm or more and 200 μm or less.
[0063] The peeling layer 18 is a layer having the following functions: reducing the peeling strength of the carrier 17, ensuring the stability of the strength, and further suppressing the mutual diffusion that may occur between the carrier and the metal foil when the press molding is performed at high temperature. The peeling layer is usually formed on one side of the carrier, but it can also be formed on both sides. The peeling layer can be any of an organic peeling layer and an inorganic peeling layer. Examples of organic components used in the organic peeling layer include nitrogen-containing organic compounds, sulfur-containing organic compounds, carboxylic acids, etc. Examples of nitrogen-containing organic compounds include triazole compounds, imidazole compounds, etc., among which triazole compounds are preferred from the perspective of easy and stable peeling properties. Examples of triazole compounds include 1,2,3-benzotriazole, carbonylbenzotriazole, N',N'-bis(benzotriazolylmethyl)urea, 1H-1,2,4-triazole and 3-amino-1H-1,2,4-triazole, etc. Examples of sulfur-containing organic compounds include mercaptobenzothiazole, trithiocyanate, 2-benzimidazolethiol, etc. Examples of carboxylic acids include monocarboxylic acids and dicarboxylic acids. On the other hand, examples of inorganic components used in the inorganic peeling layer include Ni, Mo, Co, Cr, Fe, Ti, W, P, Zn, chromate-treated films, carbon layers, and the like. It should be noted that the peeling layer can be formed by contacting a solution containing peeling layer components with the surface of at least one side of the carrier, adsorbing the peeling layer components on the surface of the carrier in the solution, and the like. When the carrier is contacted with the solution containing peeling layer components, the contact can be carried out by immersing in the solution containing peeling layer components, spraying the solution containing peeling layer components, and flowing the solution containing peeling layer components. In addition, a method of forming a coating of the peeling layer components by a plating method such as electrolytic plating and chemical plating, or a gas phase method based on evaporation, sputtering, and the like can also be used. In addition, the fixing of the peeling layer components on the surface of the carrier can be carried out by drying the solution containing the peeling layer components, electrodeposition of the peeling layer components in the solution containing the peeling layer components, and the like. The thickness of the peeling layer is typically 1 nm to 1 μm, preferably 5 nm to 500 nm. It should be noted that the peeling strength between the peeling layer 18 and the carrier is preferably 5 gf / cm to 50 gf / cm, more preferably 5 gf / cm to 40 gf / cm, and further preferably 6 gf / cm to 30 gf / cm.
[0064] Metal-clad laminate
[0065] The metal foil of the present invention is preferably used for the production of metal-clad laminates for printed circuit boards. That is, according to a preferred embodiment of the present invention, a metal-clad laminate having the above-mentioned metal foil can be provided. The metal-clad laminate can be provided with a metal foil in the form of a metal foil with a carrier. In addition, the metal foil can be provided on a single side of the resin layer, or on both sides. The resin layer typically contains a resin, preferably an insulating resin. The resin layer is preferably a prepreg and / or a resin sheet, more preferably a prepreg. Prepreg is a general term for composite materials formed by impregnating or laminating synthetic resins on substrates such as synthetic resin plates, glass plates, glass fabrics, glass non-woven fabrics, and paper. As preferred examples of insulating resins impregnated in prepregs, epoxy resins, cyanate resins, bismaleimide triazine resins (BT resins), polyphenylene ether resins, phenolic resins, polyamide resins, etc. can be cited. In addition, as examples of insulating resins constituting resin sheets, insulating resins such as epoxy resins, polyimide resins, and polyester resins (liquid crystal polymers) can be cited. In addition, from the viewpoint of reducing the thermal expansion coefficient of the resin layer and improving rigidity, filler particles composed of various inorganic particles such as silicon dioxide and aluminum oxide may also be contained. The thickness of the resin layer is not particularly limited, preferably 3 μm or more and 1000 μm or less, more preferably 5 μm or more and 400 μm or less, and further preferably 10 μm or more and 200 μm or less. The resin layer may be composed of multiple layers. The resin layer such as prepreg and / or resin sheet may be pre-clamped on the metal foil surface and disposed on the metal foil with a carrier.
[0066] Method for manufacturing printed circuit board
[0067] The metal foil of the present invention or the metal foil with a carrier as described above can be used to preferably manufacture a printed circuit board. Preferred examples of the method for manufacturing a printed circuit board include the MSAP method (modified semi-additive method) and the coreless lamination method (ETS method), but are not limited to these methods. The metal foil of the present invention or the metal foil with a carrier can be used in various methods that can expect certain advantages brought about by the sacrificial effect of the first etching sacrificial layer 11 and the second etching sacrificial layer 12.
[0068] As an example, a method for manufacturing a printed circuit board based on a coreless build-up method (ETS method) using the metal foil of the present invention is described below. In this method, first, a support body is obtained using a metal foil 10 having an additional copper layer 14 (if present), an anti-diffusion layer 15 (if present), a first etching sacrificial layer 11, a second etching sacrificial layer 12, and a copper layer 13. Next, a build-up wiring layer including at least a first wiring layer 26 made of copper and an insulating layer 28 is formed on the copper layer 13 to obtain a laminated body with a build-up wiring layer. It should be noted that, as described later Fig.12As shown, it is obvious that the built-up wiring layer can be a multi-layered built-up wiring layer formed up to the n-th wiring layer 40 (n is an integer greater than 2). Then, the additional copper layer 14 (if present), the diffusion prevention layer 15 (if present), the first etching sacrificial layer 11, the second etching sacrificial layer 12 and the copper layer 13 are removed by an etching solution to expose the first wiring layer 26, thereby obtaining a printed circuit board including the built-up wiring layer.
[0069] Below, in Figure 1 Based on the reference Fig.11 and 12 The manufacturing method is described with reference to the process diagram shown. Fig.11 and 12 Although the method shown is drawn as providing the metal foil 16 with a carrier on one side of the coreless support body 19 to form the built-up wiring layer 42 for the sake of simplicity of explanation, it is ideal to provide the metal foil 16 with a carrier on both sides of the coreless support body 19 to form the built-up wiring layer 42 on these two sides.
[0070] (1) Preparation of a support using metal foil
[0071] Prepare a metal foil 10 or a metal foil 16 with a carrier containing the metal foil 10 as a support. As desired, before forming a laminate with a built-up wiring layer, the metal foil 10 (additional copper layer 14 side) or the metal foil 16 with a carrier (carrier 17 side) can be stacked on one or both sides of a coreless support 19 to form a laminate. That is, the above-mentioned metal-clad laminate can also be formed at this stage. The stacking can be carried out according to the known conditions and methods used in stacking copper foil and prepreg in the usual printed circuit board manufacturing process. The coreless support 19 typically contains a resin, preferably an insulating resin. The coreless support 19 is preferably a prepreg and / or a resin sheet, more preferably a prepreg. That is, the coreless support 19 is equivalent to the resin layer in the above-mentioned metal-clad laminate, and therefore, the above-mentioned preferred method for the metal-clad laminate and / or the resin layer is directly applicable to the coreless support 19.
[0072] (2) Formation of a Laminated Body with Build-up Wiring Layers
[0073] A build-up wiring layer 42 including at least a first wiring layer 26 made of copper and an insulating layer 28 is formed on the copper layer 13 to obtain a laminate with a build-up wiring layer. The insulating layer 28 can be composed of an insulating resin as described above. The build-up wiring layer 42 can be formed according to a known method for manufacturing a printed circuit board, and is not particularly limited. According to a preferred embodiment of the present invention, as described below, after (i) forming a photoresist pattern, (ii) electroplating copper, and (iii) stripping the photoresist pattern to form the first wiring layer 26, (iv) the build-up wiring layer 42 is formed.
[0074] (i) Forming a photoresist pattern
[0075] First, a photoresist pattern 20 is formed on the surface of the copper layer 13. The photoresist pattern 20 can be formed by using either a negative resist or a positive resist, and the photoresist can be either a film type or a liquid type. In addition, the developer can be a developer such as sodium carbonate, sodium hydroxide, or an amine aqueous solution, and can be carried out according to various methods and conditions commonly used in the manufacture of printed circuit boards without particular limitation.
[0076] (ii) Electroplated copper
[0077] Next, copper layer 13 having photoresist pattern 20 formed thereon is subjected to copper electroplating 22. The formation of copper electroplating 22 can be performed by various pattern plating methods and conditions commonly used in the manufacture of printed circuit boards, such as copper sulfate plating solution and copper pyrophosphate plating solution, and is not particularly limited.
[0078] (iii) Stripping of photoresist pattern
[0079] The photoresist pattern 20 is peeled off to form a wiring pattern 24. The photoresist pattern 20 can be peeled off by using a sodium hydroxide aqueous solution, an amine solution and / or an aqueous solution thereof, etc., and can be carried out according to various peeling methods and conditions commonly used in the manufacture of printed circuit boards, without particular limitation. In this way, a wiring pattern 24 consisting of a first wiring layer 26 and in which wiring portions (lines) are arranged with gap portions (spaces) is directly formed on the surface of the copper layer 13. For example, in order to miniaturize the circuit, it is preferred to form a wiring pattern with a line / space (L / S) height miniaturized to a level of less than 13μm / less than 13μm (e.g., 12μm / 12μm, 10μm / 10μm, 5μm / 5μm, 2μm / 2μm).
[0080] (iv) Formation of build-up wiring layer
[0081] The built-up wiring layer 42 is formed on the copper layer 13 to produce a laminated body with the built-up wiring layer. For example, on the basis of the first wiring layer 26 already formed on the copper layer 13, the insulating layer 28 and the second wiring layer 38 are sequentially formed to produce the built-up wiring layer 42. Fig.12As shown, in order to form the built-up wiring layer 42, the insulating layer 28 and the copper foil 30 with a carrier (including the carrier 32, the peeling layer 34 and the copper foil 36) may be stacked, the carrier 32 may be peeled off, and the copper foil 36 and the insulating layer 28 directly thereunder may be laser processed using a carbon dioxide gas laser or the like. Then, the second wiring layer 38 may be formed by patterning by chemical copper plating, photoresist processing, electrolytic copper plating, photoresist peeling and flash etching, and this patterning may be repeated as needed until the n-th wiring layer 40 (n is an integer greater than or equal to 2) is formed.
[0082] The method for forming the second wiring layer 38 and subsequent build-up layers is not limited to the above method, and a subtractive method, MSAP (modified semi-additive process) method, SAP (semi-additive) method, full-additive method, etc. can be used. For example, in the case where a resin layer and a metal foil represented by a copper foil are laminated simultaneously by pressing, the panel plating and the metal foil are etched in combination with the formation of interlayer conduction means such as via formation and panel plating, so that a wiring pattern can be formed. In addition, in the case where only a resin layer is laminated on the surface of the copper layer 13 by pressing or lamination, a wiring pattern can also be formed on the surface by a semi-additive method.
[0083] The above steps are repeated as needed to obtain a laminate with a built-up wiring layer. In this step, it is preferred that a built-up wiring layer is formed by alternately stacking a resin layer and a wiring layer containing a wiring pattern to obtain a laminate with a built-up wiring layer formed up to the nth wiring layer 40 (n is an integer greater than 2). This step can be repeated until the desired number of built-up wiring layers are formed. At this stage, bumps for mounting such as solder resist and pillars can also be formed on the outer surface as needed. In addition, the outermost surface of the built-up wiring layer can also be formed into an outer wiring pattern in a subsequent outer layer processing step.
[0084] (3) Formation of printed circuit boards including build-up wiring layers
[0085] (i) Separation of a Laminated Body with Build-up Wiring Layers
[0086] After forming the laminate with the built-up wiring layer, the laminate with the built-up wiring layer can be separated by the peeling layer 18 or the like. When the metal foil with a carrier sequentially includes the carrier 17, the peeling layer 18, the additional copper layer 14, the diffusion prevention layer 15, the first etching sacrificial layer 11, the second etching sacrificial layer 12, and the copper layer 13, the method of the present invention preferably separates the laminate with the built-up wiring layer by the peeling layer 18 to expose the additional copper layer 14 before removing it with the etching solution described later. The separation method is preferably physical peeling, and the peeling method can be a method based on a machine or a jig, manual work, or a combination thereof.
[0087] On the other hand, when the metal foil with a carrier sequentially comprises a carrier 17, an additional copper layer 14, a first etching sacrificial layer 11, a second etching sacrificial layer 12, and a copper layer 13 (i.e., when the peeling layer 18 is not present as a separate layer), the method of the present invention preferably separates the laminate with the build-up wiring layer between the carrier 17 and the additional copper layer 14 or inside the additional copper layer 14 to expose the additional copper layer 14 before removing it using the etching solution described later.
[0088] (ii) Etching of sacrificial layer and copper layer
[0089] In the method of the present invention, the additional copper layer 14, the diffusion prevention layer 15, the first etching sacrificial layer 11, the second etching sacrificial layer 12, and the copper layer 13 are removed by an etching liquid to expose the first wiring layer 26, thereby obtaining a printed circuit board 46 including a built-up wiring layer 42. The printed circuit board 46 is preferably a multilayer printed circuit board. In any case, due to the presence of the first etching sacrificial layer 11 and the second etching sacrificial layer 12, the etching removal based on each layer can be efficiently and uniformly performed in the surface by Cu etching, without the need for an additional etching process, and the occurrence of local circuit depression can be suppressed. Therefore, according to the method of the present invention, the additional copper layer 14, the diffusion prevention layer 15, the first etching sacrificial layer 11, the second etching sacrificial layer 12, and the copper layer 13 can be removed by an etching liquid in one process. The etching liquid and etching method used at this time are as described above.
[0090] (iii) External layer processing
[0091] Fig.12 The printed circuit board 46 shown can be processed on the outer layer by various methods. For example, an insulating layer and a wiring layer as a build-up wiring layer can be further stacked in any number of layers on the first wiring layer 26 of the printed circuit board 46, or a solder resist layer can be formed on the surface of the first wiring layer 26, and Ni-Au plating, Ni-Pd-Au plating, water-soluble pre-flux treatment, etc. can be implemented as surface treatment of the outer pad. Further, a columnar support, etc. can be set on the outer pad. At this time, the first wiring layer 26 made by etching the sacrificial layer in the present invention can maintain the uniformity of the circuit thickness in the plane, and the surface of the first wiring layer 26 rarely has local circuit depressions. Therefore, a printed circuit board with excellent installation reliability can be obtained, which has a low incidence of poor local processing in the surface treatment process caused by extremely thin parts of the circuit thickness, circuit depressions, etc., poor solder resist residues, and poor installation caused by unevenness of the mounting pad.
[0092] The above-mentioned method for manufacturing a printed circuit board is based on a coreless build-up method (ETS method), while the method for manufacturing a printed circuit board based on the MSAP method is based on Figure 6 and 7In the conventional MSAP method described above, by using the metal foil 10 of the present invention instead of the ultra-thin copper foil 110 , a printed wiring board can be preferably manufactured.
[0093] Example
[0094] The present invention is further described in detail by the following examples.
[0095] Examples 1 to 4
[0096] The metal foil for printed wiring board production of the present invention was produced and various evaluations were performed as follows.
[0097] (1) Preparation of vector
[0098] As the cathode, a titanium electrode with a polished surface using a #2000 polishing wheel was prepared. In addition, a DSA (dimensional stability anode) was prepared as the anode. These electrodes were immersed in a copper sulfate solution with a copper concentration of 80 g / L and a sulfuric acid concentration of 260 g / L at a solution temperature of 45°C and a current density of 55 A / dm 2 Electrolysis was performed to obtain an electrolytic copper foil having a thickness of 18 μm as a carrier.
[0099] (2) Formation of the peeling layer
[0100] The acid-washed support was immersed in a CBTA solution containing 1 g / L CBTA, 150 g / L sulfuric acid and 10 g / L copper at a temperature of 30°C for 30 seconds to adsorb the CBTA component on the electrode surface of the support. In this way, a CBTA layer was formed on the surface of the electrode surface of the support as an organic release layer.
[0101] (3) Formation of auxiliary metal layer
[0102] The support having the organic release layer formed thereon was immersed in a solution having a nickel concentration of 20 g / L prepared using nickel sulfate and the reaction mixture was stirred at a temperature of 45° C., a pH of 3, and a current density of 5 A / dm 2 Under the condition of , nickel in an amount corresponding to a thickness of 0.001 μm was deposited on the organic release layer. Thus, a nickel layer was formed on the organic release layer as an auxiliary metal layer.
[0103] (4) Formation of additional copper layer
[0104] For Examples 1 to 3, the support having the auxiliary metal layer formed thereon was immersed in a copper sulfate solution having a copper concentration of 60 g / L and a sulfuric acid concentration of 200 g / L, and the solution temperature was 50° C. and the current density was 5 A / dm 2 Above and 30A / dm 2Then, electrolysis was performed to form an additional copper layer having a thickness of 0.3 μm on the auxiliary metal layer. On the other hand, in Example 4, no additional copper layer was formed.
[0105] (5) Formation of diffusion-resistant layer
[0106] In Examples 1 and 2, the carrier having the additional copper layer formed thereon was immersed in the plating bath shown in Table 1, and electrolysis was performed under the plating conditions shown in Table 1, thereby forming a diffusion prevention layer having the composition and thickness shown in Table 2 on the additional copper layer. On the other hand, in Examples 3 and 4, the diffusion prevention layer was not formed.
[0107] (6) Formation of the First Etching Sacrificial Layer
[0108] The carrier formed with the diffusion prevention layer (Examples 1 and 2) or the carrier formed with the additional copper layer (Example 3) was immersed in the plating bath shown in Table 1, and electrolysis was performed under the plating conditions shown in Table 1, thereby forming a first etching sacrificial layer having the composition and thickness shown in Table 2 on the diffusion prevention layer or the additional copper layer. On the other hand, in Example 4, the first etching sacrificial layer was not formed.
[0109] (7) Formation of the Second Etching Sacrificial Layer
[0110] In Examples 1 and 2, the carrier having the first etching sacrificial layer formed thereon was immersed in the plating bath shown in Table 1, and electrolysis was performed under the plating conditions shown in Table 1, thereby forming a second etching sacrificial layer having the composition and thickness shown in Table 2 on the first etching sacrificial layer. On the other hand, in Examples 3 and 4, the second etching sacrificial layer was not formed.
[0111] (8) Formation of copper layer (seed layer)
[0112] The carrier formed with the second etching sacrificial layer (Examples 1 and 2), the carrier formed with the first etching sacrificial layer (Example 3), or the carrier formed with the auxiliary metal layer (Example 4) was immersed in a copper sulfate solution with a copper concentration of 60 g / L and a sulfuric acid concentration of 145 g / L, and the solution temperature was 45° C. and the current density was 30 A / dm 2 Electrolysis was performed to form a copper layer having a thickness shown in Table 2 on the second etching sacrificial layer, the first etching sacrificial layer, or the auxiliary metal layer.
[0113] (9) Roughening treatment
[0114] The surface of the metal foil with carrier thus formed was subjected to a roughening treatment. The roughening treatment consisted of the following steps: a calcination step for precipitating and attaching fine copper particles on the copper layer; and a coating plating step for preventing the fine copper particles from falling off. In the calcination step, an acidic copper sulfate solution containing a copper concentration of 10 g / L and a sulfuric acid concentration of 120 g / L was used at a liquid temperature of 25°C and a current density of 15 A / dm 2In the subsequent coating plating step, an acidic copper sulfate solution containing a copper concentration of 70 g / L and a sulfuric acid concentration of 120 g / L was used at a liquid temperature of 40°C and a current density of 15 A / dm 2 Electrodeposition was carried out under smooth plating conditions.
[0115] (10) Anti-rust treatment
[0116] The surface of the obtained metal foil with carrier was subjected to rust prevention treatment consisting of zinc-nickel alloy plating and chromate treatment. First, an electrolyte solution with a zinc concentration of 0.2 g / L, a nickel concentration of 2 g / L, and a potassium pyrophosphate concentration of 300 g / L was used at a liquid temperature of 40°C and a current density of 0.5 A / dm 2 The surface of the roughened layer and the carrier was plated with zinc-nickel alloy under the conditions of 3 g / L chromic acid solution at pH 10 and current density 5 A / dm 2 The surface treated with zinc-nickel alloy was chromated under the conditions of.
[0117] (11) Silane coupling agent treatment
[0118] The silane coupling agent treatment was performed by adsorbing an aqueous solution containing 2 g / L of 3-glycidoxypropyltrimethoxysilane on the copper layer side surface of the metal foil with a carrier, and evaporating the water with an electric heater. At this time, the carrier side was not treated with a silane coupling agent.
[0119] (12) Evaluation
[0120] The thus obtained metal foil with a carrier and its constituent layers were subjected to various evaluations as shown below.
[0121] Rating 1 : Etching rate ratio
[0122] The etching rate ratio r2 ′ of the diffusion prevention layer, the etching rate ratio r1 of the first etching sacrificial layer, and the etching rate ratio r2 of the second etching sacrificial layer were measured as shown below.
[0123] First, for Examples 1 and 2, the following samples (i) to (iii) were prepared, and for Example 3, the following sample (ii) was prepared. In addition, for Example 4, the following sample (iv) was prepared.
[0124] (i) A metal foil with a carrier whose outermost surface obtained in (5) is a diffusion-preventing layer (i.e., an intermediate product formed up to the diffusion-preventing layer and without forming a first etching sacrificial layer and subsequent treatment)
[0125] (ii) A metal foil with a carrier whose outermost surface obtained in (6) is the first etching sacrificial layer (i.e., an intermediate product in which the first etching sacrificial layer has been formed but the second etching sacrificial layer has not been formed and subsequent treatments have not been performed)
[0126] (iii) A metal foil with a carrier whose outermost surface obtained in (7) above is a second etching sacrifice layer (i.e., an intermediate product formed up to the second etching sacrifice layer and without forming a copper layer and subsequent treatment)
[0127] (iv) A metal foil with a carrier having a copper layer on the outermost surface obtained in (8) above (i.e., an intermediate product formed up to the copper layer and not subjected to roughening treatment or subsequent treatment)
[0128] On the other hand, commercially available concentrated sulfuric acid (95% by weight) and hydrogen peroxide (30% by weight) were dissolved in water to prepare an etching solution with a sulfuric acid concentration of 5.9% by weight and a hydrogen peroxide concentration of 2.1% by weight. Each metal foil sample with a carrier was masked so that the carrier side was not etched, and was immersed in the etching solution at 25°C for a certain period of time to dissolve it. The thickness change of the plated film before and after dissolution was measured using a fluorescent X-ray thickness meter (Fischerscope X-Ray XDAL-FD, manufactured by Fischer Instruments). By dividing the obtained thickness change by the dissolution time, the etching rate of each plated film that is the object is calculated. The etching rate of sample (iv) of Example 4 thus calculated is the etching rate of Cu, and the etching rates of samples (i), (ii) and (iii) in Examples 1 to 3 are the etching rates of each diffusion prevention layer, each first etching sacrificial layer and each second etching sacrificial layer, respectively. Next, by dividing the etching rates of the diffusion prevention layer, the first etching sacrificial layer, and the second etching sacrificial layer by the etching rate of Cu, the etching rate ratio r2' of the diffusion prevention layer, the etching rate ratio r1 of the first etching sacrificial layer, and the etching rate ratio r2 of the second etching sacrificial layer were calculated. The results are shown in Table 2.
[0129] Rating 2 : Number of pinholes per unit area
[0130] In order to determine the number of pinholes per unit area of the additional copper layer, a copper foil with a carrier whose outermost surface is an additional copper layer obtained in (4) above (i.e., an intermediate product in which an additional copper layer is formed to a thickness of 0.3 μm and no diffusion prevention layer is formed and no subsequent treatment is performed) was prepared. The copper foil with a carrier was laminated on an insulating resin substrate (prepreg R-1661 manufactured by Panasonic Corporation, thickness 0.1 mm) in a manner that the additional copper layer was in contact with one side, and hot pressing was performed at a pressure of 4.0 MPa and a temperature of 190°C for 90 minutes. Then, the carrier was peeled off to obtain a laminated board. The laminated board was observed with an optical microscope in a dark room while irradiating with backlight, and the number of pinholes was counted. In this way, the number of pinholes per 1 mm was determined. 2 The number of pinholes per unit area of the additional copper layer was 2 / mm in Examples 1 to 3. 2 the following.
[0131] Rating 3 :Thermal diffusion of metal into the copper layer (seed layer)
[0132] In order to evaluate thermal diffusion, for Examples 1 to 3, a metal foil with a carrier having a copper layer on the outermost surface obtained in (8) above (i.e., an intermediate product formed up to the copper layer without roughening treatment and subsequent treatment) was prepared. The metal foil with a carrier was heated at a temperature of 220°C for 2 hours in a vacuum, and the composition of the metal foil with a carrier before and after heating was analyzed by a glow discharge optical emission spectrometer (GD-OES) (manufactured by Horiba, Ltd., JY-5000RF). In the sample before heating, an element that is contained in the copper layer at less than 1 weight % (including 0 weight %) and in at least one of the first etching sacrificial layer and the second etching sacrificial layer (if present) at more than 1 weight % is defined as a diffusion confirmation element. For the sample after heating, at the following sites:
[0133] (a) the surface of the copper layer opposite to the second etching sacrificial layer (the surface of the copper layer opposite to the first etching sacrificial layer when the second etching sacrificial layer is not present), or
[0134] (b) a point at a distance of 0.3 μm from the boundary surface between the copper layer and the second etching sacrificial layer (or the boundary surface between the copper layer and the first etching sacrificial layer when the second etching sacrificial layer does not exist) in the depth direction of the copper layer,
[0135] The case where the content of all diffusion confirmation elements at a site close to the second etching sacrificial layer (the first etching sacrificial layer when the second etching sacrificial layer does not exist) is less than 1 weight % is judged as no diffusion, and the case where this is not the case is judged as diffusion. It should be noted that the case where the boundary between the copper layer and the second etching sacrificial layer cannot be distinguished is also judged as diffusion. The results are shown in Table 2.
[0136] Rating 4 :Seed layer defect
[0137] The metal foil with a carrier obtained in the above (11) is laminated on the surface of the inner substrate in a manner close to the copper layer side of the insulating resin substrate (prepreg manufactured by Mitsubishi Gas Chemical Co., Ltd., GHPL-830NS, thickness 0.1mm), and hot pressing is performed for 90 minutes at a pressure of 4.0MPa and a temperature of 220°C. The carrier of the metal-clad laminate thus obtained is peeled off, cut into a size of 10cm×10cm, and immersed in the etching solution prepared in Evaluation 1 until the first etching sacrificial layer and the second etching sacrificial layer (if present) completely disappear. The presence or absence of defects is visually confirmed, and the grade is evaluated according to the following criteria. It should be noted that the so-called defect here refers to the state of the substrate of the base that can be visually identified. The results are shown in Table 2.
[0138] Evaluation A: No defects in the copper layer
[0139] Evaluation B: There are more than 1 and less than 3 defects on the copper layer.
[0140] Evaluation C: Four or more defects appear on the copper layer [Table 1]
[0141]
[0142] [Table 2]
[0143]
Claims
1. A metal foil for printed circuit board manufacturing, comprising a first etching sacrificial layer, a second etching sacrificial layer and a copper layer in sequence, wherein when the ratio of the etching rate of the first etching sacrificial layer to the etching rate of Cu is set to r1 and the ratio of the etching rate of the second etching sacrificial layer to the etching rate of Cu is set to r2, r1>r2>1.0 is satisfied.
2. The metal foil according to claim 1, wherein The ratio r1 is 1.2 or more.
3. The metal foil according to claim 1 or 2, wherein The ratio r2 is greater than or equal to 1.
2.
4. The metal foil according to claim 1 or 2, wherein The first etching sacrificial layer is composed of at least one selected from the group consisting of Cu-Zn alloy, Cu-Sn alloy, Cu-Mn alloy, Cu-Al alloy, Cu-Mg alloy, Fe metal, Zn metal, Co metal, Mo metal and their oxides, and the second etching sacrificial layer is composed of at least one selected from the group consisting of Cu-Zn alloy, Cu-Sn alloy, Cu-Mn alloy, Cu-Al alloy, Cu-Mg alloy, Fe metal, Zn metal, Co metal, Mo metal and their oxides.
5. The metal foil according to claim 1 or 2, wherein The first etching sacrificial layer and the second etching sacrificial layer are respectively made of Cu-Zn alloy, and when the Zn content of the first etching sacrificial layer is x and the Zn content of the second etching sacrificial layer is y, x>y≥50 weight % is satisfied.
6. The metal foil according to claim 1 or 2, wherein The first etching sacrificial layer is made of Cu—Zn alloy or Zn metal, and the second etching sacrificial layer is made of Fe metal.
7. The metal foil according to claim 1, wherein An additional copper layer is further provided on a surface of the first etching sacrificial layer on the opposite side to the second etching sacrificial layer.
8. The metal foil according to claim 7, wherein A diffusion prevention layer is further provided between the additional copper layer and the first etching sacrificial layer.
9. The metal foil according to claim 8, wherein The diffusion prevention layer is composed of at least one selected from the group consisting of Fe metal, Fe-W alloy, Co metal, Co-W alloy, Co-Ni alloy and oxides thereof.
10. The metal foil according to claim 1 or 2, wherein The number of pinholes per unit area of the metal foil is 2 / mm 2 the following.
11. The metal foil according to claim 8, wherein The total thickness d1+d2+d3+d2′+d3′ of the thickness d1 of the first etching sacrificial layer, the thickness d2 of the second etching sacrificial layer, the thickness d3 of the copper layer, the thickness d2′ of the diffusion prevention layer, and the thickness d3′ of the additional copper layer is 3.0 μm or less.
12. The metal foil according to claim 1 or 2, wherein The thickness d2 of the second etching sacrificial layer is greater than or equal to 0.05 μm and less than or equal to 2.5 μm.
13. The metal foil according to claim 1 or 2, wherein The copper layer has a thickness d3 of 0.1 μm or more and 2.5 μm or less.
14. The metal foil according to any one of claims 7 to 9, wherein The thickness d3 ′ of the additional copper layer is greater than or equal to 0.1 μm and less than or equal to 2.5 μm.
15. The metal foil according to claim 8 or 9, wherein When the ratio of the etching rate of the anti-diffusion layer to the etching rate of Cu is set to r2', the ratio d1 / r1 of the thickness d1 of the first etching sacrificial layer to the ratio r1, the ratio d2 / r2 of the thickness d2 of the second etching sacrificial layer to the ratio r2, the thickness d3' of the additional copper layer, and the ratio d2' / r2' of the thickness d2' of the anti-diffusion layer to the ratio r2' satisfy d1 / r1+d2 / r2≥d3'+d2' / r2'. 16 . A metal foil with a carrier, comprising: a carrier, a release layer, and the metal foil according to claim 1 in this order. 17 . A metal-clad laminate comprising the metal foil according to claim 1 .
18. A method for manufacturing a printed circuit board, characterized in that: The metal foil according to any one of claims 1 to 15 or the metal foil with a carrier according to claim 16 is used.