Precursor, method for producing precursor, positive electrode material, method for producing positive electrode material, and lithium ion secondary battery

By using nickel-manganese composite hydroxide and nickel-manganese composite oxide as precursors, a nickel-manganese composite oxide cathode material is prepared, which solves the problem of insufficient discharge capacity and cycle characteristics of lithium-ion secondary batteries and achieves better Battery performance.

CN113646929BActive Publication Date: 2024-10-29JFE MINERAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202080027397.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-07
Publication Date
2024-10-29
Estimated Expiration
2040-04-07

AI Technical Summary

Technical Problem

Existing lithium-containing nickel-manganese composite oxides have problems with insufficient discharge capacity and cycle characteristics as cathode materials for lithium-ion secondary batteries.

Method used

Using nickel-manganese composite hydroxide and nickel-manganese composite oxide as precursors, the molar ratio of nickel and manganese is controlled between 0.45-0.60, the average valence of manganese is less than 4.0, the particle size is less than 0.6μm, and through specific manufacturing Methods such as co-precipitation and sintering processes are used to prepare lithium-containing nickel-manganese composite oxide cathode materials.

Benefits of technology

It improves the discharge capacity and cycle characteristics of lithium-ion secondary batteries, ensures that lithium ions can diffuse evenly, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003293467970000221
    Figure BDA0003293467970000221
  • Figure BDA0003293467970000251
    Figure BDA0003293467970000251
  • Figure BDA0003293467970000291
    Figure BDA0003293467970000291
Patent Text Reader

Abstract

The present invention provides a precursor of a positive electrode material for a lithium ion secondary battery having excellent discharge capacity and cycle characteristics and a method for manufacturing the same. The precursor is a precursor of a positive electrode material used in a lithium ion secondary battery, wherein the precursor is at least one selected from the group consisting of a nickel-manganese composite hydroxide and a nickel-manganese composite oxide, contains nickel and manganese, the ratio of the nickel content to the total of the nickel content and the manganese content is 0.45 or more and 0.60 or less in molar ratio, and the average valence of manganese is less than 4.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a precursor, a method for producing the precursor, a positive electrode material, a method for producing the positive electrode material, and a lithium ion secondary battery. Background Art

[0002] As a positive electrode material (positive electrode active material) of a lithium ion secondary battery, lithium cobalt oxide is widely used.

[0003] However, cobalt contained in lithium cobalt oxide is a rare metal with an annual production of only about 20,000 tons. Therefore, from the perspective of resource quantity and cost, a positive electrode material that can replace lithium cobalt oxide is needed.

[0004] Therefore, conventionally, a lithium-containing nickel-manganese composite oxide has been proposed as a positive electrode material that does not contain cobalt (Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2002-42813 Summary of the invention

[0008] Problems to be solved by the invention

[0009] Conventional lithium-ion secondary batteries using lithium-containing nickel-manganese composite oxides as positive electrode materials have insufficient discharge capacity and cycle characteristics.

[0010] Therefore, an object of the present invention is to provide a precursor of a positive electrode material capable of obtaining a lithium ion secondary battery having excellent discharge capacity and cycle characteristics, and a method for producing the same.

[0011] Another object of the present invention is to provide a positive electrode material and a method for producing the same that can provide a lithium ion secondary battery having excellent discharge capacity and cycle characteristics.

[0012] Another object of the present invention is to provide a lithium ion secondary battery having excellent discharge capacity and cycle characteristics.

[0013] Methods used to solve problems

[0014] The present inventors have conducted intensive studies and, as a result, have found that the above-mentioned object can be achieved by adopting the following configuration, thereby completing the present invention.

[0015] That is, the present invention provides the following [1] to

[20] .

[0016] [1] A precursor of a positive electrode material used in a lithium-ion secondary battery, wherein the precursor is at least one selected from the group consisting of a nickel-manganese composite hydroxide and a nickel-manganese composite oxide, contains nickel and manganese, the ratio of the nickel content to the total of the nickel content and the manganese content is 0.45 to 0.60 in terms of molar ratio, and the average valence of manganese is less than 4.0.

[0017] [2] The precursor according to [1] above, wherein the average particle size of the primary particles is less than 0.6 μm.

[0018] [3] The precursor according to [1] or [2] above, wherein the mass reduction when heated from room temperature to 1050° C. in an air atmosphere is 16% by mass or more.

[0019] [4] The precursor according to any one of [1] to [3] above, wherein the peak intensity ratio of the peak intensity of the

[001] orientation to the peak intensity of the

[101] orientation in X-ray diffraction, i.e., the

[001] /

[101] peak ratio, is 14 or less.

[0020] The peak intensity of the

[001] orientation is the maximum peak intensity when the diffraction angle 2θ is in the range of 17 to 21°, and the peak of the

[101] orientation is the maximum peak intensity when the diffraction angle 2θ is in the range of 30 to 40°.

[0021] [5] A method for producing a precursor, which is a method for producing the precursor described in any one of [1] to [4] above, wherein a nickel source, a manganese source, an ammonium source and an alkaline aqueous solution are introduced into a reaction tank liquid with a pH of 9 to 12 to obtain a precipitate.

[0022] [6] A method for producing a precursor as described in [5] above, wherein an aqueous solution containing the nickel source, the manganese source and the ammonium source is used as a raw aqueous solution, and the raw aqueous solution and the alkaline aqueous solution are introduced into the reaction tank liquid to obtain the precipitate.

[0023] [7] A method for producing a precursor as described in [6] above, wherein in the raw aqueous solution, the ratio of the ammonium-converted content of the ammonium source to the sum of the nickel-converted content of the nickel source and the manganese-converted content of the manganese source is greater than 0 and less than 1 in terms of molar ratio.

[0024] [8] The method for producing a precursor according to [6] or [7] above, wherein the pH of the raw material aqueous solution is 6 or less.

[0025] [9] The method for producing a precursor according to any one of [6] to [8] above, wherein the precipitate is dried at a temperature of 100° C. or less.

[0026]

[10] The method for producing a precursor according to any one of [6] to [9] above, wherein the precipitate is dried in a non-oxidizing atmosphere.

[0027]

[11] A positive electrode material used in a lithium-ion secondary battery, wherein the positive electrode material is a lithium-containing nickel-manganese composite oxide containing lithium, nickel and manganese, and is obtained using a precursor described in any one of [1] to [4] above.

[0028]

[12] A positive electrode material used in a lithium-ion secondary battery, wherein the positive electrode material is a lithium-containing nickel-manganese composite oxide containing lithium, nickel and manganese, and the content of the composite oxide represented by the formula Li2MnO3 is greater than 0 mass% and less than 20 mass%.

[0029]

[13] The positive electrode material as described in

[11] or

[12] above, further comprising at least one element A selected from the group consisting of aluminum, silicon, titanium, zirconium, calcium, potassium, barium, strontium and sulfur.

[0030]

[14] The positive electrode material as described in any one of

[11] to

[13] above, wherein the relative frequency distribution of the molar ratio of the manganese content to the nickel content has a central value of 0.85 or more and 1.20 or less and a half value width of 0.90 or less.

[0031]

[15] The positive electrode material as described in any one of

[11] to

[14] above, wherein the mass increase when left in an atmosphere at a temperature of 25° C. and a humidity of 60% for 240 hours is 0.75% by mass or less.

[0032]

[16] A method for producing a positive electrode material, which is a method for producing the positive electrode material described in any one of

[11] to

[15] above, wherein the precursor described in any one of [1] to [4] above is mixed with a lithium-containing compound, and the obtained mixture is fired to obtain a fired product.

[0033]

[17] A method for producing a positive electrode material as described in

[16] above, wherein the ratio of the lithium-converted content of the lithium-containing compound to the sum of the nickel-converted content of the precursor and the manganese-converted content of the precursor is greater than 1.03 and less than 1.10 in terms of molar ratio.

[0034]

[18] A method for producing a positive electrode material as described in

[16] or

[17] above, wherein the mixture is pre-fired at a temperature of not less than 400°C and not more than 700°C, and then the mixture is mainly fired at a temperature of not less than 800°C and not more than 1000°C to obtain the fired product.

[0035]

[19] The method for producing a positive electrode material according to any one of

[16] to

[18] above, wherein the fired product is washed with water.

[0036]

[20] A lithium ion secondary battery comprising a positive electrode containing the positive electrode material according to any one of

[11] to

[15] above, a negative electrode, and an ion conductive medium interposed between the positive electrode and the negative electrode and conducting lithium ions.

[0037] Effects of the Invention

[0038] According to the present invention, a lithium ion secondary battery having excellent discharge capacity and cycle characteristics can be obtained. DETAILED DESCRIPTION

[0039] [Precursor]

[0040] The precursor of the present invention is a precursor of a positive electrode material used in a lithium-ion secondary battery, and is at least one selected from the group consisting of a nickel-manganese composite hydroxide and a nickel-manganese composite oxide, containing nickel and manganese, the ratio of the nickel content to the total of the nickel content and the manganese content is greater than 0.45 and less than 0.60 in terms of molar ratio, and the average valence of manganese is less than 4.0.

[0041] The precursor of the present invention is used to obtain the positive electrode material (lithium-containing nickel-manganese composite hydroxide) described below. The lithium ion secondary battery using the obtained positive electrode material is excellent in discharge capacity and cycle characteristics. The reason is presumed to be as follows.

[0042] For example, when using a high-valence manganese (such as Mn 4+ ) precursor to produce a positive electrode material (lithium-containing nickel-manganese composite oxide), lithium (Li + ) and the precursor manganese (Mn 4+ ) has a strong repulsive force, and lithium cannot be uniformly diffused into the interior of the precursor. Therefore, the discharge capacity and cycle characteristics are reduced.

[0043] In contrast, the average valence of manganese in the precursor of the present invention is as low as less than 4.0. When such a precursor is used to manufacture a positive electrode material, the repulsive force between lithium and the manganese of the precursor is relatively small (lithium and the precursor react easily), and lithium is easily diffused evenly into the interior of the precursor. Therefore, the discharge capacity and cycle characteristics are excellent.

[0044] <Composition>

[0045] The precursor of the present invention contains nickel (Ni) and manganese (Mn).

[0046] In the precursor of the present invention, the ratio of the nickel content to the total of the nickel content and the manganese content (hereinafter sometimes expressed as "Ni / (Ni+Mn)") is 0.45 to 0.60, preferably 0.48 to 0.55. That is, the precursor of the present invention contains nickel and manganese in substantially the same ratio.

[0047] From the viewpoint of resource quantity and cost, the precursor of the present invention preferably does not contain cobalt (Co) substantially. Specifically, for example, the cobalt content in the precursor of the present invention is preferably 0.1 mass % or less, more preferably 0.01 mass % or less, and further preferably 0.001 mass % or less. The precursor of the present invention particularly preferably does not contain cobalt (does not contain cobalt at all).

[0048] The composition of the precursor (the content of the metal element) was determined by inductively coupled plasma (ICP) emission spectroscopy.

[0049] <Average valence of manganese>

[0050] As described above, the average valence of manganese in the precursor of the present invention is less than 4.0, and is preferably 3.8 or less, more preferably 3.5 or less, and further preferably 3.2 or less, because the discharge capacity and cycle characteristics are better.

[0051] On the other hand, the average valence of manganese in the precursor of the present invention is, for example, 2.5 or more, preferably 2.7 or more, and more preferably 2.9 or more.

[0052] The average valence of manganese (Mn) is determined by X-ray photoelectron spectroscopy (XPS).

[0053] Specifically, the precursor was subjected to narrow scan analysis under the following conditions using an XPS device (QuanteraSXM, manufactured by ULVAC-PHI) to obtain a photoelectron spectrum (also referred to as a "narrow spectrum") of the 3s orbital of manganese (Mn3s). The exchange cleavage width (ΔE) of the obtained narrow spectrum was measured.

[0054] Next, using MnO (valence: 2), Mn2O3 (valence: 3), and MnO2 (valence: 4) as standard substances, ΔE of each standard substance was measured in the same manner.

[0055] It is known that the narrow spectrum exchange splitting width (ΔE) of the 3s orbital of manganese changes depending on its valence.

[0056] A calibration curve was prepared from the ΔE of each standard substance, and the Mn valence of the precursor was determined from the prepared calibration curve and the ΔE of the precursor.

[0057] The ΔE measurement was performed three times for each precursor, and the average value of the three times was taken as the average valence of Mn of each precursor.

[0058] Primary excitation source conditions

[0059] Radiation source: X-ray monochromatic Al-Kα

[0060] Voltage: 15kV

[0061] Output power: 25kW

[0062] Beam diameter: 100μmφ

[0063] ·Analysis area: 100μmφ

[0064] Narrow scan analysis conditions

[0065] Mn3s Pass energy: 55eV

[0066] Step size: 0.1eV

[0067] From the perspective of easily obtaining the above-mentioned average valence of manganese (less than 4.0), the exchange cleavage width (ΔE) of Mn3s of the precursor of the present invention is preferably 4.9 eV or more, more preferably 5.0 eV or more.

[0068] On the other hand, the ΔE of Mn3s of the precursor of the present invention is preferably 5.7 eV or less, more preferably 5.5 eV or less.

[0069] <Average particle size of primary particles>

[0070] The precursor of the present invention preferably has a small average particle size (also referred to as "primary particle size") of primary particles. By using a precursor with a small primary particle size to manufacture a positive electrode material, the distance that lithium moves inside the precursor is short, and lithium is easily evenly diffused inside the precursor, resulting in better discharge capacity and cycle characteristics.

[0071] Specifically, the average particle size of the primary particles in the precursor of the present invention is preferably less than 0.6 μm, more preferably 0.1 μm or less. The lower limit is not particularly limited, but is, for example, 0.01 μm or more, preferably 0.03 μm or more.

[0072] The primary particle size (average particle size of primary particles) of the precursor is determined as follows.

[0073] First, the precursor is observed using a scanning electron microscope (SEM) to obtain a SEM image. More than 200 primary particles are randomly extracted from the obtained SEM image. Image analysis software is used to obtain the projected area equivalent circle diameter (the diameter of a circle with the same area as the particle on the SEM image) of the extracted primary particles. The number average diameter of the obtained diameter is used as the average particle size of the primary particles.

[0074] The precursor of the present invention is, for example, a spherical secondary particle formed by agglomeration of a plurality of primary particles. Examples of the shape of the primary particles include plate-like, needle-like, spherical, and rectangular parallelepiped shapes, and a plate-like shape is particularly preferred.

[0075] <Mass reduction>

[0076] The precursor of the present invention preferably has a large mass reduction (also simply referred to as "mass reduction" in this paragraph) when heated from room temperature to 1050°C in an air atmosphere.

[0077] The precursor with a large amount of mass reduction (selected from at least one of the group consisting of nickel-manganese composite hydroxide and nickel-manganese composite oxide) refers to a large amount of hydroxide. In the case of using a precursor with a large amount of hydroxide to manufacture a positive electrode material, the discharge capacity and cycle characteristics are better. Although the detailed reason is not clear, it is believed that this is because the crystal structure of the obtained positive electrode material (lithium-containing nickel-manganese composite oxide) can be appropriately adjusted by complexly configuring hydroxyl groups in the precursor.

[0078] Specifically, the mass reduction of the precursor of the present invention is preferably 16 mass % or more, more preferably 17 mass % or more, and even more preferably 19 mass % or more.

[0079] The upper limit is not particularly limited, but the mass reduction amount is, for example, 25 mass % or less, and preferably 22 mass % or less.

[0080] The mass reduction is determined by the heat reduction measurement described below.

[0081] First, 1 g of the sample (precursor) placed in a crucible was heated to 1050°C using an electric furnace and then naturally cooled. Next, the mass of the sample after natural cooling was measured. The mass loss was calculated from the difference between the mass of the sample before heating and the mass of the sample after heating.

[0082] <Peak intensity ratio>

[0083] The precursor of the present invention preferably has a peak intensity ratio of the peak intensity of the

[001] orientation to the peak intensity of the

[101] orientation in X-ray diffraction, that is, a

[001] /

[101] peak ratio that is small. The peak intensity of the

[001] orientation is the maximum peak intensity when the diffraction angle 2θ is in the range of 17 to 21°. The peak of the

[101] orientation is the maximum peak intensity when the diffraction angle 2θ is in the range of 30 to 40°. Hereinafter, the

[001] /

[101] peak ratio may be simply referred to as the "peak ratio".

[0084]

[001] /

[101] peak has a high tendency of amorphous property than a small precursor. Although the details are not clear, it is believed that the positive electrode material manufactured using the amorphous precursor is difficult to replace nickel at the lithium site. As a result, discharge capacity and cycle characteristics are more excellent. At this time, it is not only required that the amorphous property is high, but it is believed that the peak has an appropriate range.

[0085] Specifically, the

[001] /

[101] peak ratio of the precursor of the present invention is preferably 14 or less, more preferably 10 or less, more preferably 4.5 or less, particularly preferably 4 or less, and most preferably 3 or less.

[0086] The lower limit is not particularly limited, but the

[001] /

[101] peak ratio is, for example, 1 or more.

[0087] An X-ray diffraction apparatus (X-ray source: CuKα, tube voltage: 40 kV, tube current: 40 mA) was used to obtain an X-ray diffraction (XRD) pattern of the precursor, and the peak intensity ratio (

[001] /

[101] peak ratio) was calculated from the peak intensity of the

[001] orientation and the peak intensity of the

[101] orientation.

[0088] [Precursor production method]

[0089] Next, the method for producing the precursor of the present invention will be described.

[0090] The method for manufacturing the precursor of the present invention is a method for manufacturing the above-mentioned precursor of the present invention, wherein a nickel source, a manganese source, an ammonium source and an alkaline aqueous solution are introduced into a reaction tank liquid with a pH of greater than 9 and less than 12 to obtain a precipitate (at least one selected from the group consisting of a nickel-manganese composite hydroxide and a nickel-manganese composite oxide).

[0091] The obtained precipitate (more specifically, for example, the precipitate filtered out from the reaction tank liquid and dried) becomes the precursor of the present invention.

[0092] <Coprecipitation method>

[0093] The method for producing the precursor of the present invention is a so-called coprecipitation method. By using the coprecipitation method, nickel and manganese can be uniformly dispersed at the atomic level.

[0094] In the coprecipitation method of the present invention, it is preferred that an aqueous solution containing a nickel source, a manganese source and an ammonium source is used as a raw material aqueous solution, and the raw material aqueous solution and an alkaline aqueous solution are introduced into a reaction tank liquid to obtain a precipitate.

[0095] That is, instead of introducing the nickel source, the manganese source and the ammonium source separately into the reaction tank solution, it is preferred that the nickel source, the manganese source and the ammonium source are mixed in advance and then introduced into the reaction tank solution.

[0096] This can prevent the reaction of ammonium with the generated precipitate in the reaction tank liquid, and can easily suppress the excessive growth of primary particles.

[0097] In addition, it is believed that ammonium (NH4 + ) is coordinated with nickel ions and manganese ions and stabilized, which is also one of the reasons why the growth of primary particles can be inhibited.

[0098] In the raw material aqueous solution, the ratio of the ammonium-converted content of the ammonium source to the total content of the nickel-converted content of the nickel source and the manganese-converted content of the manganese source (hereinafter sometimes expressed as "NH4 / (Ni+Mn)") is preferably greater than 0 and less than 1 in terms of molar ratio, more preferably greater than 0.1 and less than 0.8, and further preferably greater than 0.2 and less than 0.6. It should be noted that in the raw material aqueous solution, the ratio of the nickel-converted content of the nickel source to the manganese-converted content of the manganese source (Ni / Mn) is preferably 1 / 1 in terms of molar ratio.

[0099] The pH of the raw material aqueous solution is preferably 6 or less, more preferably 5.5 or less, and further preferably 5 or less. The lower limit is not particularly limited, and the pH of the raw material aqueous solution is, for example, 3 or more, and preferably 4 or more.

[0100] Examples of the nickel source include nickel salts such as nickel sulfate, nickel carbonate, nickel nitrate, nickel acetate, and nickel chloride, and nickel sulfate (NiSO 4 ) is preferred.

[0101] Examples of the manganese source include manganese salts such as manganese sulfate, manganese carbonate, manganese nitrate, manganese acetate, and manganese chloride, and manganese sulfate (MnSO 4 ) is preferred.

[0102] Examples of the ammonium source include ammonium salts such as ammonium sulfate, ammonium chloride, ammonium nitrate, and ammonium carbonate, and ammonium sulfate ((NH 4 ) 2 SO 4 ) is preferred.

[0103] The nickel source, manganese source and ammonium source are preferably used in the form of aqueous solutions.

[0104] In each aqueous solution, the concentration (content) of the nickel source, the manganese source, and the ammonium source is preferably adjusted so as to achieve the above-mentioned molar ratio.

[0105] As the alkaline aqueous solution, a sodium hydroxide (NaOH) aqueous solution is preferred.

[0106] The reaction tank liquid is the liquid in the reaction tank, and as described above, has a pH of 9 or more and 12 or less. The reaction tank liquid is prepared by, for example, adding an alkaline aqueous solution such as an aqueous sodium hydroxide solution to pure water.

[0107] When obtaining a precipitate, it is preferred to stir the reaction tank liquid using a stirring rod or the like.

[0108] The temperature of the reaction tank liquid is preferably 30°C or higher and 60°C or lower, and more preferably 35°C or higher and 45°C or lower.

[0109] When the cathode material of the present invention described below contains the element A described below, a source of the element A may be further introduced into the reaction tank solution. The source of the element A is preferably contained in the raw material aqueous solution.

[0110] Examples of the element A source include salts of the element A such as sulfates, carbonates, nitrates, and acetates of the element A.

[0111] The amount of the element A source is appropriately adjusted depending on the desired composition.

[0112] <Drying of precipitate>

[0113] The precipitate obtained by the coprecipitation method is preferably filtered out from the reaction tank liquid (solid-liquid separation), washed with water, and then dried.

[0114] The temperature (drying temperature) when drying the precipitate is preferably low because oxidation due to the dehydration reaction of the precipitate is suppressed and the above-mentioned valence of manganese is easily obtained.

[0115] Specifically, the drying temperature is preferably 100° C. or lower, more preferably 90° C. or lower, further preferably 80° C. or lower, particularly preferably 70° C. or lower, and most preferably 60° C. or lower.

[0116] The lower limit is not particularly limited, but the drying temperature is, for example, 30° C. or higher, and preferably 40° C. or higher.

[0117] From the reason of suppressing oxidation of precipitate and reducing the valence of manganese easily, the atmosphere (drying atmosphere) when drying precipitate is preferably a non-oxidizing atmosphere. As the non-oxidizing atmosphere, for example, a non-oxidizing atmosphere with an oxygen concentration of 10 volume % or less can be cited, and as a specific example, a vacuum atmosphere (for example, 0.1 MPa or less) is preferably cited.

[0118] The time for drying the precipitate (drying time) is more preferably 5 hours or longer.

[0119] [Cathode material]

[0120] Next, the positive electrode material of the present invention is described. The positive electrode material is also called a positive electrode active material.

[0121] <First Method>

[0122] The positive electrode material (first embodiment) of the present invention is a positive electrode material used in a lithium ion secondary battery and is a lithium-containing nickel-manganese composite oxide containing lithium, nickel and manganese, and is obtained using the above-mentioned precursor of the present invention.

[0123] A lithium ion secondary battery using a positive electrode material obtained using the precursor of the present invention is excellent in discharge capacity and cycle characteristics.

[0124] <Method 2>

[0125] The positive electrode material (second embodiment) of the present invention is a positive electrode material used in a lithium-ion secondary battery, and is a lithium-containing nickel-manganese composite oxide, containing lithium, nickel and manganese, and the content of the composite oxide represented by the formula Li2MnO3 is greater than 0 mass % and less than 20 mass %. Here, the lithium-containing nickel-manganese composite oxide is preferably hexagonal.

[0126] Hereinafter, the "complex oxide represented by the formula Li2MnO3" will also be referred to as the "complex oxide of the second phase" or simply as the "second phase".

[0127] A lithium ion secondary battery using a positive electrode material having a second phase content of more than 0 mass % and 20 mass % or less is excellent in discharge capacity and cycle characteristics.

[0128] From the viewpoint of achieving better discharge capacity and cycle characteristics, the content of the second phase is preferably 2 mass % to 19 mass %, and more preferably 3 mass % to 17 mass %.

[0129] The content of the second phase in the positive electrode material is determined as follows.

[0130] First, an X-ray diffraction (XRD) pattern of the positive electrode material was obtained under the following conditions. Next, the obtained XRD pattern was subjected to Rietveld analysis using RIETAN-FP (curve: extended pseudo-Voigt function) and pattern fitting. In this way, the content of the second phase was determined.

[0131] ·Device name: Debye-Scherrer diffractometer BL5S2 (Aichi Synchrotron Radiation Center)

[0132] X-ray wavelength: 0.7

[0133] Detector: Two-dimensional semiconductor detector ピラタス

[0134] ·Measurement time: 10 minutes / sample

[0135] · Sample: Fill the sample in a Lindemann glass capillary (0.3 mm φ)

[0136] ·Measurement method: transmission method

[0137] ·Measurement temperature: room temperature

[0138] The composite oxide of the second phase is preferably a monoclinic composite oxide.

[0139] More specifically, in the positive electrode material (second embodiment) of the present invention, it is more preferable that a monoclinic composite oxide (a composite oxide of a second phase) is mixed as a different phase in a hexagonal composite oxide.

[0140] <Composition>

[0141] The positive electrode material (lithium-containing nickel-manganese composite oxide) of the present invention contains lithium (Li), nickel (Ni) and manganese (Mn).

[0142] By combining nickel and manganese, the atoms of each other undergo a disproportionation reaction. As a result, the free energy change ΔG before and after charge and discharge is large and the valence change of high-voltage Ni can be used for the charge and discharge reaction, and a high-voltage and high-capacity lithium-ion secondary battery can be obtained. In addition, a stable crystal structure is formed even in the charging state, so the obtained lithium-ion secondary battery has excellent cycle characteristics.

[0143] The positive electrode material of the present invention may further contain at least one element A selected from the group consisting of aluminum (Al), silicon (Si), titanium (Ti), zirconium (Zr), calcium (Ca), potassium (K), barium (Ba), strontium (Sr) and sulfur (S).

[0144] The positive electrode material (lithium-containing nickel-manganese composite oxide) of the present invention preferably contains a composite oxide represented by the following formula (1).

[0145] (1)Li a Ni x Mn 1-x A y O2

[0146] In formula (1), a is a number greater than 0.95 and less than 1.10, x is a number greater than 0.45 and less than 0.60, y is a number greater than 0 and less than 0.020, and A is at least one selected from the group consisting of Al, Si, Ti, Zr, Ca, K, Ba, Sr and S.

[0147] It should be noted that, when the positive electrode material of the present invention is the second embodiment described above, the composition of formula (1) is a composition containing a second phase (complex oxide represented by the formula Li2MnO3).

[0148] The composition of the positive electrode material was determined by inductively coupled plasma (ICP) emission spectroscopy.

[0149] <Median value and half width of relative frequency distribution of molar ratio (Mn / Ni)>

[0150] As described above, the positive electrode material of the present invention utilizes the disproportionation reaction of the atoms of manganese and nickel by combining them. In order to fully proceed with this reaction, it is preferred that the manganese atoms and the nickel atoms are adjacent to each other and uniformly distributed in the positive electrode material.

[0151] Therefore, in the relative frequency distribution of the molar ratio (Mn / Ni) of the manganese content to the nickel content of the positive electrode material of the present invention, the central value is preferably 0.85 or more and 1.20 or less, and the half width is 0.90 or less. The central value is more preferably 0.90 or more and 1.10 or less. The half width is more preferably 0.80 or less.

[0152] As a result, the obtained lithium ion secondary battery has a high voltage and is more excellent in discharge capacity and cycle characteristics.

[0153] The lower limit of the half width is not particularly limited, but the smaller the half width is, the more preferable it is.

[0154] The median value and half width of the relative frequency distribution of the molar ratio (Mn / Ni) of the positive electrode material were determined by observation using a transmission electron microscope (TEM) and energy dispersive X-ray analysis (EDX).

[0155] First, the powder of the positive electrode material is embedded in a resin and then thinned using a focused ion beam processing device to obtain a sample for TEM observation.

[0156] The obtained sample was observed using TEM (JEM-F200, manufactured by JEOL) (observation conditions: accelerating voltage 200 kV) to obtain a HAADF-STEM image.

[0157] The HAADF-STEM image was used for morphological observation, and EDX (analysis conditions: acceleration voltage 200 kV) and element mapping (image resolution: 1.96 nm / pixel) were performed using an apparatus attached to the TEM (Dual SDD, manufactured by JEOL).

[0158] From the obtained element mapping results, only the positive electrode material part is extracted to make the total content (molar amount) of Mn and Ni 100%, and a simple quantitative calculation is performed at each pixel. Divide the Mn content by the Ni content to calculate the molar ratio (Mn / Ni). The horizontal axis takes the molar ratio (Mn / Ni) ratio at 0.01 intervals, and the vertical axis takes the relative frequency to make a relative frequency distribution. For the produced relative frequency distribution, calculate the central value and half width.

[0159] <Mass increase>

[0160] The positive electrode material (lithium-containing nickel-manganese composite oxide) of the present invention preferably has a small mass increase (also simply referred to as "mass increase" in this paragraph) when left in an atmosphere at a temperature of 25° C. and a humidity of 60% for 240 hours.

[0161] It should be noted that, herein, the temperature "25° C." means "25±3° C.", and the humidity "60%" means "60±5%".

[0162] When the positive electrode material is left in the air, moisture and carbon dioxide in the air react with lithium in the positive electrode material or a lithium-containing compound remaining on the surface of the positive electrode material, and the mass of the positive electrode material may increase.

[0163] The small amount of mass increase when the positive electrode material is placed in the atmosphere means that the degradation caused by the reaction with moisture and carbon dioxide in the atmosphere is small. The degradation of the positive electrode material with a small amount of mass increase in the atmosphere is suppressed, and the handling property is excellent. In addition, the effect of suppressing the decomposition of the electrolyte is also excellent.

[0164] In addition, the smaller the mass increase of the positive electrode material when it is placed in the air atmosphere, the smaller the amount of lithium extracted from the positive electrode material due to the reaction with water and carbon dioxide. In this case, the reduction in charge and discharge capacity caused by the extraction of lithium from the positive electrode material is suppressed.

[0165] Specifically, the mass increase of the positive electrode material of the present invention is preferably 0.75 mass % or less, more preferably 0.70 mass % or less, more preferably 0.60 mass % or less, and particularly preferably 0.50 mass % or less.

[0166] The mass increase is calculated as follows. First, weigh a predetermined amount of the sample (positive electrode material) and place it in a sample bottle. Next, place the sample bottle containing the sample in a constant temperature and humidity chamber maintained at a temperature of 25°C and a humidity of 60% under an atmospheric atmosphere for 240 hours. The mass increase is calculated from the difference between the mass of the sample before placement and the mass of the sample after placement.

[0167] [Method for producing positive electrode material]

[0168] Next, a method for producing the positive electrode material of the present invention will be described.

[0169] The method for producing a positive electrode material of the present invention is a method for producing the positive electrode material of the present invention, comprising mixing the precursor of the present invention and a lithium-containing compound, and firing the obtained mixture to obtain a fired product.

[0170] The fired product (lithium-containing nickel-manganese composite oxide) is crushed as appropriate to obtain the positive electrode material of the present invention.

[0171] <Mixed>

[0172] The precursor of the present invention is mixed with a lithium-containing compound to obtain a mixture.

[0173] At this time, the ratio of the lithium-converted content of the lithium-containing compound to the sum of the nickel-converted content of the precursor and the manganese-converted content of the precursor (hereinafter sometimes expressed as "Li / (Ni+Mn)") is preferably greater than 1.03 and less than 1.10 in terms of molar ratio, and more preferably greater than 1.04 and less than 1.08.

[0174] When Li / (Ni+Mn) is within this range, the content of the second phase in the obtained positive electrode material of the present invention (second embodiment) is likely to be appropriate.

[0175] Examples of the lithium-containing compound include lithium hydroxide and lithium carbonate. Among them, lithium hydroxide is preferred because of its low reaction temperature.

[0176] When the obtained positive electrode material of the present invention contains the above-mentioned element A, a compound containing the element A (hereinafter also referred to as "A-containing compound") may be further mixed in the mixture.

[0177] Examples of the A-containing compound include hydroxides, oxides, chlorides, and salts (eg, sulfates, carbonates, nitrates, etc.) of element A, but are not limited thereto.

[0178] The amount of the compound containing A is appropriately adjusted depending on the desired composition.

[0179] <Firing>

[0180] The mixture obtained by mixing is fired to obtain a fired product.

[0181] At this time, it is preferred that the mixture be preliminarily fired at a temperature of 400° C. to 700° C., and then mainly fired at a temperature of 800° C. to 1000° C.

[0182] Under such sintering conditions, the content of the second phase in the obtained positive electrode material (second embodiment) of the present invention can easily become appropriate.

[0183] The main calcination temperature is more preferably 900° C. to 1000° C., and further preferably 925° C. to 975° C., because the content of the second phase can more easily become appropriate.

[0184] The atmosphere of pre-sintering is not particularly limited, and for example, oxidizing atmosphere (for example, atmospheric atmosphere, etc.), non-oxidizing atmosphere, etc. can be listed, wherein, non-oxidizing atmosphere is preferred. Non-oxidizing atmosphere can be listed, for example, non-oxidizing atmosphere (specifically, for example, nitrogen atmosphere, etc.) with oxygen concentration below 10 volume %. By pre-sintering under non-oxidizing atmosphere, the generation of low-activity nickel and / or manganese oxide is suppressed, and lithium is easily uniformly diffused in the sintered product.

[0185] The atmosphere of the main firing is not particularly limited, and examples thereof include an oxidizing atmosphere (for example, air atmosphere) and a non-oxidizing atmosphere.

[0186] The firing time is not particularly limited.

[0187] The calcination time of the preliminary calcination is preferably 6 hours to 48 hours, more preferably 12 hours to 36 hours.

[0188] The calcination time of the main calcination is preferably 5 hours to 30 hours, more preferably 10 hours to 25 hours.

[0189] <Water washing>

[0190] The burned product is preferably washed with water. Then, the washed burned product is appropriately dried to become a positive electrode material. By washing with water, the excess lithium that has not entered the interior of the obtained positive electrode material is washed away. Therefore, the amount of residual lithium in the charged state is reduced, and the above-mentioned mass increase is reduced.

[0191] It is preferred that the sintered product be sintered at 200° C. to 800° C. after washing and drying.

[0192] [Lithium-ion secondary battery]

[0193] The lithium ion secondary battery of the present invention comprises a positive electrode containing the positive electrode material of the present invention, a negative electrode, and an ion conductive medium interposed between the positive electrode and the negative electrode for conducting lithium ions.

[0194] The lithium ion secondary battery of the present invention is excellent in discharge capacity and cycle characteristics.

[0195] The ion-conducting medium is, for example, an electrolyte such as a non-aqueous electrolyte solution.

[0196] The lithium ion secondary battery of the present invention may further include a separator.

[0197] In addition, except for using the positive electrode material of the present invention, a conventionally known lithium ion secondary battery structure can be adopted.

[0198] Example

[0199] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to the following Examples.

[0200] <Precursor production>

[0201] Precursor No. 1 to Precursor No. 5 were produced as follows.

[0202] Precursor No.1

[0203] A raw material aqueous solution was obtained by mixing a 0.4 mol / L nickel sulfate (NiSO4) aqueous solution, a 0.4 mol / L manganese sulfate (MnSO4) aqueous solution, and a 0.2 mol / L ammonium sulfate ((NH4)2SO4) aqueous solution. The molar ratio (NH4 / (Ni+Mn)) in the raw material aqueous solution was 0.25. The pH of the raw material aqueous solution was 4.6.

[0204] 1 L of pure water and sodium hydroxide aqueous solution were added to the reaction tank to obtain a reaction tank solution adjusted to pH 11.

[0205] The raw material aqueous solution was added to the reaction tank liquid at a rate of 150 mL / hour. During the addition of the raw material aqueous solution, an alkaline aqueous solution (10% by mass sodium hydroxide aqueous solution) was added to the reaction tank liquid while being controlled so that the pH of the reaction tank liquid reached 11. Thus, a precipitate was obtained. At this time, the reaction tank liquid was stirred at 450 rpm using a stirring rod, and the temperature of the reaction tank liquid was controlled to 40°C.

[0206] The precipitate was filtered out and washed with water, and then dried in a vacuum atmosphere at 50° C. for 10 hours using a vacuum dryer.

[0207] In this way, Precursor No. 1 was obtained.

[0208] Precursor No.2

[0209] The drying atmosphere of the precipitate was set to the air atmosphere. Precursor No. 2 was obtained in the same manner as Precursor No. 1 except this point.

[0210] Precursor No.3

[0211] The raw aqueous solution was not mixed with an aqueous ammonium sulfate solution. The pH of the raw aqueous solution was 6.5. The raw aqueous solution and 0.06 mol / L of aqueous ammonia were added to the reaction tank solution at a rate of 150 mL / hour, respectively. During the addition of the raw aqueous solution and aqueous ammonia, an alkaline aqueous solution (a 10% by mass aqueous sodium hydroxide solution) was added to the reaction tank solution while being controlled so that the pH of the reaction tank solution reached 11. Thus, a precipitate was obtained.

[0212] Precursor No. 3 was obtained in the same manner as Precursor No. 1 except for these points.

[0213] Precursor No.4

[0214] The drying atmosphere of the precipitate was set to the air atmosphere and the drying temperature of the precipitate was set to 110°C.

[0215] Precursor No. 4 was obtained in the same manner as Precursor No. 1 except for these points.

[0216] Precursor No.5

[0217] The drying atmosphere of the precipitate was set to the air atmosphere and the drying temperature of the precipitate was set to 110°C.

[0218] Precursor No. 5 was obtained in the same manner as Precursor No. 3 except for these points.

[0219] <Characteristics of the precursor>

[0220] For the obtained precursors No. 1 to No. 5, the molar ratio (Ni / (Ni+Mn)), the exchange cleavage width (ΔE) of Mn3s, the average valence of Mn, the primary particle size, the mass reduction (the mass reduction when heated from room temperature to 1050° C. in an air atmosphere), and the

[001] /

[101] peak ratio were determined. The results are shown in Table 1 below.

[0221]

[0222] <Manufacturing of positive electrode material (first embodiment)>

[0223] Using the obtained Precursors No. 1 to No. 5, positive electrode materials No. 1 to No. 10 were produced in the following manner.

[0224] 《Positive Electrode Material No.1》

[0225] Precursor No. 1 is mixed with lithium hydroxide to obtain a mixture. The molar ratio (Li / (Ni+Mn)) during mixing is set to 1.05. The obtained mixture is calcined to obtain a calcined product. In more detail, the mixture is pre-calcined at 650° C. for 24 hours under a nitrogen atmosphere, and then mainly calcined at 950° C. for 15 hours under an air atmosphere. The obtained calcined product is crushed using a mortar. The calcined product is not washed with water. In this way, positive electrode material No. 1 is obtained.

[0226] 《Positive Electrode Material No.2~Positive Electrode Material No.5》

[0227] Precursor No. 2 to Precursor No. 5 were used respectively.

[0228] Except for this point, the same operation as that of positive electrode material No. 1 was carried out to obtain positive electrode materials No. 2 to No. 5, respectively.

[0229] 《Positive Electrode Material No.6~Positive Electrode Material No.10》

[0230] In the mixture, an Al-containing compound (aluminum nitrate), a Ti-containing compound (titanium nitrate), a Zr-containing compound (zirconium nitrate), a K-containing compound (potassium nitrate), and a Ba-containing compound (barium nitrate) are further mixed, respectively.

[0231] Except for this point, the same operation as that of positive electrode material No. 1 was carried out to obtain positive electrode materials No. 6 to No. 10, respectively.

[0232] <Characteristics and evaluation of positive electrode material (first embodiment)>

[0233] The composition, mass increase (mass increase after being left in an atmosphere of 25° C. and 60% humidity for 240 hours), discharge capacity and cycle characteristics of the obtained positive electrode materials No. 1 to No. 10 were determined. The results are shown in Table 2 below.

[0234] The discharge capacity and cycle characteristics were determined as follows (the same also applies to the second embodiment described later).

[0235] 《Discharge capacity》

[0236] N-methyl-2-pyrrolidone was added to the positive electrode material (90% by mass), acetylene black (5% by mass) and polyvinylidene fluoride (5% by mass), and kneaded to obtain a mixture. The obtained mixture was applied to an aluminum current collector with a thickness of 320 μm to form a coating. The laminate of the coating and the aluminum current collector was pressurized using a roller press with a gap set to 80 μm. A disc with a diameter of 14 mm was punched out from the pressurized laminate. The punched disc was vacuum dried at 150 ° C for 15 hours. The vacuum dried disc was used as the positive electrode.

[0237] A lithium metal sheet was used as the negative electrode, and a porous film made of polypropylene (Cell Guard #2400) was used as the separator.

[0238] One mole of LiPF6 was dissolved in 1 L of a mixed solution of ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio (EC / DMC) of 1 / 1 to obtain a non-aqueous electrolyte.

[0239] Using these positive electrodes, negative electrodes, separators and non-aqueous electrolytes, lithium ion secondary batteries (test batteries) were prepared in a glove box replaced with argon. Using the prepared test batteries, the current value was set to a constant value of 0.2C, and the voltage was charged and discharged in the range of 2.75 to 4.4V to obtain the discharge capacity [mAh / g].

[0240] 《Cyclic Characteristics》

[0241] The above charge and discharge were repeated 40 times (40 cycles) with the current value set to 0.5 C. The cycle characteristics were calculated from the obtained discharge capacity [mAh / g] using the following formula.

[0242] Cycle characteristics [%] = (discharge capacity at the 40th cycle / discharge capacity at the 1st cycle) × 100

[0243]

[0244] <Summary of evaluation results of positive electrode materials (first embodiment)>

[0245] As shown in Tables 1 and 2 above, positive electrode materials No. 1 to No. 3 and positive electrode materials No. 6 to No. 10 manufactured using precursors No. 1 to No. 3 having an average valence of Mn less than 4.0 have better discharge capacity and cycle characteristics than positive electrode materials No. 4 to No. 5 manufactured using precursors No. 4 to No. 5 having an average valence of Mn greater than 4.0.

[0246] <Manufacturing of positive electrode material (second embodiment)>

[0247] Using the obtained precursor No. 1, positive electrode materials No. 11 to No. 18 were produced in the following manner.

[0248] 《Positive Electrode Material No.11》

[0249] Precursor No. 1 is mixed with lithium hydroxide to obtain a mixture. The molar ratio (Li / (Ni+Mn)) during mixing is set to 1.05. The obtained mixture is calcined to obtain a calcined product. In more detail, the mixture is pre-calcined at 650° C. for 24 hours under a nitrogen atmosphere, and then mainly calcined at 1000° C. for 5 hours under an air atmosphere. The obtained calcined product is crushed using a mortar. The calcined product is not washed with water. In this way, positive electrode material No. 11 is obtained.

[0250] 《Positive Electrode Material No.12》

[0251] The firing temperature in the main firing was set to 900° C., and the firing time was set to 15 hours.

[0252] Positive electrode material No. 12 was obtained in the same manner as positive electrode material No. 11 except for these points.

[0253] 《Positive Electrode Material No.13》

[0254] The firing temperature in the main firing was set to 950° C., and the firing time was set to 10 hours.

[0255] Positive electrode material No. 13 was obtained in the same manner as positive electrode material No. 11 except for these points.

[0256] 《Positive Electrode Material No.14》

[0257] The firing temperature in the main firing was set to 950° C., and the firing time was set to 15 hours.

[0258] The burned product is washed with water and then dried.

[0259] Positive electrode material No. 14 was obtained in the same manner as positive electrode material No. 11 except for these points.

[0260] 《Positive Electrode Material No.15》

[0261] To the mixture was further mixed a S-containing compound (lithium sulfate).

[0262] The firing temperature in the main firing was set to 950° C., and the firing time was set to 15 hours.

[0263] Positive electrode material No. 15 was obtained in the same manner as positive electrode material No. 11 except for these points.

[0264] 《Positive Electrode Material No.16》

[0265] The molar ratio (Li / (Ni+Mn)) during mixing was set to 1.20.

[0266] The firing temperature in the main firing was set to 950° C., and the firing time was set to 10 hours.

[0267] Positive electrode material No. 16 was obtained in the same manner as positive electrode material No. 11 except for these points.

[0268] 《Positive Electrode Material No.17》

[0269] The firing temperature in the main firing was set to 780° C., and the firing time was set to 15 hours.

[0270] Positive electrode material No. 17 was obtained in the same manner as positive electrode material No. 11 except for these points.

[0271] 《Positive Electrode Material No.18》

[0272] The firing temperature in the main firing was set to 1080° C., and the firing time was set to 15 hours.

[0273] Positive electrode material No. 18 was obtained in the same manner as positive electrode material No. 11 except for these points.

[0274] <Characteristics and evaluation of positive electrode material (second embodiment)>

[0275] For the obtained positive electrode materials No. 11 to No. 18, the composition, the content of the second phase (Li2MnO3), the mass increase (the mass increase when placed in an atmosphere of temperature 25°C and humidity 60% for 240 hours), the discharge capacity and the cycle characteristics were determined. The results are shown in Table 3 below.

[0276]

[0277] <Summary of evaluation results of positive electrode material (second embodiment)>

[0278] As shown in Table 3 above, positive electrode materials No. 11 to No. 15 having a second phase (Li2MnO3) content greater than 0 mass % and less than 20 mass % have better discharge capacity and cycle characteristics than positive electrode materials No. 16 to No. 18 having a second phase (Li2MnO3) content of 0 mass % or greater than 20 mass %.

[0279] <Median value and half width of relative frequency distribution of molar ratio (Mn / Ni)>

[0280] The median value and half width of the relative frequency distribution of the molar ratio (Mn / Ni) were determined for positive electrode materials No. 1 to No. 3 and No. 11 according to the above method and are shown in Table 4 below together with the results of the discharge capacity and cycle characteristics.

[0281] [Table 4]

[0282]

[0283] As shown in Table 4, the relative frequency distribution of the molar ratio (Mn / Ni) of positive electrode materials No. 1 to No. 3 and No. 11 had a median value of 0.85 or more and 1.20 or less, and a half width of 0.90 or less.

[0284] At this time, positive electrode materials No. 1 and No. 2 having a median value of 0.90 or more and 1.10 or less had better discharge capacity and cycle characteristics than positive electrode materials No. 3 and No. 11 that did not satisfy this condition.

Claims

1. A precursor, which is a precursor of a positive electrode material used in a lithium ion secondary battery, wherein: The precursor is at least one selected from the group consisting of nickel-manganese composite hydroxides and nickel-manganese composite oxides, Contains nickel and manganese and does not contain cobalt, The ratio of the nickel content to the total of the nickel content and the manganese content is 0.45 or more and 0.60 or less in molar ratio, The average valence of manganese is less than 4.

0. The peak intensity ratio of the peak intensity of the [001] orientation to the peak intensity of the [101] orientation in X-ray diffraction, i.e., the [001] / [101] peak ratio, is 4.5 or less, The peak intensity of the [001] orientation is the maximum peak intensity when the diffraction angle 2θ is in the range of 17 to 21°, and the peak of the [101] orientation is the maximum peak intensity when the diffraction angle 2θ is in the range of 30 to 40°.

2. The precursor according to claim 1, wherein The average particle size of the primary particles is less than 0.6 μm.

3. The precursor according to claim 1 or 2, wherein The mass reduction when heated from room temperature to 1050° C. in an air atmosphere is 16 mass % or more.

4. A method for producing a precursor, which is a method for producing the precursor according to any one of claims 1 to 3, wherein: A nickel source, a manganese source, an ammonium source, and an alkaline aqueous solution are introduced into a reaction tank solution having a pH of 9 to 12 to obtain a precipitate.

5. The method for producing a precursor according to claim 4, wherein: An aqueous solution containing the nickel source, the manganese source and the ammonium source is used as a raw aqueous solution, The raw material aqueous solution and the alkaline aqueous solution are introduced into the reaction tank solution to obtain the precipitate.

6. The method for producing a precursor according to claim 5, wherein: In the raw material aqueous solution, the ratio of the ammonium-equivalent content of the ammonium source to the sum of the nickel-equivalent content of the nickel source and the manganese-equivalent content of the manganese source is greater than 0 and less than 1 in terms of molar ratio.

7. The method for producing a precursor according to claim 5 or 6, wherein: The pH of the raw aqueous solution is 6 or less.

8. The method for producing a precursor according to claim 5 or 6, wherein: The precipitate is dried at a temperature below 100°C.

9. The method for producing a precursor according to claim 5 or 6, wherein: The precipitate was dried under a non-oxidizing atmosphere.

10. A positive electrode material, which is a positive electrode material used in a lithium ion secondary battery, wherein: The positive electrode material is a lithium-containing nickel-manganese composite oxide. Contains lithium, nickel and manganese, It is obtained by using the precursor according to any one of claims 1 to 3.

11. The positive electrode material according to claim 10, wherein It further contains at least one element A selected from the group consisting of aluminum, silicon, titanium, zirconium, calcium, potassium, barium, strontium and sulfur.

12. The positive electrode material according to claim 10 or 11, wherein In the relative frequency distribution of the molar ratio of the manganese content to the nickel content, the median value is 0.85 or more and 1.20 or less, and the half value width is 0.90 or less.

13. The positive electrode material according to claim 10 or 11, wherein The mass increase when the composite was left in an atmosphere at a temperature of 25° C. and a humidity of 60% for 240 hours was 0.75% by mass or less.

14. A positive electrode material, which is a positive electrode material used in a lithium ion secondary battery, wherein: The positive electrode material is a lithium-containing nickel-manganese composite oxide. Contains lithium, nickel and manganese, The content of the composite oxide represented by the formula Li2MnO3 is greater than 0 mass % and less than 20 mass %, In the relative frequency distribution of the molar ratio of the manganese content to the nickel content, the median value is 0.85 or more and 1.20 or less, and the half value width is 0.90 or less.

15. The positive electrode material according to claim 14, wherein It further contains at least one element A selected from the group consisting of aluminum, silicon, titanium, zirconium, calcium, potassium, barium, strontium and sulfur.

16. The positive electrode material according to claim 14 or 15, wherein The mass increase when the composite was left in an atmosphere at a temperature of 25° C. and a humidity of 60% for 240 hours was 0.75% by mass or less.

17. A method for producing a positive electrode material, which is a method for producing the positive electrode material according to any one of claims 10 to 16, wherein: The precursor according to any one of claims 1 to 3 is mixed with a lithium-containing compound, and the obtained mixture is fired to obtain a fired product.

18. The method for producing a positive electrode material according to claim 17, wherein: The ratio of the lithium-equivalent content of the lithium-containing compound to the sum of the nickel-equivalent content of the precursor and the manganese-equivalent content of the precursor is greater than 1.03 and less than 1.10 in terms of molar ratio.

19. The method for producing a positive electrode material according to claim 17 or 18, wherein: The mixture is preliminarily fired at a temperature of 400° C. to 700° C., and then mainly fired at a temperature of 800° C. to 1000° C. to obtain the fired product.

20. The method for producing a positive electrode material according to claim 17 or 18, wherein: The burned product is washed with water. 21 . A lithium ion secondary battery comprising a positive electrode containing the positive electrode material according to claim 10 , a negative electrode, and an ion conductive medium interposed between the positive electrode and the negative electrode and conducting lithium ions.

Citation Information

Patent Citations

  • Positive electrode active material and non-aqueous electrolyte secondary battery using the same

    JP2002042813A

  • Positive electrode active material for lithium secondary battery, and use thereof

    CN102576871A

  • Positive electrode active material, lithium ion secondary battery positive electrode, and lithium ion secondary battery

    CN109075335A

  • Lithium nickel manganese oxide, its manufacturing method and lithium-ion secondary cell using the same

    JP2004002141A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery arranged by use thereof