Electrolytic copper foil capable of preventing tearing or wrinkling defects and method for producing the same, electrode including the electrolytic copper foil, and secondary battery including the electrode

By controlling the mechanical properties and surface characteristics of the electrolytic copper foil and combining with the use of the protective layer, the curling, wrinkling and tearing problems of extremely thin electrolytic copper foil in manufacturing and use are solved, and the capacity maintenance and stability of the secondary battery is improved. .

CN113661587BActive Publication Date: 2024-11-19SK NEXILIS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080027239.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-21
Filing Date
2020-11-13
Publication Date
2024-11-19
Estimated Expiration
2040-11-13

AI Technical Summary

Technical Problem

When manufacturing and using extremely thin electrolytic copper foils, curling, wrinkling or tearing is prone to occur, resulting in capacity maintenance and stability problems of secondary batteries, especially during roll-to-roll process and coating of active substances.

Method used

By controlling the valley average roughness (VMR), surface roughness, tensile strength and structural coefficient of the electrolytic copper foil, combined with the use of the protective layer, the mechanical properties and surface characteristics of the electrolytic copper foil are ensured, and curling, wrinkling and tearing are prevented. And improve the adhesion strength to the active material layer.

Benefits of technology

It is realized to prevent curling, wrinkle and tear in the manufacturing and use of thin electrolytic copper foil, extend the charging and discharge capacity retention time of the secondary battery, and improve the processability and capacity retention rate of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113661587B_ABST
    Figure CN113661587B_ABST
Patent Text Reader

Abstract

One embodiment of the present invention provides an electrolytic copper foil, comprising a copper layer, wherein the electrolytic copper foil has a valley mean roughness of 0.8 to 12.5, a structural coefficient of (220) surface [TC(220)] of 0.49 to 1.28, and a thermal conductivity of 25 to 51 kgf / mm 2 tensile strength and a width weight deviation of less than 3%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrolytic copper foil having optimized valley mean roughness (VMR) in order to prevent tearing or wrinkling defects, an electrode including the electrolytic copper foil, a secondary battery including the electrode, and a method for manufacturing the electrolytic copper foil. Background Art

[0002] Secondary batteries are a type of energy converter that converts electrical energy into chemical energy and stores it. When electricity is needed, the chemical energy is converted back into electrical energy to generate electricity. Secondary batteries are not only used in portable household appliances such as mobile phones and notebooks, but are also used as energy sources for electric vehicles. Since secondary batteries can be recharged repeatedly, they are also called rechargeable batteries.

[0003] As secondary batteries that are economical and environmentally friendly compared to disposable primary batteries, there are lead storage batteries, nickel-cadmium secondary batteries, nickel-hydrogen secondary batteries, lithium secondary batteries, and the like.

[0004] In particular, lithium secondary batteries can store a relatively large amount of energy relative to their size and weight compared to other secondary batteries. Therefore, lithium secondary batteries are preferred in the field of information and communication equipment that emphasizes portability and mobility, and their application range is also expanding to energy storage devices for hybrid vehicles and electric vehicles.

[0005] Lithium secondary batteries are repeatedly used with charge and discharge as a cycle. When a device is operated with a fully charged lithium secondary battery, the lithium ion secondary battery should have a higher charge / discharge capacity to increase the operating time of the device. Therefore, research is constantly needed to meet the growing needs of demanders for the charge / discharge capacity of lithium secondary batteries.

[0006] This secondary battery includes a negative electrode collector made of copper foil, and among the copper foils, electrolytic copper foil is widely used as the negative electrode collector of the secondary battery. As the demand for secondary batteries increases, the demand for secondary batteries with high capacity, high efficiency and high quality increases, and therefore, electrolytic copper foil capable of improving the characteristics of the secondary battery is needed. In particular, copper foil capable of ensuring high capacity and stable capacity retention of the secondary battery is needed.

[0007] The thinner the thickness of the electrolytic copper foil, the more active material can be contained in the same space, and the number of collectors can be increased, thereby increasing the capacity of the secondary battery. However, as the electrolytic copper foil becomes thinner, curling occurs, and when the electrolytic copper foil is rolled up, the edge portion curls, causing defects such as tearing or wrinkling of the electrolytic copper foil, so it is difficult to manufacture and use electrolytic copper foil in the form of very thin films. Therefore, in order to manufacture an electrolytic copper foil with a very thin thickness, it is necessary to prevent the curl of the electrolytic copper foil.

[0008] In addition, the electrolytic copper foil should not be curled, wrinkled or torn during the manufacturing process of the electrolytic copper foil and the manufacturing process of the secondary battery electrode or the secondary battery using the electrolytic copper foil. In particular, during the winding process of the electrolytic copper foil or the secondary battery electrode using the electrolytic copper foil in the roll-to-roll (RTR) process or the coating process of the active material, the edge tearing of the electrolytic copper foil should not occur. Summary of the invention

[0009] Problems to be solved by the invention

[0010] Therefore, the present invention relates to an electrolytic copper foil, an electrode including the electrolytic copper foil, a secondary battery including the electrode, and a method for manufacturing the electrolytic copper foil that can satisfy the limitations and requirements of the related art as described above.

[0011] An object of one embodiment of the present invention is to provide an electrolytic copper foil that does not curl, wrinkle or tear during the manufacturing process even if it has a thin thickness. In addition, an object of one embodiment of the present invention is to provide an electrolytic copper foil that does not curl, wrinkle or tear during the manufacturing process of a secondary battery electrode or a secondary battery using the electrolytic copper foil.

[0012] Another embodiment of the present invention aims to provide an electrode for a secondary battery including the electrolytic copper foil and a secondary battery including the electrode for a secondary battery.

[0013] Another embodiment of the present invention aims to provide a method for manufacturing an electrolytic copper foil that prevents curling, wrinkling, or tearing.

[0014] In addition to the above-mentioned modes of the present invention, other features and advantages of the present invention will be described below, or may be clearly understood by a person skilled in the art to which the present invention belongs through these descriptions.

[0015] Technical solutions to the problem

[0016] According to one embodiment of the present invention as described above, there is provided an electrolytic copper foil including a copper layer, wherein the electrolytic copper foil has a valley mean roughness of 0.8 to 12.5, a structural coefficient of (220) surface [TC(220)] of 0.49 to 1.28, and a relative humidity of 25 to 51 kgf / mm 2 and a width direction weight deviation of 3% or less, wherein the width direction weight deviation is calculated by the following formula 1, and the valley mean roughness is calculated by the following formula 2.

[0017] [Formula 1]

[0018] Weight deviation in width direction (%) = (weight standard deviation / weight arithmetic mean) × 100

[0019] [Formula 2]

[0020] Valley mean roughness (VMR) = [maximum valley depth of roughness profile (Rv)] / [surface roughness (Ra)]

[0021] The electrolytic copper foil may have a surface roughness of 2.5 μm or less.

[0022] The difference in surface roughness between the two surfaces of the electrolytic copper foil may be 0.65 μm or less.

[0023] The electrolytic copper foil may have a thickness of 4 to 30 μm.

[0024] The electrolytic copper foil may include a protective layer disposed on the copper layer.

[0025] The protective layer may include at least one of chromium (Cr), a silane compound, and a nitrogen compound.

[0026] According to another embodiment of the present invention, there is provided an electrode for a secondary battery, comprising an electrolytic copper foil; and an active material layer, arranged on the electrolytic copper foil, wherein the electrolytic copper foil comprises a copper layer, and the electrolytic copper foil has: a valley mean roughness of 0.8 to 12.5; a structural coefficient of (220) surface [TC(220)] of 0.49 to 1.28; and a surface roughness of 25 to 51 kgf / mm 2 and a width direction weight deviation of 3% or less, the width direction weight deviation is calculated by the following formula 1, the valley average roughness (Valley Mean Roughness) is calculated by the following formula 2.

[0027] [Formula 1]

[0028] Weight deviation in width direction (%) = (weight standard deviation / weight arithmetic mean) × 100

[0029] [Formula 2]

[0030] Valley mean roughness (VMR) = [maximum valley depth of roughness profile (Rv)] / [surface roughness (Ra)]

[0031] The electrolytic copper foil of the secondary battery electrode may have a surface roughness of 2.5 μm or less.

[0032] The difference in surface roughness between both surfaces of the electrolytic copper foil of the secondary battery electrode may be 0.65 μm or less.

[0033] The electrolytic copper foil of the secondary battery electrode may have a thickness of 4 to 30 μm.

[0034] The electrolytic copper foil for a secondary battery electrode may include a protective layer disposed on the copper layer.

[0035] The protective layer of the secondary battery electrode may include at least one of chromium (Cr), a silane compound, and a nitrogen compound.

[0036] The active material layer may include one or more active materials selected from the group consisting of carbon; metals of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; alloys containing the metals; oxides of the metals; and composites of the metals and carbon.

[0037] According to another embodiment of the present invention, a secondary battery is provided, characterized in that it includes: a positive electrode (cathode); a negative electrode (anode), which is composed of the electrode for the secondary battery; an electrolyte (electrolyte), which provides an environment for lithium ions to move between the positive electrode and the negative electrode; and a separator (separator), which electrically insulates the positive electrode and the negative electrode.

[0038] According to another embodiment of the present invention, a method for manufacturing an electrolytic copper foil is provided, comprising: a step of preparing an electrolyte; and a step of using the electrolyte to perform electroplating to form a copper layer, wherein the electrolyte comprises: 70 to 90 g / L of copper ions; 50 to 150 g / L of sulfuric acid; 5 to 45 mg / L of arsenic (As); 5 to 25 mg / L of acetamide; and 5 to 20 mg / L of polypropylene glycol (PPG), wherein the step of forming the copper layer comprises: applying 40 to 80 A / dm between an electrode plate and a rotating drum that are arranged in a manner separated from each other in the electrolyte. 2 The current density steps.

[0039] In the step of forming the copper layer, the electrolyte may be supplied at a flow rate deviation of 5% or less, and the flow rate deviation is calculated by the following Formula 4.

[0040] [Formula 4]

[0041] Electrolyte flow rate deviation per minute (%) = [(maximum flow rate per minute - minimum flow rate per minute) / average flow rate per minute] × 100

[0042] The method for manufacturing the electrolytic copper foil may further include: forming a protective layer on the copper layer.

[0043] The step of forming the protection layer may include the step of performing an anti-rust treatment on the surface of the copper layer using at least one of chromium (Cr), a silane compound, and a nitrogen compound.

[0044] The step of forming the protective layer may include the step of immersing the copper layer in a rust-proofing liquid including 0.5 to 1.5 g / L of chromium (Cr).

[0045] The general description of the present invention as above is only for illustrating and explaining the present invention, but not for limiting the scope of rights of the present invention.

[0046] Effects of the Invention

[0047] According to one embodiment of the present invention, curling, wrinkling or tearing of the electrolytic copper foil is prevented during the manufacturing process of the electrolytic copper foil. In addition, a long-life secondary battery that can maintain a high charge and discharge capacity for a long time even if the charge and discharge cycle is repeated can be manufactured. In addition, when using this electrolytic copper foil, curling, wrinkling or tearing of the electrolytic copper foil is prevented during the manufacturing process of the secondary battery electrode or the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] The accompanying drawings are used to help the understanding of the present invention and constitute a part of this specification. They illustrate embodiments of the present invention and, together with the detailed description of the invention, are used to explain the principles of the present invention.

[0049] Figure 1 This is a schematic cross-sectional view of an electrolytic copper foil according to an embodiment of the present invention.

[0050] Figure 2 This is an example of a roughness profile for explaining “maximum valley depth of roughness profile (Rv)” according to JIS B 0601:2001.

[0051] Figure 3 This is an example of an XRD spectrum of an electrolytic copper foil.

[0052] Figure 4 It is a schematic cross-sectional view of an electrolytic copper foil according to another embodiment of the present invention.

[0053] Figure 5 This is a schematic cross-sectional view of a secondary battery electrode according to still another embodiment of the present invention.

[0054] Figure 6 This is a schematic cross-sectional view of a secondary battery electrode according to still another embodiment of the present invention.

[0055] Figure 7 is a schematic cross-sectional view of a secondary battery according to still another embodiment of the present invention.

[0056] Figure 8 yes Figure 4 Schematic diagram of the copper foil manufacturing process is shown. DETAILED DESCRIPTION

[0057] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0058] It is obvious to those skilled in the art that various changes and modifications can be made to the present invention without exceeding the technical concept and scope of the present invention. Therefore, the present invention includes all changes and modifications within the scope of the invention described in the claims and their equivalents.

[0059] The shapes, sizes, ratios, angles, quantities, etc. disclosed in the accompanying drawings for illustrating the embodiments of the present invention are exemplary, and therefore, the present invention is not limited by the contents shown in the accompanying drawings. Throughout the specification, the same constituent elements may be represented by the same reference numerals.

[0060] When the words "including", "having", "consisting of", etc. are used in this specification, other parts may be added unless the expression "only" is used. When a constituent element is expressed in the singular, the plural number is included unless otherwise explicitly stated. Furthermore, when interpreting a constituent element, it is interpreted as including a tolerance range even if there is no separate explicit description.

[0061] When describing the positional relationship, for example, when describing the positional relationship of two parts by using "on ...", "upper ...", "lower ...", "beside ...", etc., one or more other parts may be provided between the two parts, unless the expression "directly" or "directly" is used.

[0062] When describing a temporal relationship, for example, when describing a temporal sequence using "afterwards", "subsequently", "next", "before", etc., discontinuous situations may also be included unless the expression "immediately" or "directly" is used.

[0063] In order to describe various components, expressions such as "first" and "second" are used, but these components are not limited by these terms. These terms are only used to distinguish one component from another component. Therefore, within the technical concept of the present invention, the first component mentioned below may be the second component.

[0064] The term "at least one" should be understood to include all combinations that can be given from more than one of the related items.

[0065] Each feature of each embodiment of the present invention may be partially or entirely combined or combined with each other, may be technically linked and driven in various ways, and each embodiment may be implemented independently of each other, or may be implemented together in an associated relationship.

[0066] Figure 1 1 is a schematic cross-sectional view of an electrolytic copper foil 101 according to an embodiment of the present invention.

[0067] like Figure 1 As shown, the electrolytic copper foil 101 of the present invention includes a copper layer 111. The copper layer 111 has a matte surface MS and a shiny surface SS opposite to the matte surface MS.

[0068] For example, the copper layer 111 may be formed on the rotating cathode roller by electroplating (see Figure 8 ). At this time, the smooth surface SS refers to the surface that has been in contact with the rotating cathode roller during the electroplating process, and the matte surface MS refers to the opposite surface of the smooth surface SS.

[0069] The electrolytic copper foil 101 has a first surface S1 as a surface in the matte surface MS direction and a second surface S2 as a surface in the smooth surface SS direction, based on the copper layer 111. Figure 1 The first surface S1 of the electrolytic copper foil 101 is the surface of the first protective layer 112a, and the second surface S2 is the smooth surface SS. According to an embodiment of the present invention, the first protective layer 112a may be omitted. In this case, the matte surface MS of the copper layer 111 becomes the first surface S1 of the electrolytic copper foil 101.

[0070] Generally, the second surface has a smaller surface roughness (Rz) than the first surface. However, one embodiment of the present invention is not limited thereto, and the surface roughness (Rz) of the second surface may be the same as the surface roughness (Rz) of the first surface, or greater than the surface roughness (Rz) of the first surface. For example, according to the rotating cathode roller 12 (refer to Figure 8) of the grinding degree, the surface roughness of the second surface can be less than or greater than the surface roughness (Rz) of the first surface. The surface of the rotating cathode drum 12 can be ground by a grinding brush having a grit of #800 to #3000.

[0071] Reference Figure 1 The electrolytic copper foil 101 includes a first protective layer 112a disposed on the matte surface MS of the copper layer 111. The first protective layer 112a may also be omitted.

[0072] The protective layer 112 may be disposed on at least one of the matte surface MS and the smooth surface SS of the copper layer 111. Figure 1 , the first protective layer 112a is disposed on the matte surface MS. However, an embodiment of the present invention is not limited thereto, and the first protective layer 112a may be disposed only on the smooth surface SS, or may be disposed on both the matte surface MS and the smooth surface SS.

[0073] The protective layer 112 can protect the copper layer 111 to prevent the copper layer 111 from being oxidized or deteriorated during storage or circulation. Therefore, the protective layer 112 is also called an anti-rust film.

[0074] According to an embodiment of the present invention, the protection layer 112 may include at least one of chromium (Cr), a silane compound, and a nitrogen compound.

[0075] For example, the protective layer 112 may be made of a rust-proof liquid containing chromium (Cr), that is, a rust-proof liquid containing a chromic acid compound.

[0076] The electrolytic copper foil 101 of the present invention can have a thermal conductivity of 25 to 51 kgf / mm at room temperature (25±15°C). 2 tensile strength.

[0077] The tensile strength is measured by using a universal testing machine (UTM), at which time the sample is heat treated at 135° C. for 10 minutes, at which the width of the sample is 12.7 mm, the distance between the grips is 50 mm, and the test speed is 50 mm / min.

[0078] If the tensile strength of the electrolytic copper foil 101 is less than 25 kgf / mm 2 , the electrolytic copper foil 101 is easily deformed by the force applied in the roll-to-roll process of the electrode manufacturing process and / or the secondary battery manufacturing process, and there is a risk of tearing and / or wrinkling. On the contrary, if the tensile strength of the electrolytic copper foil 101 exceeds 51kgf / mm 2 , as the electrolytic copper foil 101 is subjected to tension during the manufacturing process, the risk of tearing increases, and the workability of the secondary battery manufacturing process is reduced.

[0079] The width-direction weight deviation of the electrolytic copper foil 101 of the present invention may be 3% or less. The width-direction weight deviation may be obtained as follows.

[0080] First, samples with a size of 5 cm x 5 cm were taken from the left point, the center point, and the right point in the width direction of the electrolytic copper foil 101, and the weights of the three samples were measured. Then, the arithmetic mean and standard deviation of the measured values ​​were obtained, and the width direction weight deviation was calculated according to the following formula 1.

[0081] [Formula 1]

[0082] Weight deviation in width direction (%) = (weight standard deviation / weight arithmetic mean) × 100

[0083] If the weight deviation of the electrolytic copper foil 101 in the width direction exceeds 3%, wrinkles will occur at the portion where the weight deviation exceeds 3% in the roll-to-roll process of battery production, thereby increasing the defect rate.

[0084] On the other hand, according to one embodiment of the present invention, as the charge and discharge of the secondary battery are repeated, the active material layers 120a and 120b shrink and expand alternately, which causes the active material layers 120a and 120b to separate from the electrolytic copper foil 101, thereby reducing the capacity of the secondary battery. Therefore, in order to ensure that the electrode has a capacity retention rate and lifespan above a predetermined level (that is, in order to suppress the capacity reduction of the secondary battery), the electrolytic copper foil 101 should have excellent coating properties relative to the active material to improve the bonding strength between the electrolytic copper foil 101 and the active material layers 120a and 120b.

[0085] Generally, it is well known that the bonding strength between the electrolytic copper foil 101 and the active material layers 120a, 120b can be improved by controlling the surface roughness (Rz) of the electrolytic copper foil 101. The surface roughness (Rz) is also called the ten-point average roughness. The surface roughness (Rz) is determined as follows: the sum of the distances (absolute value) of the 5 farthest points upward from the center line of the sample interval in the surface roughness profile and the sum of the distances (absolute value) of the 5 farthest points downward are added and divided by 5. The surface roughness (Rz) can be measured using MahrsurfM300 roughness measuring instrument of Mahr according to JIS B 0601:2001 standard.

[0086] According to one embodiment of the present invention, the surface roughness (Rz1, Rz2) of the first surface S1 and the second surface S2 of the electrolytic copper foil 101 may be 2.5 μm or less. When the surface roughness (Rz1, Rz2) exceeds 2.5 μm, the first surface S1 and the second surface S2 of the electrolytic copper foil 101 are too uneven, resulting in a decrease in the uniformity of the coating of the negative electrode active material, thereby significantly reducing the bonding force between the electrolytic copper foil 101 and the first active material layer 120a and the second active material layer 120b.

[0087] According to one embodiment of the present invention, the difference (|Rz1-Rz2|) between the surface roughness (Rz1) of the first surface and the surface roughness (Rz2) of the second surface may be less than 0.65 μm. If the difference in surface roughness between the first surface and the second surface exceeds 0.65, the active material cannot be evenly coated on the first surface S1 and the second surface S2 due to the difference in surface roughness (Rz) between the first surface S1 and the second surface S2. As a result, during the charge and discharge of the secondary battery, the electrical and physical properties of the two surfaces S1 and S2 may differ, which may result in a reduction in the capacity retention rate and life of the secondary battery. For example, after the active material is applied, a difference in adhesion between the first active material layer 120a and the second active material layer 120b and the electrolytic copper foil 101 occurs on the first surface and the second surface. Therefore, this causes the electrode to bend in the direction of greater adhesion after the electrode is manufactured, thereby increasing the defective rate.

[0088] However, in reality, the electrolytic copper foil 101 with a properly adjusted surface roughness (Rz) (for example, adjusted to 2.5 μm or less) does not necessarily satisfy the adhesion between the electrolytic copper foil 101 and the active material layers 120a, 120b required in the specification. That is, the electrolytic copper foil 101 with a surface roughness (Rz) of less than 2.5 μm cannot always maintain the secondary battery capacity retention rate of more than 83% (after 500 charge and discharge cycles) required in the industry.

[0089] In particular, when the active material layers 120 a and 120 b contain Si to increase the capacity of the secondary battery, the correlation between the surface roughness (Rz) of the electrolytic copper foil 101 and the capacity retention rate of the secondary battery is lower.

[0090] According to one embodiment of the present invention, when the adhesion between the electrolytic copper foil 101 and the active material layers 120a, 120b is large enough to ensure a secondary battery capacity retention rate of more than 83%, it is found that the "Valley Mean Roughness (VMR)" of the electrolytic copper foil 101 is a more important factor than the surface roughness (Rz).

[0091] Below, refer to Figure 2The “valley mean roughness (VMR)” of the electrolytic copper foil 101 will be specifically described.

[0092] The “valley average roughness (VMR)” can be calculated by respectively measuring the “maximum valley depth (Rv) of the roughness profile” and the “surface roughness (Ra)” of the electrolytic copper foil 101, and calculating the measured values ​​of the “maximum valley depth (Rv) of the roughness profile” and the “surface roughness (Ra)” according to the following formula 2.

[0093] [Formula 2]

[0094] Valley mean roughness (VMR) = [maximum valley depth of roughness profile (Rv)] / [surface roughness (Ra)]

[0095] like Figure 2 As shown in FIG. 1 , the “maximum valley depth (Rv) of the roughness profile” defined in JIS B 0601:2001 standard refers to the depth from the mean line to the deepest valley in the surface roughness profile (sampling length: 4 mm).

[0096] The "surface roughness (Ra)" defined in the JIS B 0601:2001 standard is also referred to as arithmetic mean roughness. The surface roughness (Ra) is determined as a value obtained by finding the sum of the total area from the center line of the measurement interval (reference length) to the top and bottom in the surface roughness profile and dividing the sum by the length of the measurement interval.

[0097] The "maximum valley depth (Rv) of the roughness profile" and "surface roughness (Ra)" can be obtained by measuring the "maximum valley depth (Rv) of the roughness profile" and "surface roughness (Ra)" at any three points on the surface using a roughness measuring instrument of Mitutoyo according to JIS B 0601:2001 standard [sampling length: 4mm, radius of the stylus tip: 2μm, taper angle of the stylus tip: 60°, measuring force: 0.75mN], and then calculating their average values. The roughness profile is for the surface of the electrolytic copper foil.

[0098] According to an embodiment of the present invention, the valley mean roughness (VMR) of the roughness profiles of the first surface S1 and the second surface S2 is in a range of 0.8 to 12.5.

[0099] If the valley mean roughness (VMR) of the roughness profiles of the first surface S1 and the second surface S2 is less than 0.8, the copper foil may slip on the rollers during the roll-to-roll process for manufacturing the electrolytic copper foil 101 , causing uneven tension on the copper foil, thereby causing tearing.

[0100] On the contrary, if the valley mean roughness (VMR) of the roughness profiles of the first surface S1 and the second surface S2 exceeds 12.5, portions with high valley mean roughness (VMR) act as notches and may be torn during the secondary battery manufacturing process.

[0101] According to an embodiment of the present invention, the matte surface MS and the smooth surface SS of the copper layer 111 have crystal planes, and the structural coefficient [TC(220)] of the (220) plane of each of the matte surface MS and the smooth surface SS of the copper layer 111 is 0.49 to 1.28.

[0102] More specifically, the copper layer 111 has a plurality of crystal planes, which can be represented by Miller Index. Specifically, the crystal planes of the copper layer 111 can be represented by (hkl) planes. These crystal planes have texture coefficients (TC), respectively, and the texture coefficients (TC) of the crystal planes can be measured or calculated using X-ray diffraction (XRD).

[0103] Below, refer to Figure 3 , a method for measuring and calculating the structure coefficient (TC) of the crystal plane of the copper layer 111 constituting the electrolytic copper foil 101 is described.

[0104] Figure 3 is an example of an XRD spectrum of an electrolytic copper foil. More specifically, Figure 3 This is an XRD spectrum of the copper layer 111 constituting the electrolytic copper foil 101 . Figure 3 The peaks correspond to the crystal planes.

[0105] The structural coefficient [TC(220)] of the (220) surface can be calculated as follows.

[0106] An XRD pattern having peaks corresponding to n crystal planes was obtained by performing X-ray diffraction (XRD) in the diffraction angle (2θ) range of 30° to 95° [target: copper Kα1, 2θ spacing: 0.01°, 2θ scanning speed: 3° / min] [e.g. Figure 3The XRD spectrum of peaks (n=4) corresponding to the (111) plane, (200) plane, (220) plane and (311) plane shown in FIG] is obtained, and the XRD diffraction intensity [I(hkl)] of each crystal plane (hkl) is obtained from the spectrum. In addition, the XRD diffraction intensity [I0(hkl)] of each of the n crystal planes of the standard copper powder specified by JCPDS (Joint Committee on Powder Diffraction Standards) is obtained. Next, the arithmetic mean of I(hkl) / I0(hkl) of the n crystal planes is obtained, and then the structural coefficient [TC(220)] of the (220) plane is calculated by dividing I(220) / I0(220) of the (220) plane by the arithmetic mean. That is, the structural coefficient [TC(220)] of the (220) plane is calculated based on the following formula 3.

[0107] [Formula 3]

[0108]

[0109] As the structural coefficient [TC(220)] of the (220) surface increases, it indicates that the copper layer 111 has a denser crystal structure. The structural coefficient [TC(220)] of the (220) surface of each of the matte surface MS and the smooth surface SS is preferably greater than 0.49. If the structural coefficient [TC(220)] of the (220) surface is less than 0.49, the risk of tearing during the manufacturing process of the electrolytic copper foil 101 is high due to the loose crystal structure of the electrolytic copper foil 101. According to one embodiment of the present invention, the structural coefficient of the (220) surface of the matte surface MS or the smooth surface SS of the copper layer 111 is also referred to as the structural coefficient [TC(220)] of the (220) surface of the electrolytic copper foil 101. In addition, according to one embodiment of the present invention, the crystal structure of the copper layer 111 can also be referred to as the crystal structure of the electrolytic copper foil 101.

[0110] On the contrary, if the structural coefficient [TC(220)] of the (220) plane exceeds 1.28, the elongation is reduced to less than 3% due to the overly dense crystal structure of the copper layer 111, which is easy to tear during the manufacturing process. In addition, due to the lack of active area that enables the negative electrode active material to be stably contacted, sufficient adhesion cannot be ensured between the electrolytic copper foil 101 and the negative electrode active material. Therefore, when the secondary battery is charged and discharged, the electrolytic copper foil 101 does not expand and contract with the first active material layer 120a and the second active material layer 120b, thereby increasing the risk of the first active material layer 120a and the second active material layer 120b being separated from the electrolytic copper foil 101. As a result, the capacity retention rate of the secondary battery is reduced, resulting in the inability to manufacture a stable product.

[0111] According to an embodiment of the present invention, the electrolytic copper foil 101 may have a thickness of 4 to 30 μm.

[0112] When the electrolytic copper foil 101 is used as a collector of an electrode in a secondary battery, the thinner the thickness of the electrolytic copper foil 101, the more collectors can be accommodated in the same space, which is conducive to the high capacity of the secondary battery. However, when the thickness of the electrolytic copper foil 101 is less than 4 μm, the processability of the secondary battery electrode and the secondary battery using the electrolytic copper foil 101 is significantly reduced during the manufacturing process.

[0113] On the contrary, in the case where the thickness of the electrolytic copper foil 101 exceeds 30 μm, the thickness of the secondary battery electrode using the electrolytic copper foil 101 increases, and due to such thickness, it may be difficult to achieve a high capacity of the secondary battery.

[0114] Figure 4 1 is a schematic cross-sectional view of an electrolytic copper foil 102 according to another embodiment of the present invention. In order to avoid redundancy, the description of the components that have already been described will be omitted.

[0115] Reference Figure 4 In another embodiment of the present invention, an electrolytic copper foil 102 includes a copper layer 111 and a first protective layer 112a and a second protective layer 112b respectively disposed on a matte surface MS and a smooth surface SS of the copper layer 111. Figure 1 Compared with the electrolytic copper foil 101 shown, Figure 4 The illustrated electrolytic copper foil 102 further includes a protective layer 112 b disposed on the smooth surface SS of the copper layer 111 .

[0116] For convenience of description, of the two protective layers 112a and 112b, the protective layer 112a disposed on the matte surface MS of the copper layer 111 is referred to as a first protective layer, and the protective layer 112b disposed on the smooth surface SS is referred to as a second protective layer.

[0117] In addition, taking the copper layer 111 as a reference, Figure 4 The electrolytic copper foil 102 shown has a first surface S1 as a surface in the direction of the matte surface MS and a second surface S2 as a surface in the direction of the smooth surface SS. Here, the first surface S1 of the electrolytic copper foil 102 is the surface of the first protective layer 112a arranged on the matte surface MS, and the second surface S2 is the surface of the second protective layer 112b arranged on the smooth surface SS.

[0118] According to another embodiment of the present invention, the two protection layers 112 a and 112 b may respectively contain at least one of chromium (Cr), a silane compound, and a nitrogen compound.

[0119] Figure 4The roughness profiles of the first surface S1 and the second surface S2 of the electrolytic copper foil 102 shown have a valley mean roughness (VMR) of 0.8 to 12.5.

[0120] The structural coefficient [TC(220)] of the (220) plane of each of the matte surface MS and the smooth surface SS of the electrolytic copper foil 102 may be 0.49 to 1.28.

[0121] The electrolytic copper foil 102 can have a strength of 25 to 51 kgf / mm at room temperature (25±15°C). 2 tensile strength.

[0122] The weight deviation of the electrolytic copper foil 102 in the width direction may be 3% or less.

[0123] Figure 4 The surface roughness (Rz1, Rz2) of the first surface S1 and the second surface S2 of the electrolytic copper foil 102 shown may be 2.5 μm or less, and the difference (|Rz1-Rz2|) between the surface roughness (Rz1) of the first surface and the surface roughness (Rz2) of the second surface may be 0.65 μm or less.

[0124] Figure 4 The electrolytic copper foil 102 has a thickness of 4 to 30 μm.

[0125] Figure 5 1 is a schematic cross-sectional view of a secondary battery electrode 103 according to another embodiment of the present invention. Figure 5 The secondary battery electrode 103 shown can be applied to Figure 7 The secondary battery 105 is shown.

[0126] Reference Figure 5 A secondary battery electrode 103 according to another embodiment of the present invention includes an electrolytic copper foil 101 and an active material layer 120a disposed on the electrolytic copper foil 101. Here, the electrolytic copper foil 101 includes a copper layer 111 and a first protective layer 112a disposed on the copper layer 111, and serves as a current collector.

[0127] Specifically, the electrolytic copper foil 101 has a first surface S1 and a second surface S2, and the active material layer 120a is disposed on at least one of the first surface S1 and the second surface S2 of the electrolytic copper foil 101. The active material layer 120a may be disposed on the first protective layer 112a.

[0128] Figure 5 Shows the Figure 1 The electrolytic copper foil 101 is used as an example of a current collector. However, another embodiment of the present invention is not limited to this, and it is also possible to use Figure 4 The copper foil 102 shown is used as a current collector of an electrode 103 for a secondary battery.

[0129] In addition, although Figure 5 , the structure in which the first active material layer 120a is arranged only on the first surface S1 of the electrolytic copper foil 101 is shown, but another embodiment of the present invention is not limited thereto, and the first active material layer 120a and the second active material layer 120b may be arranged respectively on the first surface S1 and the second surface S2 of the electrolytic copper foil 101. In addition, the active material layer 120 may also be arranged only on the second surface S2 of the electrolytic copper foil 101.

[0130] Figure 5 The first active material layer 120a shown is made of an electrode active material, and in particular, can be made of a negative electrode active material. Figure 5 The secondary battery electrode 103 shown can be used as a negative electrode.

[0131] The active material layers 120a and 120b may include at least one of carbon, metal, metal-containing alloy, metal oxide, and a metal-carbon composite as a negative electrode active material. As the metal, at least one of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni, and Fe may be used. Specifically, the metal preferably includes silicon (Si) to increase the charge and discharge capacity of the secondary battery.

[0132] As the secondary battery is repeatedly charged and discharged, the active material layers 120a and 120b shrink and expand alternately, which causes the active material layers 120a and 120b to separate from the copper foil 101, thereby reducing the charge and discharge efficiency of the secondary battery. In particular, the active material layers 120a and 120b containing silicon (Si) expand and shrink to a greater extent.

[0133] According to another embodiment of the present invention, since the electrolytic copper foil 101 used as a current collector can shrink and expand corresponding to the shrinkage and expansion of the active material layers 120a and 120b, even if the active material layers 120a and 120b shrink and expand, the electrolytic copper foil 101 will not be deformed or torn. As a result, separation will not occur between the electrolytic copper foil 101 and the active material layer 120a. Therefore, the secondary battery including such a secondary battery electrode 103 has excellent charge and discharge efficiency and excellent capacity retention rate.

[0134] Figure 6 1 is a schematic cross-sectional view of a secondary battery electrode 104 according to still another embodiment of the present invention.

[0135] A secondary battery electrode 104 according to another embodiment of the present invention includes an electrolytic copper foil 102 and a first active material layer 120a and a second active material layer 120b disposed on the electrolytic copper foil 102. The electrolytic copper foil 102 includes a copper layer 111 and a first protective layer 112a and a second protective layer 112b disposed on both sides of the copper layer 111. However, one embodiment of the present invention is not limited thereto, and any one of the first active material layer 120a and the second active material layer 120b may be omitted.

[0136] Specifically, Figure 6 The secondary battery electrode 104 shown includes two first active material layers 120a and second active material layers 120b respectively arranged on the first surface S1 and the second surface S2 of the electrolytic copper foil 102. Here, the active material layer 120a arranged on the first surface S1 of the electrolytic copper foil 102 is referred to as the first active material layer, and the active material layer 120b arranged on the second surface S2 of the electrolytic copper foil 102 is referred to as the second active material layer.

[0137] The two first active material layers 120 a and the second active material layer 120 b may be made of the same material by the same method, or may be made of different materials or by different methods.

[0138] Figure 7 1 is a schematic cross-sectional view of a secondary battery 105 according to another embodiment of the present invention. For example, Figure 7 The secondary battery 105 shown is a lithium secondary battery.

[0139] Reference Figure 7 , the secondary battery 105 includes: a positive electrode (cathode) 370; a negative electrode (anode) 340; an electrolyte (electrolyte) 350, which is arranged between the positive electrode 370 and the negative electrode 340 to provide an environment in which ions can move; and a separator (separator) 360, which electrically insulates the positive electrode 370 and the negative electrode 340. Here, for example, the ions moving between the positive electrode 370 and the negative electrode 340 are lithium ions. The separator 360 separates the positive electrode 370 from the negative electrode 340 to prevent the charge generated at one electrode from moving to the other electrode through the interior of the secondary battery 105 and being consumed uselessly. Figure 7 , the separator 360 is disposed in the electrolyte 350 .

[0140] The positive electrode 370 includes a positive electrode current collector 371 and a positive electrode active material layer 372 . Aluminum foil can be used as the positive electrode current collector 371 .

[0141] The negative electrode 340 includes a negative electrode current collector 341 and a negative electrode active material layer 342 . Electrolytic copper foil can be used as the negative electrode current collector 341 .

[0142] According to one embodiment of the present invention, the negative electrode current collector 341 may be Figure 1 or Figure 4 The disclosed electrolytic copper foils 101 and 102. Figure 5 or Figure 6 The secondary battery electrodes 103 and 104 shown can be used as Figure 7 A negative electrode 340 of the secondary battery 105 is shown.

[0143] Below, refer to Figure 8 , a method for manufacturing the electrolytic copper foil 102 according to an embodiment of the present invention is specifically described.

[0144] Figure 8 yes Figure 4 Schematic diagram of a method for manufacturing an electrolytic copper foil 102 is shown.

[0145] The method for manufacturing the electrolytic copper foil 102 of the present invention includes: preparing an electrolytic solution 11 ; and performing electroplating using the electrolytic solution 11 to form a copper layer 111 .

[0146] Specifically, in the step of preparing the electrolytic solution 11 , the electrolytic solution 11 containing copper ions is first prepared. The electrolytic solution 11 is contained in the electrolytic tank 10 .

[0147] Next, in the step of electroplating the electrolytic solution 11 to form the copper layer 111, the electrolytic solution 11 is electroplated at 40 to 80 ASD (A / dm 2 ) current density is applied to the anode plate 13 and the rotating cathode roller 12 which are spaced apart from each other in the electrolyte 11 to perform electroplating, so that the copper layer 111 is formed on the rotating cathode roller 12. The copper layer 111 is formed by the principle of electroplating.

[0148] If the current density applied between the anode plate 13 and the rotating cathode roller 12 is less than 40 ASD, the grain formation of the copper layer 111 increases, and if it exceeds 80 ASD, the grain refinement is accelerated. More specifically, the current density can be adjusted to 50 ASD or more.

[0149] The surface properties of the smooth surface SS of the copper layer 111 may differ depending on the degree of polishing or grinding of the surface of the rotating cathode drum 12. To adjust the surface in the smooth surface SS direction, for example, the surface of the rotating cathode drum 12 may be ground with a grinding brush having a grit of #800 to #3000.

[0150] In the step of forming the copper layer 111, the electrolyte 11 is maintained at a temperature of 50 to 65°C, and the deviation of the flow rate of the supplied electrolyte 11 is maintained at less than 5% per minute. At this time, the physical, chemical and electrical properties of the copper layer 111 can be controlled by adjusting the composition of the electrolyte 11.

[0151] According to one embodiment of the present invention, the electrolyte 11 includes 70 to 90 g / L of copper ions, 50 to 150 g / L of sulfuric acid, 5 to 45 mg / L of arsenic (As), 5 to 25 mg / L of acetamide, and 5 to 20 mg / L of polypropylene glycol (PPG).

[0152] In order to smoothly form the copper layer 111 by copper electrodeposition, the copper ion concentration and the sulfuric acid concentration in the electrolyte 11 are adjusted to be in the range of 70 to 90 g / L and in the range of 50 to 150 g / L, respectively. More specifically, the sulfuric acid concentration in the electrolyte 11 is preferably adjusted to be 70 to 120 g / L.

[0153] In the electrolyte 11, the concentration of arsenic (As) is controlled within a range of 5 to 45 mg / L. However, an embodiment of the present invention is not limited thereto.

[0154] Arsenic acts as an accelerator for the reduction reaction of copper (Cu) in a certain concentration range. When the concentration of arsenic is less than 5 mg / L, in the process of forming the copper layer 111, the surface of the copper layer 111 is plated evenly, so that the valley average roughness (VMR) of the first side and the second side of the electrolytic copper foil 102 is less than 0.8.

[0155] On the contrary, when the concentration of arsenic exceeds 45 mg / L, the copper ion Cu 2+ Cu 1+ When reduced to copper (Cu), an insoluble compound is formed, and impurities may be electrodeposited (eutectoidally) together with the copper layer 111. Therefore, the copper layer 111 is plated in a powdery state, and the depth of the valley increases sharply, thereby the valley average roughness (VMR) of the first and second surfaces of the electrolytic copper foil 102 exceeds 12.5. In addition, when the concentration of arsenic is high, in the process of forming the copper layer 111, the (311) plane, the (111) plane, and the (100) plane can be preferentially grown based on the crystal plane, and the growth of the (220) plane can be suppressed.

[0156] Therefore, in the crystal structure of the copper layer 111, in order to make the structural coefficient [TC(220)] of the (220) plane within the range of 0.49 to 1.28, and to make the valley average roughness (VMR) of the first and second surfaces of the electrolytic copper foil 102 respectively within the range of 0.8 to 12.5, the arsenic concentration in the electrolyte 11 is adjusted to within 5 to 45 mg / L.

[0157] Acetamide is a substance added to the electrolyte 11 to control the size of copper-plated particles in the electrolyte 11. If the size of the copper-plated particles is too small, the tensile strength of the electrolytic copper foil 102 increases, and conversely, if the size of the copper-plated particles is too large, the tensile strength of the electrolytic copper foil 102 decreases.

[0158] The concentration of acetamide in the electrolyte 11 is controlled within a range of 5 to 25 mg / L. However, an embodiment of the present invention is not limited thereto.

[0159] When the concentration of acetamide exceeds 25 mg / L, the copper plating particles are plated ultrafinely, so that the tensile strength of the electrolytic copper foil 102 after heat treatment exceeds 51 kgf / mm 2 .

[0160] On the contrary, when the concentration of acetamide is less than 5 mg / L, the copper plating particles are coarsely plated, so that the tensile strength of the electrolytic copper foil 102 after heat treatment is less than 25 kgf / mm. 2 .

[0161] The polypropylene glycol (PPG) is a substance added to the electrolyte to control the crystal structure of plated copper.

[0162] The higher the concentration of polypropylene glycol (PPG) in the electrolyte, the denser the crystal structure of the electrolytic copper foil 102, thereby further increasing the structural coefficient of the (220) plane. The lower the concentration of polypropylene glycol (PPG) in the electrolyte, the less dense the crystal structure of the electrolytic copper foil 102, thereby further reducing the structural coefficient of the (220) plane.

[0163] According to the present invention, the concentration of polypropylene glycol (PPG) in the electrolyte is in the range of 5 to 20 mg / L.

[0164] If the concentration of polypropylene glycol (PPG) in the electrolyte is less than 5 mg / L, the crystal structure of the electrolytic copper foil 102 is not sufficiently developed, so that the structure coefficient of the (220) plane is less than 0.49. As described above, if the structure coefficient of the (220) plane is less than 0.49, the risk of tearing of the electrolytic copper foil 102 during the manufacturing process is relatively high due to the loose crystal structure of the electrolytic copper foil 102.

[0165] On the contrary, if the concentration of polypropylene glycol (PPG) in the electrolyte exceeds 20 mg / L, the crystal structure of the electrolytic copper foil 102 is too dense and the structural coefficient of the (220) plane exceeds 1.28. As described above, if the structural coefficient of the (220) plane exceeds 1.28, the elongation is reduced to less than 3%, which makes it easy to tear during the manufacturing process. In addition, due to the lack of active area that can stably contact the negative electrode active material, it is not possible to ensure sufficient bonding between the electrolytic copper foil 102 and the negative electrode active material.

[0166] In the step of forming the copper layer 111, the flow rate deviation of the supplied electrolyte 11 is kept below 5% per minute. The flow rate deviation of the supplied electrolyte 11 is used to adjust the weight deviation in the width direction of the electrolytic copper foil 102. The flow rate deviation can be obtained as follows.

[0167] First, the flow rate of the electrolyte 11 supplied within one minute is measured at least twice. The average flow rate per minute, the maximum flow rate per minute, and the minimum flow rate per minute are calculated using the measured flow rate per minute values, and then the deviation of the flow rate of the electrolyte supply can be calculated by the following formula 4.

[0168] [Formula 4]

[0169] Electrolyte flow rate deviation per minute (%) = [(maximum flow rate per minute - minimum flow rate per minute) / average flow rate per minute] × 100

[0170] In order to make the weight deviation of the electrolytic copper foil 102 in the width direction less than 3%, the deviation of the flow rate of the supplied electrolyte 11 is kept less than 5% per minute. If the deviation of the flow rate of the supplied electrolyte 11 exceeds 5%, the supply flow rate of the electrolyte 11 in the width direction of the electrolytic copper foil 102 will vary. As a result, a difference in efficiency occurs when copper is plated in the width direction, which causes the weight deviation of the electrolytic copper foil 102 to exceed 3%.

[0171] The copper layer 111 manufactured in the manner described above may be cleaned in the cleaning tank 20 .

[0172] For example, acid cleaning for removing impurities such as resin components and natural oxide on the surface of the copper layer 111 and water cleaning for removing the acid solution used in the acid cleaning may be performed in sequence. The cleaning step may also be omitted.

[0173] According to an embodiment of the present invention, the method may further include the step of forming a first protective layer 112 a and a second protective layer 112 b on the copper layer 111 .

[0174] In the step of forming the protective layer 112 , the first protective layer 112 a and the second protective layer 112 b are formed on the copper layer 111 manufactured in the manner described above.

[0175] Reference Figure 8 The copper layer 111 is immersed in the rust-proof liquid 31 contained in the rust-proof tank 30 to form a first protective layer 112 a and a second protective layer 112 b on the copper layer 111 .

[0176] The rust-proof liquid 31 may include at least one of chromium (Cr), a silane compound, and a nitrogen compound.

[0177] Specifically, the rust-proof liquid 31 of the copper layer 111 may include chromium (Cr), and the chromium (Cr) may exist in the rust-proof liquid 31 in an ion state.

[0178] The rust-proof liquid 31 may contain 0.5 to 1.5 g / L of chromium. To form the first protective layer 112a and the second protective layer 112b, the temperature of the rust-proof liquid 31 may be maintained at 20 to 40° C. The copper layer 111 may be immersed in the rust-proof liquid 31 for about 1 to 30 seconds.

[0179] Specifically, the manufactured copper layer 111 is immersed in a rust-proof liquid containing 0.5 to 1.5 g / L of chromium (Cr) (for example, for 2 to 20 seconds at room temperature) and then dried, thereby forming the first protective layer 112a and the second protective layer 112b on the copper layer 111, respectively.

[0180] The rust-proof liquid may further include at least one of a silane compound and a nitrogen compound. For example, the rust-proof liquid may include 0.5 to 1.5 g / L of chromium (Cr) and 0.5 to 1.5 g / L of a silane compound.

[0181] By forming such a protective layer 112 , the electrolytic copper foil 102 can be manufactured.

[0182] Then, the electrolytic copper foil 102 is cleaned in the cleaning tank 40. This cleaning step may be omitted.

[0183] Then, after a drying process is performed, the electrolytic copper foil 102 is wound up on a winder (WR).

[0184] The secondary battery electrode (ie, negative electrode) of the present invention can be manufactured by coating a negative electrode active material on the electrolytic copper foil 102 of the present invention manufactured as described above.

[0185] The negative electrode active material can be selected from the group consisting of carbon; a metal of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; an alloy containing the metal; an oxide of the metal; and a composite of the metal and carbon.

[0186] For example, 1 to 3 parts by weight of styrene-butadiene rubber (SBR) and 1 to 3 parts by weight of carboxymethyl cellulose (CMC) are mixed in 100 parts by weight of carbon for negative electrode active material, and then distilled water is used as a solvent to prepare a slurry. Next, the slurry is applied to the electrolytic copper foil 102 with a scraper at a thickness of 20 to 100 μm, and the slurry is heated at 110 to 130° C. at a temperature of 0.5 to 1.5 ton / cm 2 pressure.

[0187] A lithium secondary battery can be manufactured using a conventional positive electrode, electrolyte, and separator together with the secondary battery electrode (negative electrode) of the present invention manufactured by the above method.

[0188] Hereinafter, the present invention will be specifically described by way of examples and comparative examples. However, the following examples and comparative examples are only used to help understanding of the present invention, and the scope of rights of the present invention is not limited to the examples or comparative examples.

[0189] Examples 1 to 7 and Comparative Examples 1 to 7

[0190] The copper layer 111 was produced by electroplating a foil making machine including an anode plate 13 and a rotating cathode roller 12 arranged in a spaced relationship in an electrolyte 11, with current passing through at a current density of 60 ASD. The electrolyte 11 was a copper sulfate solution. The copper ion concentration in the electrolyte 11 was set to 75 g / L, the sulfuric acid concentration was set to 100 g / L, the electrolyte temperature was set to 55°C, and the current density was set to 60 ASD. During the electroplating, the plating solution was circulated at 42 m / s by a circulation pump. 3 / hr flow rate circulates between the supply tank and the plating tank, and fine impurities in the plating solution are removed by the cartridge filter between the supply tank and the plating tank.

[0191] In addition, the concentration of arsenic (As), the concentration of acetamide (Acetamide), and the concentration of polypropylene glycol (PPG) contained in the electrolyte 11 and the deviation of the flow rate of the electrolyte supplied during electroplating are shown in Table 1 below.

[0192] A current is applied between the rotating cathode roller 12 and the anode plate 13 at a current density of 50 ASD to produce a copper layer 111. Then, the copper layer 111 is immersed in a rust-proof liquid for 2 seconds to perform a chromate treatment on the surface of the copper layer 111 to form a first protective layer 112a and a second protective layer 112b, thereby producing an electrolytic copper foil 102. As the rust-proof liquid, a rust-proof liquid with chromic acid as a main component is used, and the concentration of chromic acid is 1.0 g / L. The copper layer formed by the electroplating is immersed in the rust-proof liquid and then dried to complete the electrolytic copper foil.

[0193] As a result, electrolytic copper foils of Examples 1 to 7 and Comparative Examples 1 to 7 were produced.

[0194] [Table 1]

[0195]

[0196] The electrolytic copper foils of Examples 1 to 7 and Comparative Examples 1 to 7 manufactured as described above were measured for (i) valley average roughness (VMR), (ii) tensile strength, (iii) structural coefficient of the (220) surface [TC(220)], (iv) weight deviation, and (v) surface roughness (Rz) of the first surface and the second surface.

[0197] In addition, after a secondary battery is manufactured using the electrolytic copper foil and the secondary battery is charged and discharged, (vi) the secondary battery is disassembled to observe whether the electrolytic copper foil is torn or wrinkled.

[0198] (i) Determination of valley mean roughness (VMR)

[0199] The "maximum valley depth (Rv) of the roughness profile" and "surface roughness (Ra)" are measured at three arbitrary points on the surface of the electrolytic copper foil using a roughness measuring instrument produced by Mitutoyo according to JIS B 0601:2001 [sampling length: 4 mm, radius of the stylus tip: 2 μm, taper angle of the stylus tip: 60°, measuring force: 0.75 mN], and then their average values ​​are calculated. The measured values ​​of the "maximum valley depth (Rv) of the roughness profile" and "surface roughness (Ra)" are calculated according to the following formula 2, thereby calculating the "valley average roughness (VMR)".

[0200] [Formula 2]

[0201] Valley mean roughness (VMR) = [maximum valley depth of roughness profile (Rv)] / [surface roughness (Ra)]

[0202] (ii) Determination of tensile strength

[0203] The tensile strength was measured using a universal testing machine (UTM) after heat treating the sample at 135° C. for 10 minutes. The width of the sample was 12.7 mm, the distance between the grips was 50 mm, and the measurement speed was 50 mm / min.

[0204] (iii) Determination of the structural coefficient of the (220) surface [TC(220)]

[0205] X-ray diffraction (XRD) was performed in the diffraction angle (2θ) range of 30° to 95° [target: copper Kα1, 2θ spacing: 0.01°, 2θ scanning speed: 3° / min], thereby obtaining an XRD spectrum having peaks corresponding to n crystal planes [e.g., Figure 3 The XRD spectrum of peaks (n=4) corresponding to the (111) plane, (200) plane, (220) plane and (311) plane shown in FIG] is obtained, and then the XRD diffraction intensity [I(hkl)] of each crystal plane (hkl) is obtained from the spectrum. In addition, the XRD diffraction intensity [I0(hkl)] of each of the n crystal planes of the standard copper powder specified by JCPDS (Joint Committee on Powder Diffraction Standards) is obtained. Next, the arithmetic mean of I(hkl) / I0(hkl) of the n crystal planes is obtained, and then the structural coefficient [TC(220)] of the (220) plane is calculated by dividing I(220) / I0(220) of the (220) plane by the arithmetic mean. That is, the structural coefficient [TC(220)] of the (220) plane is calculated based on the following formula 3.

[0206] [Formula 3]

[0207]

[0208] (iv) Determination of weight deviation in width direction

[0209] Samples of 5 cm x 5 cm in size were taken from the left, center and right points in the width direction of the electrolytic copper foil 102, and the weights of the three samples were measured. Then, the arithmetic mean and standard deviation of the measured values ​​were obtained, and the width direction weight deviation was calculated according to the following formula 1.

[0210] [Formula 1]

[0211] Weight deviation in width direction (%) = (weight standard deviation / weight arithmetic mean) × 100

[0212] (v) Surface roughness of the first and second surfaces (Rz1, Rz2) and their difference (|Rz1-Rz2|)

[0213] The surface roughness (Rz1, Rz2) of the first surface S1 and the second surface S2 of the electrolytic copper foil 102 manufactured in Examples 1 to 7 and Comparative Examples 1 to 7 was measured using a surface roughness measuring instrument (M300, Mahr) according to JIS B 0601-2001. Using the measurement results, the difference (|Rz1-Rz2|) in the surface roughness of the first surface S1 and the second surface S2 of the electrolytic copper foil was calculated.

[0214] (vi) Observe the occurrence of wrinkles and tears

[0215] 1) Anode manufacturing

[0216] 2 parts by weight of styrene-butadiene rubber (SBR) and 2 parts by weight of carboxymethyl cellulose (CMC) were mixed with 100 parts by weight of commercially available silicon / carbon composite negative electrode material for negative electrode active material, and distilled water was used as a solvent to prepare a slurry for negative electrode active material. The slurry for negative electrode active material was applied to the electrolytic copper foil of Examples 1 to 7 and Comparative Examples 1 to 7 with a width of 10 cm using a scraper at a thickness of 40 μm, dried at 120°C, and applied with 1 ton / cm 2 of pressure, thereby manufacturing a negative electrode for a secondary battery.

[0217] 2) Preparation of electrolyte

[0218] The base electrolyte was prepared by dissolving LiPF6 as a solute at a concentration of 1 M in a non-aqueous organic solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a ratio of 1:2. The non-aqueous electrolyte was prepared by mixing 99.5 wt % of the base electrolyte and 0.5 wt % of succinic anhydride.

[0219] 3) Cathode manufacturing

[0220] Lithium manganese oxide Li 1.1 Mn 1.85 Al 0.05 O4 and lithium manganese oxide o-LiMnO2 having an orthorhombic crystal structure are mixed in a ratio of 90:10 (weight ratio) to produce a positive electrode active material. The positive electrode active material, carbon black, and poly (vinylidene fluoride) [PVDF: Poly (vinylidene fluoride)] as a binder are mixed in a ratio of 85:10:5 (weight ratio), and mixed with NMP as an organic solvent to prepare a slurry. The slurry prepared as described above is applied to both sides of an Al foil having a thickness of 20 μm, and then dried to produce a positive electrode.

[0221] 4) Manufacturing of lithium secondary batteries for testing

[0222] A coin-shaped lithium secondary battery was manufactured by placing a positive electrode and a negative electrode in an insulated manner inside an aluminum can, and placing a nonaqueous electrolyte and a separator between them. The separator used was polypropylene (Celgard 2325; thickness: 25 μm, average pore size: φ28 nm, porosity: 40%).

[0223] 5) Charging and discharging of secondary batteries

[0224] The lithium secondary battery manufactured as described above was used to drive the battery at a charge voltage of 4.3 V and a discharge voltage of 3.4 V, and was charged / discharged 100 times at a high temperature of 50° C. and a current rate (C-rate) of 0.2.

[0225] 6) Whether wrinkles or tears occur

[0226] After 100 cycles of charge and discharge, the secondary battery was disassembled to observe whether wrinkles or tears occurred in the copper foil. The case where wrinkles or tears occurred in the copper foil was marked as "occurred", and the case where wrinkles or tears did not occur was marked as "none".

[0227] The above test results are shown in Table 2.

[0228] [Table 2]

[0229]

[0230] With reference to Tables 1 and 2, the following results can be confirmed.

[0231] The VMR of the electrolytic copper foil of Comparative Example 1 manufactured by an electrolyte containing a small amount of arsenic (As) was 0.7, which was less than the reference value, and tearing occurred. In addition, the VMR of the electrolytic copper foil of Comparative Example 2 manufactured by an electrolyte containing an excessive amount of arsenic (As) was 12.7, which was greater than the reference value, and the difference in surface roughness between the two surfaces (|Rz1-Rz2|) was 0.66, which was also greater than the reference value, and tearing occurred.

[0232] The electrolytic copper foil of Comparative Example 3 manufactured by an electrolyte containing a small amount of acetamide had a tensile strength less than the reference value and was torn. On the contrary, the electrolytic copper foil of Comparative Example 4 manufactured by an electrolyte containing an excessive amount of acetamide had a tensile strength greater than the reference value and was torn.

[0233] The structure coefficient [TC(220)] of the (220) surface of the electrolytic copper foil of Comparative Example 5 manufactured by an electrolyte containing a small amount of polypropylene glycol (PPG) was less than the reference value, and tearing occurred. On the contrary, the structure coefficient [TC(220)] of the (220) surface of the electrolytic copper foil of Comparative Example 6 manufactured by an electrolyte containing an excessive amount of polypropylene glycol (PPG) was greater than the reference value, and tearing occurred.

[0234] The electrolytic copper foil of Comparative Example 7, which was manufactured by supplying the electrolyte solution 11 with a high flow rate deviation of 5.3% per minute, had a weight deviation higher than the reference value, and wrinkles occurred but no tearing occurred.

[0235] On the other hand, in the copper foils of Examples 1 to 7 of the present invention, all numerical values ​​were within the range of the reference value, and wrinkles and tears were not generated in any of them.

[0236] The present invention described above is not limited to the aforementioned embodiments and drawings. It is obvious to those skilled in the art that various substitutions, deformations or changes can be made within the scope of the technical content of the present invention. Therefore, the scope of the present invention is expressed by the claims, and it should be interpreted that all changes or deformations derived from the meaning, scope and equivalent concepts of the claims are included in the scope of the present invention.

[0237] Description of Reference Numerals

[0238] 101, 102: Copper foil

[0239] 112a, 112b: first protective layer and second protective layer

[0240] 120a, 120b: first active material layer and second active material layer

[0241] 103, 104: Electrodes for secondary batteries

[0242] MS: rough surface

[0243] SS: Smooth

Claims

1. An electrolytic copper foil, wherein: Including copper layer, The electrolytic copper foil has: Valley average roughness of 0.8 to 12.5; The structural coefficient of the (220) surface [TC(220)] ranges from 0.49 to 1.28; 25 to 51 kgf / mm 2 tensile strength; and 3% or less weight deviation in width direction, The width direction weight deviation is calculated by the following formula 1: The valley average roughness is calculated by the following formula 2: The structural coefficient [TC(220)] of the (220) plane is calculated as follows: an XRD spectrum having peaks corresponding to n crystal planes is obtained by performing X-ray diffraction (XRD) within a diffraction angle (2θ) range of 30° to 95°, and the XRD diffraction intensity [I(hkl)] of each crystal plane (hkl) is obtained from the XRD spectrum; the XRD diffraction intensity [I0(hkl)] of each of the n crystal planes of the standard copper powder specified by the Joint Committee on Powder Diffraction Standards JCPDS is obtained; the arithmetic mean value of I(hkl) / I0(hkl) of the n crystal planes is obtained; and then the structural coefficient [TC(220)] of the (220) plane is calculated by the following formula 3 by dividing I(220) / I0(220) of the (220) plane by the arithmetic mean value. In the X-ray diffraction method, the target material is copper Kα1, the 2θ spacing is 0.01°, and the 2θ scanning speed is 3° / min. The n is 4: Formula 1 Weight deviation in width direction (%) = (weight standard deviation / weight arithmetic mean) × 100 Formula 2 Valley mean roughness (VMR) = [maximum valley depth of roughness profile (Rv)] / [surface roughness (Ra)] Formula 3 2. The electrolytic copper foil according to claim 1, wherein The surface roughness is less than 2.5 μm.

3. The electrolytic copper foil according to claim 1, wherein The difference in surface roughness between the two surfaces is 0.65 μm or less.

4. The electrolytic copper foil according to claim 1, wherein The thickness is 4 to 30 μm.

5. The electrolytic copper foil according to claim 1, wherein The invention comprises a protection layer disposed on the copper layer.

6. The electrolytic copper foil according to claim 5, wherein The protective layer contains at least one of chromium (Cr), a silane compound and a nitrogen compound.

7. An electrode for a secondary battery, wherein: include: Electrolytic copper foil; as well as The active material layer is arranged on the electrolytic copper foil. The electrolytic copper foil comprises a copper layer, The electrolytic copper foil has: Valley average roughness of 0.8 to 12.5; The structural coefficient of the (220) surface [TC(220)] ranges from 0.49 to 1.28; 25 to 51 kgf / mm 2 tensile strength; and 3% or less weight deviation in width direction, The width direction weight deviation is calculated by the following formula 1: The valley average roughness is calculated by the following formula 2: The structural coefficient [TC(220)] of the (220) plane is calculated as follows: an XRD spectrum having peaks corresponding to n crystal planes is obtained by performing X-ray diffraction (XRD) within a diffraction angle (2θ) range of 30° to 95°, and the XRD diffraction intensity [I(hkl)] of each crystal plane (hkl) is obtained from the XRD spectrum; the XRD diffraction intensity [I0(hkl)] of each of the n crystal planes of the standard copper powder specified by the Joint Committee on Powder Diffraction Standards JCPDS is obtained; the arithmetic mean value of I(hkl) / I0(hkl) of the n crystal planes is obtained; and then the structural coefficient [TC(220)] of the (220) plane is calculated by the following formula 3 by dividing I(220) / I0(220) of the (220) plane by the arithmetic mean value. In the X-ray diffraction method, the target material is copper Kα1, the 2θ spacing is 0.01°, and the 2θ scanning speed is 3° / min. The n is 4: Formula 1 Weight deviation in width direction (%) = (weight standard deviation / weight arithmetic mean) × 100 Formula 2 Valley mean roughness (VMR) = [maximum valley depth of roughness profile (Rv)] / [surface roughness (Ra)] [Formula 3] 8. The secondary battery electrode according to claim 7, wherein The electrolytic copper foil has a surface roughness of 2.5 μm or less.

9. The secondary battery electrode according to claim 7, wherein: The difference in surface roughness between both surfaces of the electrolytic copper foil is 0.65 μm or less.

10. The secondary battery electrode according to claim 7, wherein The electrolytic copper foil has a thickness of 4 to 30 μm.

11. The secondary battery electrode according to claim 7, wherein The electrolytic copper foil includes a protective layer disposed on the copper layer.

12. The secondary battery electrode according to claim 11, wherein The protective layer contains at least one of chromium (Cr), a silane compound and a nitrogen compound.

13. The secondary battery electrode according to claim 7, wherein: The active material layer contains one or more active materials selected from the group consisting of carbon; metals of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; alloys containing the metals; oxides of the metals; and composites of the metals and carbon.

14. A secondary battery, characterized in that: include: positive electrode; A negative electrode, comprising the electrode for a secondary battery according to any one of claims 7 to 13; an electrolyte providing an environment between the positive electrode and the negative electrode that enables lithium ions to move; as well as The separator electrically insulates the positive electrode from the negative electrode.

15. A method for producing an electrolytic copper foil, wherein: include: Steps for preparing electrolyte; as well as The step of using the electrolyte to perform electroplating to form a copper layer, The electrolyte comprises: 70 to 90 g / L of copper ions; 50 to 150 g / L sulfuric acid; 5 to 45 mg / L of arsenic; 5 to 25 mg / L acetamide; as well as 5 to 20 mg / L of polypropylene glycol PPG, The step of forming the copper layer includes applying 40 to 80 A / dm between the electrode plates and the rotating drum arranged in a manner separated from each other in the electrolyte. 2 The current density step, In the step of forming the copper layer, the electrolyte is supplied at a flow rate deviation of 5% or less per minute, The flow rate deviation per minute is calculated by the following formula 4: Formula 4 The electrolyte flow rate deviation per minute (%)=[(maximum flow rate per minute-minimum flow rate per minute) / average flow rate per minute]×100.

16. The method for producing an electrolytic copper foil according to claim 15, wherein: Also includes: The step of forming a protective layer on the copper layer.

17. The method for producing an electrolytic copper foil according to claim 16, wherein: The step of forming the protective layer includes the step of performing rust prevention treatment on the surface of the copper layer using at least one of chromium Cr, a silane compound, and a nitrogen compound.

18. The method for producing an electrolytic copper foil according to claim 16, wherein: The step of forming the protective layer includes: immersing the copper layer in a rust-proofing liquid containing 0.5 to 1.5 g / L of chromium (Cr).