Preparation method of monodisperse magnetic fluorescent microspheres
Through dispersion polymerization and seed swelling polymerization combined with dichloromethane swelling, monodispersed magnetic fluorescent microspheres with high uniformity and fluorescence stability were prepared, which solved the shortcomings of magnetic microsphere convenience and fluorescence stability in the existing swelling method, and achieved the goal of achieving the It effectively exerts the dual effects of magnetism and fluorescence.
Patent Information
- Application Number
- CN202111172419.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-10-08
AI Technical Summary
The existing swelling method can not take into account the convenience of preparing magnetic fluorescent microspheres and the stability of microsphere fluorescence, and fluorescent dyes are prone to leakage, and the scope of application is limited.
Monodispersed seed microspheres were prepared by dispersed polymerization method. Through seed swelling polymerization and dichloromethane as swelling agent, Fe3O4 nanoparticles were combined with porous green fluorescent microspheres to form monodispersed magnetic fluorescent microspheres to ensure the uniformity of the microspheres. and fluorescence stability.
The high uniformity, narrow particle size distribution, fluorescence stability and tolerance of magnetic fluorescence microspheres have been achieved, and the problem of fluorescence leakage in traditional methods has been overcome, which has enhanced the dual effects of magnetic and fluorescence of composite microspheres, and expanded the Application possibilities.
Smart Images

Figure CN113736451B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fluorescent microsphere preparation, and particularly relates to a method for preparing monodisperse magnetic fluorescent microspheres. Background Art
[0002] In current practical applications, single-function micro-nanospheres cannot cope with more complex application requirements and are inevitably subject to certain limitations. Multifunctional composite microspheres have more diversified properties than single microspheres, such as magnetic microspheres and fluorescent microspheres. In particular, dual-function fluorescent magnetic composite microspheres can move under an external magnetic field and use their fluorescent signals to achieve tracer labeling. They have become a research hotspot in the fields of biology, medicine, and environmental science, and have a wide range of applications in bioimaging, targeted drug delivery, biochemical detection, cell screening and separation, etc.
[0003] At present, there are many methods for preparing magnetic fluorescent microspheres, which can be summarized into two categories, namely one-step polymerization and step-by-step modification. The one-step polymerization method is a method of adding magnetic nano-sized particles and fluorescent substances to the microsphere synthesis monomer for one-step polymerization. Its advantage is that the operation process is relatively simple, but the presence of magnetic particles and fluorescent substances will break the balance of the original polymerization system, making the particle size of the microspheres produced after polymerization difficult to control, the distribution is wide, the morphology is poor, and the coating of magnetic particles and fluorescent substances is uneven and the content is low, thereby limiting its application. The step-by-step modification method mainly includes encapsulation method, layer-by-layer self-assembly method and swelling method, among which the encapsulation method usually uses ferroferric oxide magnetic spheres as the core, and then encapsulates the fluorescent substance in the shell to form a core-shell structure composite microsphere, and silica and polymers are often used as the preferred materials for the shell. However, the existence of the shell encapsulated by the encapsulation method has a certain degree of shielding effect, which in turn affects the fluorescence properties and magnetic responsiveness of the composite microspheres. The preparation of magnetic fluorescent microspheres by layer-by-layer self-assembly method mainly involves surface modification of magnetic nanoparticles and fluorescent particles to carry charges, and alternate adsorption on the surface of charged template microspheres through electrostatic action to form a functional coating. The layer-by-layer self-assembly method has fewer restrictions on the reaction substances and matrix materials, is highly adaptable, and has relatively mild reaction conditions, but has the disadvantages of relatively cumbersome operation and difficult process repeatability. The solvent swelling method refers to the microspheres being swollen by organic solvents such as chloroform. Usually, nano fluorescent quantum dots and magnetic materials are added to the dispersion system, and the solvent is evaporated to restore the microspheres to their initial structure, so that the nanoparticles enter the interior of the microspheres. The solvent swelling method has good reproducibility and low cost in preparing composite microspheres, and can maintain the regularity and monodispersity of the microspheres. However, the fluorescence of the microspheres is usually easily leaked in organic solvents after swelling, and the scope of application is limited. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing monodisperse magnetic fluorescent microspheres, the purpose of which is to solve the technical problem that the existing swelling method for preparing magnetic fluorescent microspheres cannot take into account both the convenience of preparing magnetic microspheres and the stability of the fluorescence of the microspheres.
[0005] The present invention provides a method for preparing monodisperse magnetic fluorescent microspheres, and the specific technical scheme is as follows:
[0006] The method for preparing monodisperse magnetic fluorescent microspheres comprises the following steps:
[0007] S1, preparation of green fluorescent dye using 4-chloro-7-nitro-2,1,3-benzoxadiazole and 4-aminostyrene;
[0008] S2, monodisperse seed microspheres were prepared by dispersion polymerization method;
[0009] S3, using the green fluorescent dye in step S1 and the polystyrene seed balls in step S2 to prepare monodisperse porous green fluorescent microspheres by seed swelling polymerization method;
[0010] S4, using Fe3O4 nanoparticles and the monodisperse porous green fluorescent microspheres in step S3 and using dichloromethane as a swelling agent to prepare monodisperse magnetic fluorescent microspheres.
[0011] In certain embodiments, in step S1, the green fluorescent dye biological preparation comprises the following steps:
[0012] S11, adding 4-aminostyrene and anhydrous ethanol to 4-chloro-7-nitro-2,1,3-benzoxadiazole, placing in a water bath at 40° C. under nitrogen and stirring for 24 hours to obtain a stirred mixture;
[0013] S12, removing unreacted materials from the stirred mixture in step S11 by rotary evaporation to obtain a rotary evaporation product;
[0014] S13, washing the rotary evaporation product in step S12 with ethyl acetate for chromatography to obtain a green fluorescent dye.
[0015] Furthermore, in step S11, the mass ratio of 4-chloro-7-nitro-2,1,3-benzoxadiazole, 4-aminostyrene and anhydrous ethanol is 5:3:100.
[0016] In some embodiments, in step S2, the preparation of polystyrene seed balls comprises the following steps:
[0017] S21, adding hydroxymethyl cellulose ether to a mixed solution of ethylene glycol methyl ether and ethanol, stirring thoroughly, and forming a transparent and clear solution at a constant temperature of 70° C., thereby obtaining a stirred mixed solution;
[0018] S22, adding styrene monomer to the stirred mixed solution in step S21, continuing stirring, introducing nitrogen, and reacting at a constant temperature of 70° C. for 24 hours to obtain a reaction solution;
[0019] S23, washing and drying the reaction solution in step S22 to obtain polystyrene seed microspheres, namely, monodisperse seed microspheres.
[0020] Furthermore, in step S21, the ratio of hydroxymethyl cellulose ether, ethylene glycol methyl ether and ethanol is 0.1:8:2-0.5:8:2; in step S22, the ratio of styrene monomer and stirred mixed liquid is 1:10-1:50; in step S23, the reaction liquid is centrifugally washed 3 times with ethanol, the drying temperature is 40°C, and the particle size of the polystyrene seed microspheres is 1-5 microns.
[0021] In certain embodiments, in step S3, the preparation of monodisperse porous green fluorescent microspheres comprises the following steps:
[0022] S31, dispersing polystyrene seed microspheres in pure water to form a polystyrene seed microsphere dispersion liquid, adding the same volume of 0.5 wt % sodium dodecyl sulfate solution to the polystyrene seed microsphere dispersion liquid, mixing evenly, and obtaining a dispersed mixed liquid;
[0023] S32, adding the dispersed mixed solution in step S31 to the green fluorescent monomer, styrene, divinylbenzene and porogen emulsion after ultrasound, and swelling for 24 hours to obtain a swelling solution;
[0024] S33, adding 10 wt % polyvinyl alcohol solution to the swelling solution in step S32, reacting at 70° C. for 24 hours to obtain a reaction product;
[0025] S34, washing and drying the reaction product in step S33 to obtain monodisperse porous green fluorescent microspheres.
[0026] Furthermore, the ratio of polystyrene to pure water is 1:10; in step S32, the addition amount of green fluorescent monomer, styrene, divinylbenzene and porogen emulsion accounts for 10wt% of the total weight; in step S33, the addition ratio of 10wt% polyvinyl alcohol solution accounts for 1wt% of the total weight; in step S34, the reaction product is centrifugally washed 3 times with ethanol, the drying temperature is 40°C, and the particle size of the monodisperse porous green fluorescent microspheres is 5-30 microns.
[0027] In certain embodiments, in step S3, the preparation of monodisperse magnetic fluorescent microspheres comprises the following steps:
[0028] S41, coating 10-20 nm Fe3O4 nanoparticles with oleic acid and dispersing them in dichloromethane to obtain a dispersion, adding the dispersion into a 0.5 wt% sodium dodecyl sulfate solution and performing ultrasonication to form an emulsion;
[0029] S42, dispersing monodisperse porous green fluorescent microspheres in a 0.5 wt % sodium dodecyl sulfate solution to obtain a dispersed suspension;
[0030] S43, adding the emulsion in step S41 to the dispersed suspension in step S42, swelling for 24 hours, to obtain a mixed solution;
[0031] S44, filtering the mixed solution in step S43, collecting the microspheres, washing and centrifuging, and collecting the monodisperse magnetic fluorescent microspheres.
[0032] Further, in step S41, the ratio of 0.5wt% sodium dodecyl sulfate solution to Fe3O4 nanoparticles; in step S42, the ratio of monodisperse porous green fluorescent microspheres to 0.5wt% sodium dodecyl sulfate solution; in step S43, the ratio of emulsion to dispersed suspension is; in step S44, the microspheres are washed at least 3 times with butanol and ethanol respectively, the centrifugal speed is 6000rpm, and the centrifugal time is 5 minutes.
[0033] The present invention has the following beneficial effects: the preparation method provided by the present invention improves the swelling method to obtain magnetic fluorescent microspheres having high uniformity, narrow particle size distribution, stable fluorescence, tolerance to organic solvents, and high stability, while the existing commercial magnetic fluorescent microspheres have low uniformity and problems such as easy leakage of fluorescent dyes. At the same time, the present invention can subsequently derive different functional groups on the surface of the microspheres, thereby enhancing the possibility of application in different fields. In addition, the present invention not only takes into account the convenience of preparing magnetic microspheres by the swelling method, but also ensures the stability of the fluorescence of the microspheres, overcomes some defects of the traditional preparation method, and maximizes the dual effects of the magnetism and fluorescence of the composite microspheres. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the preparation method of monodisperse magnetic fluorescent microspheres provided by the present invention;
[0035] Figure 2 is a fluorescence microscope image of monodisperse fluorescent magnetic microspheres in Example 1 of the present invention;
[0036] Figure 3 This is a state diagram of monodisperse fluorescent magnetic microspheres being attracted by a magnet under ultraviolet lamp excitation conditions in Example 1 of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the following is a detailed description of the present invention in conjunction with the accompanying drawings. Figure 1-3 , the present invention is further described in detail.
[0038] Example 1
[0039] The method for preparing monodisperse magnetic fluorescent microspheres provided in the present embodiment has the following specific technical scheme:
[0040] (1) Preparation of green fluorescent dye:
[0041] Add 1g 4-chloro-7-nitro-2,1,3-benzoxadiazole (NBD-Cl) to a three-necked flask, and then add 0.6g 4-aminostyrene and 20g anhydrous ethanol. Place the mixture in a 40°C water bath under nitrogen and stir for 24 hours. Rotary evaporate the unreacted material. Finally, purify the mixture by ethyl acetate washing chromatography, and the yield of the green fluorescent dye monomer is 0.5g.
[0042] (2) Preparation of monodisperse seed microspheres
[0043] The polystyrene seed balls were prepared by the dispersion polymerization method. 200 g of hydroxymethyl cellulose ether was added to a mixed solution of ethylene glycol methyl ether and ethanol. The ratio of hydroxymethyl cellulose ether, ethylene glycol methyl ether and ethanol was 0.5:8:2. After a transparent and clear solution was formed at 70°C, 20 g of styrene monomer was added. The speed was adjusted to 200 rpm, nitrogen was introduced, and the reaction was carried out at 70°C for 24 hours. The mixture was washed by centrifugation with ethanol for 3 times and dried at 40°C to obtain 3 μm polystyrene seed microspheres.
[0044] (3) Preparation of monodisperse porous green fluorescent microspheres
[0045] Using the seed swelling polymerization method, 1 gram of polystyrene seed balls prepared in step (2) were dispersed in 10 grams of pure water, and the same volume of 0.5 wt% sodium dodecyl sulfate solution was added. After mixing evenly, 20 grams of ultrasonically treated green fluorescent monomer, styrene, divinylbenzene and porogen emulsion were added. After swelling for 24 hours, 4 grams of 10 wt% polyvinyl alcohol solution were added. After mixing, the mixture was heated to 70°C and kept at this temperature for 24 hours. The mixture was washed three times by centrifugation with ethanol and dried at 40°C to obtain green fluorescent porous microspheres with a particle size of 10 microns.
[0046] (4) Preparation of monodisperse green fluorescent magnetic microspheres
[0047] First, 10-20 nm Fe3O4 nanoparticles are coated with oleic acid and dispersed in dichloromethane. Then, 1 gram of the dispersion is added to 20 g of 0.5 wt% sodium dodecyl sulfate solution for ultrasonication to form an emulsion. Finally, 5 g of the emulsion is added to 50 g of the porous fluorescent microspheres prepared in step (3) and dispersed in 0.5 wt% sodium dodecyl sulfate solution. The swelling is carried out at room temperature for 24 hours. After the swelling, the mixed solution is filtered, and the microspheres are washed with butanol and ethanol for more than 3 times to remove unbound magnetic particles, and 10 μm monodisperse green fluorescent magnetic microspheres are obtained by centrifugation at 6000 rpm for 5 minutes and then magnetic separation.
[0048] The monodisperse green fluorescent magnetic microspheres prepared by the method provided in this example show green fluorescence under a fluorescence microscope (eg Figure 2 As shown), Figure 3 As shown, the monodisperse magnetic fluorescent microspheres are excited to emit green fluorescence under UV light and are attracted by a magnet.
[0049] Example 2
[0050] The method for preparing monodisperse magnetic fluorescent microspheres provided in the present embodiment has the following specific technical scheme:
[0051] (1) Preparation of green fluorescent dye:
[0052] Add 1g 4-chloro-7-nitro-2,1,3-benzoxadiazole (NBD-Cl) to a three-necked flask, and then add 0.6g butylamine and 20g anhydrous ethanol. Place the mixture in a 40°C water bath under nitrogen and stir for 24 hours. Rotary evaporate the unreacted material. Finally, purify the mixture by ethyl acetate washing chromatography, and the yield of the green fluorescent dye monomer is 0.5g.
[0053] (2) Preparation of monodisperse seed microspheres
[0054] The polystyrene seed balls were prepared by the dispersion polymerization method. 200 g of hydroxymethyl cellulose ether was added to a mixed solution of ethylene glycol methyl ether and ethanol. The ratio of hydroxymethyl cellulose ether, ethylene glycol methyl ether and ethanol was 0.1:8:2. After a transparent and clear solution was formed at 70°C, 10 g of styrene monomer was added. The speed was adjusted to 200, nitrogen was introduced, and the reaction was carried out at 70°C for 24 hours. The mixture was washed by centrifugation with ethanol for 3 times and dried at 40°C to obtain 5 μm polystyrene seed microspheres.
[0055] (3) Preparation of monodisperse porous green fluorescent microspheres
[0056] Using the seed swelling polymerization method, 1 gram of polystyrene seed balls prepared in step (2) were dispersed in 10 grams of pure water, and the same volume of 0.5 wt% sodium dodecyl sulfate solution was added. After mixing evenly, 20 grams of ultrasonically treated green fluorescent monomer, styrene, divinylbenzene and porogen emulsion were added. After swelling for 24 hours, 4 grams of 10 wt% polyvinyl alcohol solution were added. After mixing, the mixture was heated to 70°C and kept at this temperature for 24 hours. The mixture was washed by centrifugation with ethanol for 3 times and dried at 40°C to obtain green fluorescent porous microspheres with a particle size of 20 microns.
[0057] (4) Preparation of monodisperse green fluorescent magnetic microspheres
[0058] First, 10-20 nm Fe3O4 nanoparticles are coated with oleic acid and dispersed in dichloromethane. Then, 1 gram of the dispersion is added to 20 g of 0.5 wt% sodium dodecyl sulfate solution for ultrasonication to form an emulsion. Finally, 5 g of the emulsion is added to 50 g of the porous fluorescent microspheres prepared in step (3) and dispersed in 0.5 wt% sodium dodecyl sulfate solution. The swelling is carried out at room temperature for 24 hours. After the swelling, the mixed solution is filtered, and the microspheres are washed with butanol and ethanol for more than 3 times to remove unbound magnetic particles, and 20 μm monodisperse green fluorescent magnetic microspheres are obtained by centrifugation at 6000 rpm for 5 minutes and then magnetic separation.
[0059] The monodisperse green fluorescent magnetic microspheres prepared by the method provided in this embodiment show green fluorescence under a fluorescence microscope and are attracted by a magnet under ultraviolet light excitation.
[0060] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. The present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. Preparation method of monodisperse magnetic fluorescent microspheres, It is characterized in that The steps include: S1, preparing a green fluorescent dye using 4-chloro-7-nitro-2,1,3-benzoxadiazole and 4-aminostyrene, comprising the following steps: S11, adding 4-aminostyrene and anhydrous ethanol to 4-chloro-7-nitro-2,1,3-benzoxadiazole, placing in a water bath at 40° C. under nitrogen and stirring for 24 hours to obtain a stirred mixture; S12, removing unreacted materials from the stirred mixture in step S11 by rotary evaporation to obtain a rotary evaporation product; S13, washing the rotary evaporation product in step S12 with ethyl acetate for chromatography to obtain a green fluorescent dye; S2, preparing monodisperse seed microspheres by dispersion polymerization method, comprising the following steps: S21, adding hydroxymethyl cellulose ether to a mixed solution of ethylene glycol methyl ether and ethanol, stirring thoroughly, and forming a transparent and clear solution at a constant temperature of 70° C., thereby obtaining a stirred mixed solution; S22, adding styrene monomer to the stirred mixed solution in step S21, continuing stirring, introducing nitrogen, and reacting at a constant temperature of 70° C. for 24 hours to obtain a reaction solution; S23, washing and drying the reaction solution in step S22 to obtain polystyrene seed microspheres, i.e., monodisperse seed microspheres; S3, using the green fluorescent dye in step S1 and the polystyrene seed balls in step S2 to prepare monodisperse porous green fluorescent microspheres by seed swelling polymerization method, comprising the following steps: S31, dispersing polystyrene seed microspheres in pure water to form a polystyrene seed microsphere dispersion liquid, adding the same volume of 0.5 wt % sodium dodecyl sulfate solution to the polystyrene seed microsphere dispersion liquid, mixing evenly, and obtaining a dispersed mixed liquid; S32, adding the dispersed mixed solution in step S31 to the green fluorescent monomer, styrene, divinylbenzene and porogen emulsion after ultrasound, and swelling for 24 hours to obtain a swelling solution; S33, adding 10 wt % polyvinyl alcohol solution to the swelling solution in step S32, reacting at 70° C. for 24 hours to obtain a reaction product; S34, washing and drying the reaction product in step S33 to obtain monodisperse porous green fluorescent microspheres; S4, using Fe 3 O 4 The monodisperse porous green fluorescent microspheres of the nanoparticles and step S4 are prepared by using dichloromethane as a swelling agent to prepare monodisperse magnetic fluorescent microspheres, comprising the following steps: S41, 10-20nm Fe 3 O 4 The nanoparticles were coated with oleic acid and dispersed in dichloromethane to obtain a dispersion, and the dispersion was added to a 0.5 wt % sodium dodecyl sulfate solution and subjected to ultrasonication to form an emulsion; S42, dispersing monodisperse porous green fluorescent microspheres in a 0.5 wt % sodium dodecyl sulfate solution to obtain a dispersed suspension; S43, adding the emulsion in step S41 to the dispersed suspension in step S42, swelling for 24 hours, and obtaining a mixed solution; S44, filtering the mixed solution in step S43, collecting the microspheres, washing and centrifuging, and collecting the monodisperse magnetic fluorescent microspheres.
2. The method for preparing monodisperse magnetic fluorescent microspheres according to claim 1, It is characterized in that In step S11, the mass ratio of 4-chloro-7-nitro-2,1,3-benzoxadiazole, 4-aminostyrene and anhydrous ethanol is 5:3:
100.
3. The method for preparing monodisperse magnetic fluorescent microspheres according to claim 1, It is characterized in that In step S21, the ratio of hydroxymethyl cellulose ether, ethylene glycol methyl ether and ethanol is 0.1:8:2-0.5:8:2; in step S22, the ratio of styrene monomer and stirred mixed liquid is 1:10-1:50; in step S23, the reaction liquid is centrifuged and washed 3 times with ethanol, the drying temperature is 40°C, and the particle size of the polystyrene seed microspheres is 1-5 microns.
4. The method for preparing monodisperse magnetic fluorescent microspheres according to claim 1, It is characterized in that In step S31, the ratio of polystyrene to pure water is 1:10; in step S32, the addition amount of green fluorescent monomer, styrene, divinylbenzene and porogen emulsion is 10wt% of the total weight; in step S33, the addition ratio of 10wt% polyvinyl alcohol solution is 1wt% of the total weight; in step S34, the reaction product is centrifugally washed 3 times with ethanol, the drying temperature is 40°C, and the particle size of the monodisperse porous green fluorescent microspheres is 5-30 microns.
5. The method for preparing monodisperse magnetic fluorescent microspheres according to claim 1, It is characterized in that In step S41, 0.5 wt% sodium dodecyl sulfate solution and Fe 3 O 4 The ratio of nanoparticles is 1:20; in step S42, the ratio of monodisperse porous green fluorescent microspheres to 0.5wt% sodium dodecyl sulfate solution is 1:50; in step S43, the ratio of emulsion to dispersed suspension is 1:10; in step S44, the microspheres are washed at least 3 times with butanol and ethanol respectively, the centrifugal speed is 6000rpm, and the centrifugal time is 5 minutes.