Anisotropic bonded magnet and preparation method thereof

By using preform stacking with different magnetic properties and densities and a warm-pressure magnetic field orientation molding process in the preparation of high aspect ratio magnets, the problem of non-uniform magnetic properties in the axial direction is solved and uniformity of density and performance is achieved. promote.

CN113744946BActive Publication Date: 2024-10-15GUOKE RE ADVANCED MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010476262.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-29
Publication Date
2024-10-15
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

In the preparation process of high aspect ratio magnets, existing technology is difficult to ensure the uniformity of magnetic properties in the axial direction, resulting in low density in the middle or high density at the periphery, affecting the performance and dimensional accuracy of the magnet.

Method used

Using a stacking method of multiple preformed blanks with different magnetic properties and/or densities, the density and magnetic properties of the magnets are adjusted through room temperature preforming and warm pressure magnetic field orientation molding processes, gradually decreasing from the middle to both ends or the outer periphery. Compensates for performance deviations caused by density differences.

Benefits of technology

It effectively improves the density uniformity and magnetic performance uniformity of the magnet along the pressing direction, and ensures the axial performance uniformity and dimensional accuracy of the magnet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113744946B_ABST
    Figure CN113744946B_ABST
Patent Text Reader

Abstract

An anisotropic bonded magnet and a preparation method thereof, by stacking magnets with different magnetic properties and / or densities, the magnet in the middle has high performance and the magnets at both ends and / or the periphery have low performance, thereby compensating for the performance deviation caused by the difference in pressing density during the pressing process and improving the performance uniformity of the magnet in the axial direction. This method solves the problem of "low in the middle and high on both sides" produced due to the magnetic field orientation and density unevenness in the height direction during the orientation densification process. The anisotropic bonded magnet prepared by this method has the characteristic of a density deviation of less than 2% along the pressing direction, which effectively improves the orientation degree and density of the magnet, as well as the uniformity of the magnetic properties and dimensional accuracy of the magnet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bonded magnet materials, and in particular to an anisotropic bonded magnet and a preparation method thereof. Background Art

[0002] Bonded permanent magnets have good processing properties, large shape freedom, high dimensional accuracy, and no need for secondary processing. They have become an indispensable component of modern high-tech products and are widely used in electronic information, computers, motors, automobiles, etc. Anisotropic bonded magnets have more excellent magnetic properties and can effectively promote the miniaturization, high efficiency, energy saving, and lightweight of electronic products, and have become the development direction of bonded permanent magnets.

[0003] The molding methods of bonded permanent magnets include compression molding, calendering molding, injection molding and extrusion molding. Among them, compression molding magnets are the most widely used due to their highest magnetic properties.

[0004] The basic process flow of preparing anisotropic bonded magnets by compression molding using thermosetting resin is as follows:

[0005] Magnetic powder is mixed with binder and additives to obtain composite magnetic powder → orientation pressing → demagnetization → curing → anti-corrosion treatment → performance testing, where additives refer to lubricants, coupling agents, etc.: binders generally use thermosetting resins such as epoxy resins and phenolic resins. The orientation forming process can be carried out in three ways: room temperature forming, warm pressing forming and multi-step forming. The preparation of anisotropic bonded magnets by room temperature forming has low magnetic properties due to the low density and poor orientation of the magnets. During the warm pressing forming process, the high temperature softens the binder and melts it into a viscous flow state. Its low viscosity plays a certain lubricating role, achieving the purpose of reducing the rotation resistance of the magnetic powder particles during orientation and the friction resistance between the magnetic powder and the mold wall, thereby effectively improving the orientation and density of the magnet. At present, warm pressing forming technology is widely used in the preparation of anisotropic bonded magnets. Therefore, improving the orientation and density is the key to preparing anisotropic bonded permanent magnets.

[0006] In the prior art, CN101599333A provides a method for manufacturing a dry-pressed anisotropic multipolar magnetic ring, which comprises wet-crushing magnetic powder, adding one or more adhesives and lubricants to the dried magnetic powder; then pre-pressing and pre-magnetizing, and then mixing with a high-speed crusher, and finally double-sided isostatic pressing of the aforementioned powder in a radial magnetic field.

[0007] CN101814368A provides a method for preparing anisotropic magnets: adjusting the powder particle size, wherein the first mixture is composed of a first magnetic powder with a particle size greater than 20μm and less than 150μm, a thermosetting resin with an addition amount of less than 2.0wt% in the anisotropic bonded magnet, and a first additive, and the second mixture is composed of a second magnetic powder with a particle size greater than 1μm and less than 20μm and a second additive, which is used to improve the density and magnetic properties of the magnet, but the magnetic field strength at the center of the magnet differs by more than 5% from that at the end.

[0008] CN103489621A provides a method for preparing a molded anisotropic bonded magnet, which adopts a two-step molding process, namely, room temperature preforming and orientation densification warm pressing molding process to prepare the anisotropic bonded magnet. During the orientation densification process, there will be a phenomenon of highly directional magnetic field orientation and uneven density, resulting in a phenomenon of low in the middle and high on both sides.

[0009] CN107393709A provides a method for preparing a highly oriented anisotropic bonded magnet by cold isostatic pressing, wherein a thermosetting resin and a curing agent are made into a binder, anisotropic bonded magnetic powder is added to the binder solution, and the mixture is fully stirred and then injected into a silicone mold, which is vacuum sealed and oriented in a 1.5T to 2T magnetic field, and then cold isostatic pressing is performed to prepare the magnet.

[0010] In industrial production, for magnetic rings with high aspect ratio, the existing technology of directly filling the high-temperature magnetic field cavity with magnetic powder will result in a high height of the magnetic powder in the cavity, which is easy to cause uneven magnetic field orientation along the height direction. In addition, the mixed magnetic powder is heated during high-temperature filling, which is easy to cause the magnetic powder to stick to the wall, making it difficult to ensure the uniformity of the filling, affecting the uniformity of the magnetic properties and dimensional accuracy of the magnet. Summary of the invention

[0011] The purpose of the present invention is to address the problem of uneven performance caused by low density in the middle in the axial direction and high density at both ends or at the periphery during the preparation of high aspect ratio magnets. A method of stacking multiple magnets is adopted, in which the performance in the middle is high and the performance at both ends or at the periphery is low, so as to compensate for the performance deviation caused by density difference during the pressing process and improve the uniformity of the performance of the magnet in the axial direction.

[0012] In order to achieve the above purpose, the present invention adopts the following scheme:

[0013] The first aspect of the present invention provides an anisotropic bonded magnet, comprising RTB permanent magnet powder, wherein R is selected from one or more rare earth elements, T is Fe or FeCo and a small amount of transition metal, and B is boron;

[0014] Among them, the content of R is 28-31wt.%, the content of B is 0.9-1.1wt.%, and the balance is T;

[0015] The anisotropic bonded magnet is formed by pressing a plurality of different preformed bodies, and the density deviation along the pressing direction is less than 2%.

[0016] Furthermore, the plurality of different preforms include preforms having different magnetic properties and / or densities.

[0017] Furthermore, R is one or more elements selected from Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu, preferably Nd or PrNd.

[0018] Furthermore, the bonded magnet is a bonded magnetic ring, the aspect ratio of the bonded magnetic ring is greater than 0.6, preferably 1.0-5.0, more preferably 1.2-2.5; the wall thickness is greater than 1 mm, preferably 1-20 mm, more preferably 1-5 mm.

[0019] A second aspect of the present invention provides a method for preparing anisotropic bonded magnets, comprising the following steps:

[0020] Step 1, preparing bonded magnet raw materials: the raw materials include RTB permanent magnet powder, thermosetting resin binder, coupling agent and lubricant; wherein the weight content of RTB permanent magnet powder is 100, the weight content of binder is 1.0% to 6.0% of RTB permanent magnet powder, preferably 2.5% to 3.5%, the weight content of coupling agent is 0.05% to 1.0% of RTB permanent magnet powder, preferably 0.1% to 0.3%, the weight content of lubricant is 0.05% to 2.0% of RTB permanent magnet powder, preferably 0.05% to 0.50%;

[0021] Step 2, mixing: uniformly mixing the RTB permanent magnetic powder in the raw material with the thermosetting resin binder, coupling agent and lubricant to obtain composite magnetic powder;

[0022] Step 3, preforming at room temperature: placing the dried composite magnetic powders with different magnetic properties in a first mold and placing them in a magnetic field H1 for press forming to obtain a variety of different preformed bodies, wherein the pressing pressure is 100-600 MPa, the magnetic field H1 is less than 0.15 T, and the pressing temperature is room temperature;

[0023] Step 4, warm-pressing magnetic field orientation molding: placing a plurality of different preformed bodies in a second mold and placing them in a magnetic field H2 for warm-pressing molding and orientation, and then pressing again; then demagnetizing, cooling, and demolding to obtain anisotropic bonded magnets that have been molded by warm-pressing magnetic field orientation; wherein the magnetic field intensity H2 is 0.6-3T, the pressing pressure is 300-1000MPa, and the molding temperature is 60-200°C;

[0024] Step 5, curing: heating the anisotropic bonded magnet formed by warm-pressing magnetic field orientation to a certain temperature and then keeping it warm, the warming temperature is 100-200° C., preferably 120-180° C.; the warming time is 0.5-2 hours.

[0025] Furthermore, the step 2 comprises:

[0026] The coupling agent measured in the above step is dissolved in the corresponding organic solvent, and then mixed evenly with the RTB permanent magnet powder. After the organic solvent is volatilized and removed, the coupling agent is evenly coated on the surface of the permanent magnet powder. Then the measured binder and lubricant are dissolved in the corresponding organic solvent, and mixed evenly with the RTB permanent magnet powder coated with the coupling agent. After the organic solvent is removed, the composite magnetic powder required for preparing the bonded magnet is obtained.

[0027] Furthermore, the plurality of different preforms include a first preform and a second preform; the first preform is made of composite magnetic powder with lower magnetic properties, and the second preform is made of composite magnetic powder with higher magnetic properties, wherein the ratio of the remanence Br of the RTB type permanent magnetic powder in the two types of composite magnetic powder is B 高 / B 低 =1.00~1.08.

[0028] Furthermore, the plurality of different preforms include a first preform and a second preform; the density of the first preform is less than the density of the second preform.

[0029] Furthermore, in step 4, stacking a plurality of different preforms into the second mold includes: a second preform in the middle, first preforms at both ends, and the length of the second preform in the middle is less than the length of the first preforms at both ends.

[0030] Furthermore, in step 4, stacking a plurality of different preforms into the second mold includes: the second preform in the middle and the first preform on the periphery.

[0031] Furthermore, stacking a plurality of different preforms into the second mold includes: the density and / or magnetic properties of the preforms arranged from the middle to the two ends gradually decrease; or the density and / or magnetic properties of the preforms arranged from the center to the periphery gradually decrease.

[0032] Furthermore, in step 4, the gap ratio between the preformed body and the warm-pressing magnetic field orientation forming die is 0.5% to 40%, preferably 3.5% to 25%.

[0033] Furthermore, the first preformed body and the second preformed body are magnetic cylinders or magnetic rings of the same shape, and the number ratio of the first preformed body to the second preformed body is 1:1 to 10:1.

[0034] In summary, the present invention provides an anisotropic bonded magnet and a method for preparing the same. By stacking magnets with different magnetic properties and / or densities, the magnet in the middle has high performance and the magnets at both ends and / or the periphery have low performance, thereby compensating for the performance deviation caused by density differences during the pressing process and improving the performance uniformity of the magnet in the axial direction. This method solves the problem of highly directional magnetic field orientation and uneven density during the orientation and densification process, as well as the problem of low in the middle and high on both sides. The anisotropic bonded magnet prepared by this method has the characteristic of a density deviation of less than 2% along the pressing direction, which effectively improves the orientation degree and density of the magnet, as well as the uniformity and dimensional accuracy of the magnetic properties of the magnet. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic flow chart of a method for preparing anisotropic bonded magnets according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0037] The first aspect of the present invention provides an anisotropic rare earth bonded magnet. The bonded magnet comprises RTB permanent magnet powder prepared by the HDDR method, wherein R is one or more rare earth elements including Y, T is Fe or FeCo and a small amount of transition metal, wherein the content of R is 28-31wt.%, the content of B is 0.9-1.1wt.%, and the balance is T; the anisotropic bonded magnet is formed by pressing a plurality of different preformed bodies, the bonded magnet has an aspect ratio greater than 0.6, a wall thickness greater than 1mm, and a density deviation of the bonded magnetic ring along the pressing direction is less than 2%.

[0038] Further, the plurality of different preforms include preforms having different magnetic properties and / or densities.

[0039] Furthermore, the rare earth element R constituting the RTB permanent magnet powder of the present invention can be one or more selected from Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu. From the perspective of cost and magnetic properties, Nd or PrNd is preferably used.

[0040] Furthermore, the element T constituting the RTB rare earth magnet powder of the present invention is Fe or FeCo. The T amount of the average composition of the powder is the remainder excluding other elements constituting the powder. In addition, the Curie temperature can be increased by adding Co as an element replacing Fe, but too much will cause the residual magnetic flux density of the powder to decrease. Adding transition elements as elements replacing Fe can increase the residual magnetic flux density Br, but too much will passivate the hydrogenation reaction in the HDDR process and affect the magnetic properties.

[0041] Furthermore, the bonded magnet can have various shapes. The following is a further explanation using a bonded magnetic ring as an example, but it is not limited to a bonded magnetic ring. The density of the bonded magnetic ring determines its magnetic properties. For a magnetic ring with a length-to-diameter ratio, the pressing process of the magnetic ring determines that the axial density will have deviations. The density deviation will cause the magnetic ring to have uneven axial magnetic properties, thereby affecting the output stability of the motor after the magnetic ring is assembled. The density deviation of the bonded magnetic ring of the present invention along the pressing direction is less than 2%, which fully guarantees the performance uniformity of the magnetic ring and the output stability of the motor after assembly. The bonded magnetic ring constituting the present invention has an aspect ratio greater than 0.6, preferably 1.0 to 10, and more preferably 2 to 8, because for a magnetic ring with a small aspect ratio (less than 0.6), the density deviation in the pressing direction is small, which can be accomplished in the prior art. If the aspect ratio of the magnetic ring is too large (greater than 10), it will bring greater difficulties to the molding of the magnetic ring and the subsequent equipment process.

[0042] Furthermore, the wall thickness of the bonded magnetic ring constituting the present invention is greater than 1 mm, preferably 1 to 20 mm, and more preferably 1 to 5 mm. If the wall thickness of the magnetic ring is too thin (less than 1 mm), the preparation process of the magnetic ring is difficult and it is easy to be damaged; if the wall thickness of the magnetic ring is too thick (greater than 20 mm), the bonding strength is too weak due to the lack of radial compression. Too thick a wall thickness is not conducive to the overall molding of the magnetic ring. At the same time, too thick a wall thickness does not conform to the trend of lightweighting, which limits its assembly process and application areas.

[0043] The second aspect of the present invention provides a method for preparing anisotropic bonded magnets, which is used to make the above-mentioned anisotropic bonded magnets. A method for preparing anisotropic bonded magnetic rings (hereinafter, the anisotropic bonded magnets in the present invention take magnetic rings as specific embodiments, but are not limited to magnetic ring structures) using a two-step molding process, namely room temperature preforming and oriented warm pressing molding, wherein the room temperature preforming process prepares several pre-pressed magnetic rings with different properties, and in the oriented warm pressing process, multiple pre-pressed magnetic rings are stacked and pressed, wherein the magnetic ring in the middle has high performance and the performance of the two sides is low. Specifically, the following process is included, such as Figure 1 As shown:

[0044] Step 1: Prepare the raw materials for bonding magnetic rings:

[0045] The raw materials of bonded magnetic rings are RTB permanent magnet powder, thermosetting resin binder, coupling agent and lubricant.

[0046] The rare earth element R constituting the RTB permanent magnet powder of the present invention can be selected from one or more of Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu. In view of cost and magnetic properties, Nd or PrNd is preferably used. The element T constituting the RTB rare earth magnet powder is Fe or FeCo; the thermosetting resin binder is a thermosetting resin such as epoxy resin and phenolic resin; the coupling agent is a silane coupling agent, titanate, etc. The lubricant is paraffin, stearate, silicone oil, etc.

[0047] Taking the weight content of RTB permanent magnet powder as 100, the weight content of binder is 1.0% to 6.0% of the RTB permanent magnet powder, preferably 2.5% to 3.5%; the weight content of coupling agent is 0.05% to 1.0% of the RTB permanent magnet powder, preferably 0.1% to 0.3%; the weight content of lubricant is 0.05% to 2.0% of the RTB permanent magnet powder, preferably 0.05% to 0.50%.

[0048] Step 2, mixing: uniformly mixing the RTB permanent magnetic powder in the raw material with the thermosetting resin binder, coupling agent and lubricant to obtain composite magnetic powder.

[0049] Specifically, the coupling agent measured in the above step is dissolved in the corresponding organic solvent, and then mixed evenly with the RTB permanent magnet powder. After the organic solvent is evaporated and removed, the coupling agent is evenly coated on the surface of the anisotropic magnetic powder. Subsequently, the measured binder and lubricant are dissolved in the corresponding solvent, and then mixed evenly with the RTB permanent magnet powder coated with the coupling agent. After the organic solvent is removed, the composite magnetic powder used to prepare the bonded magnet can be obtained.

[0050] Produce a variety of composite magnetic powders with different magnetic properties and / or densities.

[0051] Step 3: Preforming at room temperature:

[0052] Placing the dried composite magnetic powders in a mold cavity and placing them in a magnetic field H1 for pressure molding to obtain various preforms, wherein the pressing pressure is 100-600 MPa, the magnetic field H1 is less than 0.15 T, and the molding temperature is room temperature;

[0053] The density of the preform is 3.6-5.5 g / cm 3 Since the strength of the preform decreases with the decrease of density, when the density is lower than 3.6g / cm 3When the density is higher than 5.5g / cm 3 It is difficult to obtain a high degree of orientation in the subsequent temperature-pressure magnetic field orientation process.

[0054] Specifically, the preformed bodies are divided into two categories, one is a composite magnetic powder (Br: 12.5-13.0 kGs) prepared from RTB permanent magnetic powder with lower magnetic properties, and the other is a composite magnetic powder (Br: 13.0-13.5 kGs) prepared from RTB permanent magnetic powder with higher magnetic properties, wherein the Br ratio of the RTB permanent magnetic powder in the two types of composite magnetic powder is B 高 / B 低 =1.00~1.20, preferably 1.00~1.08.

[0055] Specifically, the preformed bodies are divided into two categories, including a first preformed body and a second preformed body; the density of the first preformed body is less than the density of the second preformed body.

[0056] Furthermore, the first preformed body and the second preformed body are magnetic cylinders or magnetic rings of the same shape, and the number ratio of the first preformed body to the second preformed body is 1:1 to 10:1.

[0057] Step 4: Warm-pressing magnetic field orientation molding:

[0058] A stack of several demolded preforms of different types is placed in another mold and placed in a magnetic field H2 for warm pressing and orientation, wherein the middle one is a high-performance preform and the two sides are low-performance preforms; or the center one is a high-performance preform and the periphery one is a low-performance preform, and the pressing is performed again. Specifically, the density and / or magnetic properties of the preforms arranged from the middle to the two ends gradually decrease; or, the density and / or magnetic properties of the preforms arranged from the center to the periphery gradually decrease.

[0059] During the stacking process of the preformed bodies, they are positioned by mutual magnetic attraction.

[0060] During the preform stacking process, the length of the middle preform is smaller than the upper and lower preforms; specifically, the length of the middle preform is smaller than the length of the preforms at each end.

[0061] Wherein, the magnetic field intensity H2 is 0.6-3T, the pressing pressure is 300-1000MPa, the molding temperature is 60-200°C, the gap ratio is 0.5-40%, and from the perspective of the two-step operation process and improving magnetic properties, the gap between the preformed body and the warm-pressing magnetic field orientation molding die is preferably 3.5%-25%;

[0062] Subsequently, demagnetization, cooling, and demoulding are performed to obtain anisotropic bonded magnetic rings. The demagnetization method is one of AC pulse demagnetization and reverse pulse demagnetization.

[0063] Step 5: Curing:

[0064] The curing process is: heating the final molded body to a certain temperature and then keeping it warm to further improve the strength of the bonded magnetic ring. The warming temperature is generally 100-200°C, preferably 120-180°C; the warming time is generally 0.5-2 hours, which can be adjusted appropriately according to the size of the magnetic ring.

[0065] Specific embodiments of the present invention are described below, but the present invention is by no means limited to the described embodiments.

[0066] Example 1

[0067] (1) Prepare the raw materials for bonding magnetic rings

[0068] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0069] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0070] (2) Rubber mixing

[0071] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0072] (3) Room temperature preforming

[0073] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were 4.75 g / cm 3 and 4.95g / cm 3

[0074] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 3 mm. According to actual conditions, the quantity ratio of the first preformed body to the second preformed body is 2:1.

[0075] Step 4: Warm-pressing magnetic field orientation molding:

[0076] Place the above different preformed blank stacks in another mold and place them in a magnetic field H2 (2.5T) for warm pressing and orientation. The pressing pressure is 700MPa, the molding temperature is 150°C, and the gap rate between the blank and the mold cavity is 5%. The middle one is the second preformed blank with high performance and higher density, and the two sides are the first preformed blanks with lower performance and density. The height of the first preformed blank is greater than that of the second preformed blank, and the blanks are positioned by mutual magnetic adsorption for warm pressing and orientation pressing.

[0077] Subsequently, demagnetization, cooling and demoulding are performed to obtain anisotropic bonded magnetic rings.

[0078] Step 5: Curing:

[0079] The final molded body obtained above is heated to 160° C. for curing and kept at this temperature for 1 hour, thereby completing the preparation of the anisotropic magnetic ring.

[0080] Example 2

[0081] (1) Prepare the raw materials for bonding magnetic rings

[0082] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0083] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0084] (2) Rubber mixing

[0085] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0086] (3) Room temperature preforming

[0087] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were 4.00 g / cm 3 and 4.17 g / cm 3

[0088] The other steps are the same as those in Example 1

[0089] Example 3

[0090] (1) Prepare the raw materials for bonding magnetic rings

[0091] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0092] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0093] (2) Rubber mixing

[0094] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0095] (3) Room temperature preforming

[0096] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were 5.00 g / cm 3 and 5.21g / cm 3

[0097] The other steps are the same as those in Example 1

[0098] Example 4

[0099] (1) Prepare the raw materials for bonding magnetic rings

[0100] Prepare NdFeB anisotropic permanent magnet powder with a Nd content of 29.5wt.%, a thermosetting resin binder epoxy resin, a coupling agent silane and a lubricant zinc stearate, wherein there is only one batch of NdFeB anisotropic permanent magnet powder and Br is 13.00kGs.

[0101] The other steps are the same as those in Example 1

[0102] Example 5

[0103] (1) Prepare the raw materials for bonding magnetic rings

[0104] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.5kGs and 12.5kGs respectively.

[0105] The other steps are the same as those in Example 1

[0106] Example 6

[0107] (1) Prepare the raw materials for bonding magnetic rings

[0108] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0109] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 1% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0110] The other steps are the same as those in Example 1

[0111] Example 7

[0112] (2) Prepare the raw materials for bonding magnetic rings

[0113] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0114] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 6% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0115] The other steps are the same as those in Example 1

[0116] Example 8

[0117] (1) Prepare the raw materials for bonding magnetic rings

[0118] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0119] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0120] (2) Rubber mixing

[0121] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0122] (3) Room temperature preforming

[0123] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were 4.75 g / cm 3 and 4.95g / cm 3

[0124] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 3 mm. According to actual conditions, the quantity ratio of the first preformed body to the second preformed body is 2:1.

[0125] Step 4: Warm-pressing magnetic field orientation molding:

[0126] Place the above different preformed blank stacks in another mold and place them in a magnetic field H2 (2.5T) for warm pressing and orientation. The pressing pressure is 700MPa, the molding temperature is 150°C, and the gap rate between the blank and the mold cavity is 5%. The middle one is the second preformed blank with high performance and higher density, and the two sides are the first preformed blanks with lower performance and density. The height of the first preformed blank is greater than that of the second preformed blank, and the blanks are positioned by mutual magnetic adsorption for warm pressing and orientation pressing.

[0127] Subsequently, demagnetization, cooling and demoulding are performed to obtain anisotropic bonded magnetic rings.

[0128] Step 5: Curing:

[0129] The final molded body obtained above is heated to 120° C. for curing and kept at this temperature for 1 hour to complete the preparation of the anisotropic magnetic ring.

[0130] After magnetizing the prepared magnetic ring, the surface magnetic distribution at the upper, middle and lower ends is tested, and then the magnetic ring is cut into three sections to obtain the density and performance data at the two ends and the middle, and to evaluate the uniformity of the density and performance distribution along the axial direction.

[0131] The other steps are the same as those in Example 1

[0132] Example 9

[0133] (1) Prepare the raw materials for bonding magnetic rings

[0134] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0135] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0136] (2) Rubber mixing

[0137] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0138] (3) Room temperature preforming

[0139] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were 4.75 g / cm 3 and 4.95g / cm 3

[0140] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 3 mm. According to actual conditions, the quantity ratio of the first preformed body to the second preformed body is 2:1.

[0141] Step 4: Warm-pressing magnetic field orientation molding:

[0142] Place the above different preformed blank stacks in another mold and place them in a magnetic field H2 (2.5T) for warm pressing and orientation. The pressing pressure is 700MPa, the molding temperature is 150°C, and the gap rate between the blank and the mold cavity is 5%. The middle one is the second preformed blank with high performance and higher density, and the two sides are the first preformed blanks with lower performance and density. The height of the first preformed blank is greater than that of the second preformed blank, and the blanks are positioned by mutual magnetic adsorption for warm pressing and orientation pressing.

[0143] Subsequently, demagnetization, cooling and demoulding are performed to obtain anisotropic bonded magnetic rings.

[0144] Step 5: Curing:

[0145] The final molded body obtained above is heated to 180° C. for curing and kept at this temperature for 1 hour to complete the preparation of the anisotropic magnetic ring.

[0146] The other steps are the same as those in Example 1

[0147] Comparative Example 1

[0148] (1) Prepare the raw materials for bonding magnetic rings

[0149] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0150] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0151] (2) Rubber mixing

[0152] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0153] (3) Room temperature preforming

[0154] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were both 4.75 g / cm 3

[0155] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 3 mm. According to actual conditions, the quantity ratio of the first preformed body to the second preformed body is 2:1.

[0156] The other steps are the same as those in Example 1

[0157] Comparative Example 2

[0158] (1) Prepare the raw materials for bonding magnetic rings

[0159] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0160] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0161] (2) Rubber mixing

[0162] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0163] (3) Room temperature preforming

[0164] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were both 3.6 g / cm 3

[0165] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 3 mm. According to actual conditions, the quantity ratio of the first preformed body to the second preformed body is 2:1.

[0166] The other steps are the same as those in Example 1

[0167] Comparative Example 3

[0168] (1) Prepare the raw materials for bonding magnetic rings

[0169] Prepare NdFeB anisotropic permanent magnet powder with Nd content of 29.5wt.%, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate, wherein the NdFeB anisotropic permanent magnet powder has two batches of high performance and low performance, and Br is 13.25kGs and 12.75kGs respectively.

[0170] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.

[0171] (2) Rubber mixing

[0172] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of NdFeB anisotropic permanent magnet powders mentioned above, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the NdFeB anisotropic permanent magnet powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.

[0173] (3) Room temperature preforming

[0174] The two composite magnetic powders prepared above were dried and placed in a mold cavity and placed in a magnetic field H1 = 0 for pressure molding to obtain different preforms, wherein the pressing pressure was 350 MPa, and the densities of the first and second preforms were both 5.5 g / cm 3

[0175] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 3 mm. According to actual conditions, the quantity ratio of the first preformed body to the second preformed body is 2:1.

[0176] The other steps are the same as those in Example 1

[0177] After magnetizing the prepared magnetic ring, the surface magnetic distribution and radial crushing force at the upper, middle and lower ends were tested, and then the magnetic ring was cut into three sections to obtain the density and performance data at the two ends and the middle, and to evaluate the uniformity of the density and performance along the axial distribution, as shown in Table 1.

[0178] Table 1

[0179]

[0180] In summary, the present invention provides an anisotropic bonded magnet and a method for preparing the same. By stacking magnets with different magnetic properties and / or densities, the magnet in the middle has high performance and the magnets at both ends and / or the periphery have low performance, thereby compensating for the performance deviation caused by density differences during the pressing process and improving the performance uniformity of the magnet in the axial direction. This method solves the problem of highly directional magnetic field orientation and uneven density during the orientation and densification process, as well as the problem of low in the middle and high on both sides. The anisotropic bonded magnet prepared by this method has the characteristic of a density deviation of less than 2% along the pressing direction, which effectively improves the orientation degree and density of the magnet, as well as the uniformity and dimensional accuracy of the magnetic properties of the magnet.

[0181] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. An anisotropic bonded magnet, characterized in that: It includes RTB permanent magnet powder, wherein R is selected from one or more rare earth elements, T is Fe or FeCo, and B is boron; Among them, the content of R is 28-31wt.%, the content of B is 0.9-1.1wt.%, and the balance is T; The anisotropic bonded magnet is formed by pressing a plurality of different preformed bodies, and the density deviation along the pressing direction is less than 2%; the plurality of different preformed bodies include a first preformed body and a second preformed body; The first preformed body is made of composite magnetic powder with lower magnetic properties, and the second preformed body is made of composite magnetic powder with higher magnetic properties, wherein the ratio of the remanence Br of the RTB type permanent magnetic powder in the two types of composite magnetic powder is Br 高 / Br 低 =1.00~1.20,Br 高 Indicates the remanence of composite magnetic powder with higher magnetic properties, Br 低 Indicates the remanence of the composite magnetic powder with lower magnetic properties; or the density of the first preform is less than the density of the second preform; Putting the plurality of different preformed bodies into a mold for pressing comprises: the middle is a second preformed body, and the two ends or the periphery are first preformed bodies.

2. The anisotropic bonded magnet according to claim 1, characterized in that: R is one or more elements selected from the group consisting of Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu.

3. The anisotropic bonded magnet according to claim 2, characterized in that: R is Nd, or Pr and Nd.

4. The anisotropic bonded magnet according to claim 1, characterized in that: The bonded magnet is a bonded magnetic ring, the aspect ratio of the bonded magnetic ring is greater than 0.6, and the wall thickness is greater than 1 mm.

5. The anisotropic bonded magnet according to claim 4, characterized in that: The bonded magnetic ring has an aspect ratio of 1.0-10 and a wall thickness of 1-20 mm.

6. The anisotropic bonded magnet according to claim 5, characterized in that: The bonded magnetic ring has an aspect ratio of 2-8 and a wall thickness of 1-5 mm.

7. A method for preparing anisotropic bonded magnet according to claim 1, characterized in that: The steps include: Step 1, preparing bonded magnet raw materials: the raw materials include RTB permanent magnet powder, thermosetting resin binder, coupling agent and lubricant; wherein the weight content of RTB permanent magnet powder is 100, the weight content of binder is 1.0% to 6.0% of RTB permanent magnet powder, the weight content of coupling agent is 0.05% to 1.0% of RTB permanent magnet powder, and the weight content of lubricant is 0.05% to 2.0% of RTB permanent magnet powder; Step 2, mixing: uniformly mixing the RTB permanent magnetic powder in the raw material with the thermosetting resin binder, coupling agent and lubricant to obtain composite magnetic powder; Step 3, preforming at room temperature: placing the dried composite magnetic powders of various different magnetic properties in a first mold and placing them in a magnetic field H1 for press forming to obtain various different preformed bodies, wherein the pressing pressure is 100-600 MPa, the magnetic field H1 is less than 0.15 T, and the pressing temperature is room temperature; the various different preformed bodies include a first preformed body and a second preformed body; The first preformed body is made of composite magnetic powder with lower magnetic properties, and the second preformed body is made of composite magnetic powder with higher magnetic properties, wherein the ratio of the remanence Br of the RTB type permanent magnetic powder in the two types of composite magnetic powder is Br 高 / Br 低 =1.00~1.20; or, The density of the first preform is less than the density of the second preform, Step 4, warm-pressing magnetic field orientation molding: placing a plurality of different preformed green bodies in a second mold and placing them in a magnetic field H2 for warm-pressing molding and orientation, and pressing them again; then demagnetizing, cooling, and demolding to obtain anisotropic bonded magnets formed by warm-pressing magnetic field orientation; wherein the magnetic field H2 is 0.6-3T, the pressing pressure is 300-1000MPa, and the molding temperature is 60-200°C; wherein placing a plurality of different preformed green bodies in a second mold includes: the middle is the second preformed green body, and the two ends or the periphery are the first preformed green bodies; Step 5, curing: heating the anisotropic bonded magnet formed by warm-pressing magnetic field orientation to a certain temperature and then keeping it warm, the warming temperature is 100-200° C. and the warming time is 0.5-2 hours.

8. The method according to claim 7, characterized in that The step 2 comprises: The coupling agent measured in the above step is dissolved in the corresponding organic solvent, and then mixed evenly with the RTB permanent magnet powder. After the organic solvent is volatilized and removed, the coupling agent is evenly coated on the surface of the permanent magnet powder. Then the measured binder and lubricant are dissolved in the corresponding organic solvent, and mixed evenly with the RTB permanent magnet powder coated with the coupling agent. After the organic solvent is removed, the composite magnetic powder required for preparing the bonded magnet is obtained.

9. The method according to claim 8, characterized in that The ratio of the remanence Br of the RTB type permanent magnetic powder in the two types of composite magnetic powders is Br 高 / Br 低 The value is 1.00-1.

08.

10. The method according to any one of claims 7 to 9, characterized in that: In step 4, stacking a plurality of different preforms into the second mold further comprises: the length of the middle second preform is smaller than the length of the first preforms at both ends.

11. The method according to claim 7, characterized in that The stacking of a plurality of different preforms into the second mold includes: the density and / or magnetic properties of the preforms arranged from the middle to the two ends gradually decrease; or the density and / or magnetic properties of the preforms arranged from the center to the periphery gradually decrease.

12. The method according to any one of claims 7 to 9, characterized in that: In the step 4, the gap ratio between the preformed body and the warm-pressing magnetic field orientation forming die is 0.5 to 40%.

13. The method according to claim 12, characterized in that In step 4, the gap ratio between the preformed body and the warm-pressing magnetic field orientation forming mold is 3.5%-25%.

14. The method according to claim 7, characterized in that The first preformed body and the second preformed body are magnetic cylinders or magnetic rings of the same shape, and the number ratio of the first preformed body to the second preformed body is 1:1 to 10:

1.

15. The method according to claim 7, characterized in that The weight content of the binder is 2.5% to 3.5% of the RTB permanent magnet powder, the weight content of the coupling agent is 0.1% to 0.3% of the RTB permanent magnet powder, and the weight content of the lubricant is 0.05% to 0.50% of the RTB permanent magnet powder.

16. The method according to claim 7, characterized in that In step 5, the insulation temperature is 120-180°C.