Photoresist GPP chip with composite passivation film structure, preparation method and electronic device
By adding aluminum oxide film and silicon nitride film to the photoresist GPP chip to form a composite passivation film structure, the leakage problem of traditional photoresist GPP chips in high-temperature reverse bias experiments is solved, and the reliability requirements of automotive electronics customers are met. Improved product stability and shielding capabilities.
Patent Information
- Application Number
- CN202111076072.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-14
AI Technical Summary
Traditional photoresist GPP chip packaging cannot meet the reliability requirements of automotive electronics customers in high-temperature reverse bias experiments, mainly due to leakage problems caused by movable ion contamination during the SMA packaging process.
On the basis of the traditional photoresist GPP chip, an aluminum oxide film and a silicon nitride film are added to form a composite passivation film structure to prevent movable ions from moving to the silicon surface, and the movable ion electric field is controlled through a semi-insulating oxygen-doped polysilicon film. Neutralize to ensure that the product passes the assessment at 150℃/80% back pressure/1000 hours.
It effectively avoids the movement of movable ions, significantly improves the high-temperature reverse bias performance and reliability of the product, and ensures the stability of the product under high-temperature conditions and the shielding effect during the packaging process.
Smart Images

Figure CN113745173B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photoresist GPP chips, and in particular relates to a photoresist GPP chip with a composite passivation film structure, a preparation method and an electronic device. Background Art
[0002] The statements in this section merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] GPP is the abbreviation of Glassivation passivation parts or parts of an apparats, which is a general term for glass passivation devices, and refers to all active devices that introduce or contain junction film protection process means. However, since the glass passivation process measures are more effective in applying various planar diodes with exposed junction interfaces, and have become successful typical applications, GPP (Glassivation passivation parts) has gradually become synonymous with "glass passivation diodes".
[0004] The production of photoresist GPP chips is a mature process in the diode industry. The photoresist method uses the most advanced photosensitive glass powder lithography technology (photo glass technology), and through photolithography technology, it can achieve precise control of the passivation layer coverage area. The traditional photoresist GPP chip has three layers of passivation film, from the inside to the outside, they are sipos (semi-insulating polycrystalline-silicon, semi-insulating oxygen-doped polycrystalline silicon) film, glass and Lto (Low temperature oxide, low temperature oxide) film (its main component is SiO2). Among them, the first passivation film is sipos film, which is a semi-insulating oxygen-doped polycrystalline silicon film with a thickness of about 0.4μm to 0.6μm; sipos film plays a role in compensating or eliminating surface (positive / negative) ions and has the ability to capture movable ions. The second passivation film is glass, with a thickness of about 30μm to 50μm; this glass layer has a negative charge effect, which neutralizes positive ions to a certain extent, has high dielectric strength, strong radiation resistance, high mechanical strength and hardness, and plays a key role in improving the reverse breakdown voltage, but has a weak ability to block mobile ions. The third passivation film is an Lto film, which is a chemical vapor deposited SiO2 layer with a thickness of about 0.2μm to 0.6μm; the oxide layer has a poor ability to block mobile ions, but the oxide layer covers and protects the passivation layer below. Since it does not wet with solder, it can block solder, prevent solder overflow, and prevent solder from squeezing and contaminating the passivation layer.
[0005] Compared with scraped GPP and electrophoretic GPP chips, traditional photoresist GPP chips have the advantages of low high-temperature leakage, high leakage consistency at room temperature, long high-temperature life, and significantly reduced probability of glass cracks. Therefore, photoresist GPP is the most stable and reliable commercial product at present. However, the biggest disadvantage of photoresist GPP chips is that the cost will be correspondingly higher.
[0006] In the current application market of high-end electronic products, such as automotive electronics, customers have increasingly higher requirements for photoresist GPP diodes. The inventors have found that the traditional photoresist GPP chip packaged into plastic-encapsulated diodes, such as SMA-encapsulated GPP diodes, can no longer fully meet the needs of these high-end customers in high-temperature reverse bias experiments due to the serious contamination during the SMA packaging process (mobile ion contamination). Taking the SMA-encapsulated M7 product as an example, automotive electronics customers require the product to pass the high-temperature reverse bias test of 150°C / 80% reverse voltage / 1000 hours. The traditional photoresist GPP chip packaged plastic-encapsulated diode products cannot guarantee that each production batch meets this reliability requirement. Summary of the invention
[0007] In order to solve the technical problems existing in the above-mentioned background technology, the present invention provides a photoresist GPP chip, a preparation method and an electronic device with a composite passivation film structure. On the basis of the passivation layer design of the traditional photoresist GPP chip, an aluminum oxide film is added on the glass surface, and a silicon nitride film is added on the surface of the semi-insulating oxygen-doped polysilicon film. With the protection of these two passivation layers, the mobile ions can be completely prevented from moving to the silicon surface. In addition, the semi-insulating oxygen-doped polysilicon film has a neutralizing effect on the electric field of the mobile ions, which can ensure that the product can pass the high-temperature reverse bias test of 150°C / 80% reverse pressure / 1000 hours.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] The first aspect of the present invention provides a photoresist GPP chip with a composite passivation film structure, comprising a semi-insulating oxygen-doped polysilicon film, glass and a low-temperature oxide film arranged in sequence from the inside to the outside, an aluminum oxide film is arranged on the low-temperature oxide film, and a silicon nitride film is arranged on the semi-insulating oxygen-doped polysilicon film.
[0010] Furthermore, the thickness of the aluminum oxide film is 0.05 μm-0.15 μm.
[0011] The advantage of the above technical solution is that the aluminum oxide film with a thickness ranging from 0.05μm to 0.15μm has strong metal alkalinity barrier and anti-migration capabilities; it also has high mechanical strength and hardness, prevents surface scratches or bumps, and improves the stability of production and processing; it also has a certain radiation resistance, which can increase the reliability of the product.
[0012] Furthermore, the thickness of the silicon nitride film is 0.2 μm-0.4 μm.
[0013] The advantage of the above technical solution is that the silicon nitride film with a thickness in the range of 0.2 μm-0.4 μm is effective for alkali metal ions (such as Na + ) has strong blocking and capturing capabilities, and can significantly improve the shielding effect on mobile ions during the packaging process.
[0014] A second aspect of the present invention provides a method for preparing a photoresist GPP chip with a composite passivation film structure, comprising:
[0015] Coating a photoresist on the diffusion sheet where the oxide layer is grown;
[0016] Performing a photolithography trench on the exposed area to be etched to form a silicon wafer with trenches;
[0017] Depositing a semi-insulating oxygen-doped polysilicon film and a silicon nitride film in sequence on a silicon wafer having a groove;
[0018] Perform secondary photolithography on the silicon nitride film to coat a glass photoresist, and sinter to form a glass protective layer;
[0019] A low temperature oxide film and an aluminum oxide film are sequentially deposited on the glass protective layer to form a wafer, and the front side of the wafer is photoetched three times to expose the welding area;
[0020] Plating metal on the welding area on the front side of the wafer and on the back side of the wafer respectively;
[0021] The back side of the metal-plated wafer is diced to obtain a photoresist GPP chip.
[0022] Furthermore, the diffusion sheet is obtained by boron phosphorus diffusion, sandblasting and cleaning processes in sequence.
[0023] Furthermore, a negative photoresist is coated on the diffusion sheet where the oxide layer is grown by a photolithography process.
[0024] Furthermore, a mixed acid is used to perform trench etching on the area to be etched to form a silicon wafer with trenches.
[0025] Furthermore, a semi-insulating oxygen-doped polysilicon film is deposited by LPCVD, and a layer of aluminum oxide film is deposited by magnetron sputtering.
[0026] Furthermore, the metals plated on the welding area on the front side of the wafer and on the back side of the wafer are nickel and gold.
[0027] The third aspect of the present invention provides an electronic device, which includes the photoresist GPP chip with the composite passivation film structure as described above.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The present invention is based on the design of a traditional photoresist GPP chip including three passivation layers, namely, a semi-insulating oxygen-doped polysilicon film, a glass and a low-temperature oxide film, which are sequentially arranged from the inside to the outside. An aluminum oxide film is added to the surface of the low-temperature oxide film, and a silicon nitride film is added to the surface of the semi-insulating oxygen-doped polysilicon film. Due to the protection of the two passivation layers of the aluminum oxide film and the silicon nitride film, the mobile ions can be completely prevented from moving to the silicon surface. In addition, the semi-insulating oxygen-doped polysilicon film has a neutralizing effect on the electric field of the mobile ions, which ensures that the product can pass the 150°C / 80% reverse voltage / 1000 hour test at high temperature reverse bias.
[0030] Advantages of additional aspects of the present invention will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0032] Figure 1 It is a schematic diagram of the structure after one-time photolithography is completed for the groove etching according to an embodiment of the present invention.
[0033] Figure 2 It is a schematic diagram of the structure after the secondary photolithography of the embodiment of the present invention completes the photoresist development.
[0034] Figure 3 It is a schematic diagram of the structure of an embodiment of the present invention in which three photolithography steps are performed to complete the deposition of the passivation layer and etch out the P-side welding area.
[0035] Figure 4 This is a schematic diagram of the structure of a traditional photoresist GPP chip.
[0036] Figure 5 Schematic diagram of the GPP chip structure of an embodiment of the present invention.
[0037] Among them, 1-semi-insulating oxygen-doped polysilicon film; 2-glass; 3-low-temperature oxide film; 4-silicon nitride film; 5-aluminum oxide film. DETAILED DESCRIPTION
[0038] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0039] It should be noted that the following detailed descriptions are all illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0040] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0041] Embodiment 1
[0042] The conventional photoresist GPP chip packaged plastic-encapsulated diode products mentioned in the background technology cannot guarantee that each production batch meets this reliability requirement for the following reasons:
[0043] High temperature reverse bias test can check whether there is serious mobile ion contamination in semiconductor devices. In the experiment, the diode chip is applied with reverse bias voltage, and 80% reverse bias voltage is applied at high temperature of 150℃. The experiment can reveal the weakness and degradation effect of field depletion structure at the chip edge and passivation layer.
[0044] During the assembly and welding process of the photoresist GPP chip, it will be contaminated from many aspects, such as flux, solder paste, rosin volatiles in the environment, rosin volatiles in the welding furnace, etc. The chip surface is contaminated with a large amount of mobile alkaline metal ions (Na + , K + These mobile ions gradually move to the glass of the chip in the subsequent high-temperature process. When the amount of contamination is large, a large number of mobile ions will move to the surface of the sipos (semi-insulating oxygen-containing polysilicon) film. Although in theory the sipos film has a certain blocking effect on mobile ions, in reality there are always certain structural defects in the sipos film, resulting in a certain amount of mobile ions still moving through the sipos film and eventually moving to the silicon surface of the chip groove.
[0045] When the product is doing a high-temperature reverse bias experiment, due to the presence of mobile ions on the surface of the chip trench silicon, a small amount of mobile ions on the surface will affect the width of the PN junction depletion layer and the electric field distribution, resulting in local electric field concentration on the surface of the trench silicon, leading to leakage concentration. Therefore, during the high-temperature reverse bias process, the area where the leakage is concentrated is prone to a thermoelectric positive feedback mechanism, which is manifested as a continuous increase in high-temperature leakage and eventually thermal breakdown. When there are a large number of mobile ions on the surface of the trench silicon, it may even lead to the enhancement of N-type silicon, causing P-type silicon to invert to N-type silicon, resulting in leakage channels on the surface of the trench silicon, and the leakage of the product at room temperature will also increase.
[0046] In order to solve the technical problem that the conventional photoresist GPP chip packaged plastic-encapsulated diode products mentioned in the background technology cannot ensure that each production batch meets the reliability requirements, the present embodiment provides a photoresist GPP chip with a composite passivation film structure, including a semi-insulating oxygen-doped polysilicon film 1, a glass 2 and a low-temperature oxide film 3 arranged in sequence from the inside to the outside, an aluminum oxide film 5 is arranged on the low-temperature oxide film 3, and a silicon nitride film 4 is arranged on the semi-insulating oxygen-doped polysilicon film 1. Figure 5 shown.
[0047] The conventional photoresist GPP chip structure only includes three passivation layers, namely, a semi-insulating oxygen-doped polysilicon film 1 , a glass 2 , and a low-temperature oxide film 3 , which are sequentially arranged from the inside to the outside.
[0048] In this embodiment, a layer of (amorphous) silicon nitride film 4 is deposited on the surface of the semi-insulating oxygen-doped polysilicon film 1 (wherein the deposition method is, for example, by LPCVD method).
[0049] The thickness of the silicon nitride film is 0.2 μm-0.4 μm. The silicon nitride film with a thickness of 0.2 μm-0.4 μm is resistant to alkali metal ions (such as Na + ) has strong blocking and capturing capabilities, and can significantly improve the shielding effect on mobile ions during the packaging process.
[0050] When the chip is in the welding process, the mobile ions in the flux residue will adhere to the chip passivation layer. When the product goes through the processes of plastic sealing, curing, reflow soldering, etc., the low-temperature oxide film 3 and the glass have a weak shielding effect on the mobile ions, and the mobile ions can easily move to the surface of the semi-insulating oxygen-doped polysilicon film 1. However, the mobile ions can hardly move in the silicon nitride film 4, so the mobile ions are shielded on the surface of the silicon nitride film 4, and the mobile ions can hardly move to the silicon surface.
[0051] Furthermore, since the semi-insulating oxygen-doped polysilicon film 1 neutralizes the electric field of the movable ions, the movable ions on the silicon nitride surface have no effect on the PN junction on the chip trench surface, thereby significantly reducing leakage current during high temperature reverse bias.
[0052] A layer of aluminum oxide film 5 is deposited on the surface of the low temperature oxide film 3 by magnetron sputtering. Magnetron sputtering is suitable for the preparation of a surface passivation layer due to its low temperature, small radiation damage to the chip, high film density, and high adhesion between the film and the substrate low temperature oxide film 3.
[0053] The thickness of the aluminum oxide film 5 is 0.05 μm-0.15 μm. The aluminum oxide film with a thickness of 0.05 μm-0.15 μm has strong metal alkalinity barrier and anti-migration capabilities; it also has high mechanical strength and hardness, prevents surface scratches or bumps, improves the stability of production and processing; it also has a certain radiation resistance, which can increase the reliability of the product.
[0054] Since the aluminum oxide film 5 also has a blocking effect on mobile ions, after the chip is contaminated during the welding and packaging process, it is also difficult for the mobile ions to diffuse and move into the glass, thereby serving as the first barrier, that is, protecting the groove silicon surface.
[0055] Embodiment 2
[0056] This embodiment provides a method for preparing a photoresist GPP chip with a composite passivation film structure, which comprises the following steps:
[0057] Step 1: Apply photoresist on the diffusion sheet where the oxide layer is grown.
[0058] The diffusion sheet is obtained by boron-phosphorus diffusion, sandblasting and cleaning processes in sequence.
[0059] In a specific implementation, an oxide layer is first grown by a set temperature oxidation process, and the diffuser is annealed; then a negative photoresist is coated on the diffuser with the grown oxide layer by a photolithography process, and exposure and development are performed to expose the area to be etched.
[0060] Step 2: Photolithography is performed on the exposed area to be etched to form a silicon wafer with grooves, such as Figure 1 shown.
[0061] In a specific implementation, a mixed acid is used to perform trench etching on the area to be etched to form a silicon wafer with trenches.
[0062] In other embodiments, other methods may be used to perform trench etching on the area to be etched to form a silicon wafer with trenches.
[0063] Step 3: sequentially depositing a semi-insulating oxygen-doped polysilicon film and a silicon nitride film on the silicon wafer having the grooves;
[0064] Specifically, a semi-insulating oxygen-doped polysilicon film and a silicon nitride film may be deposited using LPCVD.
[0065] Step 4: Perform secondary photolithography on the silicon nitride film to coat glass photoresist, and sinter to form a glass protective layer.
[0066] Specifically, a glass photoresist is coated by a photolithography process, and then exposed and developed. Figure 2 shown.
[0067] The wafer is sintered at high temperature to form a glass protective layer.
[0068] Step 5: depositing a low-temperature oxide film and an aluminum oxide film on the glass protective layer in sequence to form a wafer, and performing three photolithography operations on the front side of the wafer to expose the welding area;
[0069] Specifically, a semi-insulating oxygen-doped polysilicon film is deposited using LPCVD, and a layer of aluminum oxide film is deposited using magnetron sputtering.
[0070] It should be noted that, in other embodiments, the method of depositing the semi-insulating oxygen-doped polysilicon film and the aluminum oxide film may also be implemented by other existing methods, which will not be described in detail here.
[0071] Step 6: Metallize the soldering area on the front side of the wafer and on the back side of the wafer.
[0072] In a preferred embodiment, the metals plated on the bonding area on the front side of the wafer and on the back side of the wafer are nickel and gold.
[0073] It is understood that in other embodiments, the plated metal may be only nickel;
[0074] The plated metal may also be titanium nickel silver or nickel silver.
[0075] Step 7: Slice the back of the metal-plated wafer to obtain a photoresist GPP chip.
[0076] Embodiment 3
[0077] This embodiment provides an electronic device, which includes a photoresist GPP chip with a composite passivation film structure as described in the first embodiment above.
[0078] It should be noted that the electronic device may be a power supply, adapter, lighting, display or automotive rectifier equipment, etc. The photoresist GPP chip with the composite passivation film structure is packaged into a diode or a bridge rectifier, and mainly plays a rectifying and protective role in the above-mentioned electronic devices.
[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a photoresist GPP chip with a composite passivation film structure, characterized in that: include: Coating a photoresist on the diffusion sheet where the oxide layer is grown; Performing a photolithography trench on the exposed area to be etched to form a silicon wafer with trenches; Depositing a semi-insulating oxygen-doped polysilicon film and a silicon nitride film in sequence on a silicon wafer having a groove; depositing the semi-insulating oxygen-doped polysilicon film using LPCVD; the thickness of the silicon nitride film is 0.2 μm-0.4 μm; Perform secondary photolithography on the silicon nitride film to coat a glass photoresist, and sinter to form a glass protective layer; A low temperature oxide film and an aluminum oxide film are sequentially deposited on the glass protective layer to form a wafer, and a layer of aluminum oxide film is deposited by magnetron sputtering; the front side of the wafer is photoetched three times to expose the welding area; the thickness of the aluminum oxide film is 0.05 μm-0.15 μm; The welding area on the front side of the wafer and the back side of the wafer are plated with metals respectively; the metals plated on the welding area on the front side of the wafer and the back side of the wafer are nickel and gold; The back side of the metal-plated wafer is diced to obtain a photoresist GPP chip, wherein the photoresist GPP chip includes a semi-insulating oxygen-doped polysilicon film, glass and a low-temperature oxide film arranged in sequence from the inside to the outside, an aluminum oxide film is arranged on the low-temperature oxide film, and a silicon nitride film is arranged on the semi-insulating oxygen-doped polysilicon film.
2. The method for preparing the photoresist GPP chip with a composite passivation film structure according to claim 1, characterized in that: The diffusion sheet is obtained by boron phosphorus diffusion, sandblasting and cleaning processes in sequence.
3. The method for preparing the photoresist GPP chip with a composite passivation film structure according to claim 1, characterized in that: A negative photoresist is coated on the diffusion sheet on which the oxide layer is grown by a photolithography process.
4. The method for preparing the photoresist GPP chip with a composite passivation film structure according to claim 1, characterized in that: A mixed acid is used to perform trench etching on the area to be etched to form a silicon wafer with grooves.
5. A photoresist GPP chip with a composite passivation film structure prepared by the method according to any one of claims 1 to 4, comprising a semi-insulating oxygen-doped polysilicon film, a glass and a low-temperature oxide film arranged in sequence from the inside to the outside, characterized in that: An aluminum oxide film is disposed on the low temperature oxide film, and a silicon nitride film is disposed on the semi-insulating oxygen-doped polysilicon film.
6. The photoresist GPP chip with a composite passivation film structure as claimed in claim 5, characterized in that: The thickness of the aluminum oxide film is 0.05 μm-0.15 μm.
7. The photoresist GPP chip with a composite passivation film structure as claimed in claim 5, characterized in that: The thickness of the silicon nitride film is 0.2 μm-0.4 μm.
8. An electronic device, characterized in that: A photoresist GPP chip comprising the composite passivation film structure according to any one of claims 5 to 7.
Citation Information
Patent Citations
Multilayer composite membrane passivation structure of table top high-power semiconductor device and manufacturing technology of multilayer composite membrane passivation structure of table top high-power semiconductor device
CN103730430A
High-reliability photoresist glass passivation chip and processing method thereof
CN109755209A
Solar cell with passivation layer structure and preparation method thereof
CN110047950A