Resin composition

By using aluminum pigments and lubricants of specific particle sizes in polyacetal resin, the problems of formaldehyde generation and mold contamination during the molding process of polyacetal resin are solved, the gloss and weather resistance are improved, and the resin composition is achieved with high efficiency Forming effect.

CN113754983BActive Publication Date: 2024-12-06ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110608665.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-03
Filing Date
2021-06-01
Publication Date
2024-12-06
Estimated Expiration
2041-06-01

AI Technical Summary

Technical Problem

The existing polyacetal resin compositions are prone to formaldehyde during the molding process, resulting in poor appearance effect and mold contamination, and insufficient gloss and weather resistance.

Method used

By adding aluminum fine particles with a particle size of less than 1 μm to the polyacetal resin, aluminum pigment with a volume average particle size in the range of 3 μm to 40 μm, and combining lubricant and formaldehyde inhibitor, the composition of the resin composition is adjusted to reduce formaldehyde production to reduce formaldehyde production. and improve gloss and weather resistance.

Benefits of technology

The amount of formaldehyde production is reduced, the appearance gloss and weather resistance is improved, mold pollution is avoided, and the mechanical characteristics and production stability of the resin are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003095078840000041
    Figure BDA0003095078840000041
  • Figure BDA0003095078840000311
    Figure BDA0003095078840000311
  • Figure FDA0004925026740000051
    Figure FDA0004925026740000051
Patent Text Reader

Abstract

The present invention relates to a resin composition. The purpose of the present disclosure is to provide a resin composition, which can obtain a molded product with less formaldehyde generation and excellent appearance and weather resistance, and can suppress mold contamination during molding. The present disclosure is a polyacetal resin composition, characterized in that the polyacetal resin composition comprises: 100 parts by mass of (A) polyacetal resin, and 0.1 parts by mass to 10 parts by mass of (B) aluminum pigment, relative to the total amount of the (B) aluminum pigment, the (B) aluminum pigment contains 0.1% by mass to 2.0% by mass of particles with a particle size of less than 1 μm, and the volume average particle size of the (B) aluminum pigment is 3 μm to 40 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to resin compositions. Background Art

[0002] Crystalline resins such as polyolefins, polyacetals or polyamides have crystals with regularly arranged molecular chains, and have a variety of useful features such as high mechanical strength and rigidity, excellent chemical resistance, etc. In addition, due to its easy processing, it has been used in a wide range of mechanical parts and sliding parts centered on precision instruments, household appliances, office automation equipment, automobiles, industrial materials and daily necessities. Among them, in order to give a characteristic metallic luster called metallic tone, a metallic coloring pigment containing metal particles represented by flaky aluminum powder (hereinafter also referred to as "thin aluminum flakes") is added to various crystalline resins. Resin compositions with metallic coloring pigments are used for automotive interior and exterior parts, computer housings, etc.

[0003] For example, in the resin compositions described in Patent Documents 1 to 5 shown below, attempts have been made to express metallic gloss and impart design properties by molding a resin containing a gloss pigment. Specifically, Patent Documents 1 and 2 disclose molded bodies of synthetic resin compositions blended with specific metal pigments. In addition, Patent Document 3 proposes a resin composition comprising a polyacetal resin, a weathering agent, aluminum particles having a specific particle size, a specific particle size distribution, and a specific particle thickness, and a specific fatty acid as a resin composition having excellent production stability, mechanical properties, molding appearance, welding performance, and brightness. In addition, Patent Document 4 proposes a polyacetal resin comprising a polyacetal resin, a guanamine compound, a weathering agent, and a specific metal pigment as a polyacetal resin composition having a low amount of formaldehyde generated from a molded body and excellent weather resistance. In addition, Patent Document 5 discloses a molded product having a metallic appearance obtained from a polymer composition comprising a polyacetal resin, a metal pigment, and an ultraviolet stabilizer in an amount of about 60% by weight or more. Furthermore, Patent Document 5 proposes a technology in which a metal pigment is present in an amount sufficient to provide an outer surface having a glossiness greater than about 45 Gs when the molded product is measured at an angle of 60 degrees in the polymer composition, and the metal pigment is sufficiently dispersed in the polymer composition.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 62-020574

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 61-159453

[0008] Patent Document 3: Japanese Patent Application Publication No. 2010-065210

[0009] Patent Document 4: Japanese Patent Application Publication No. 2009-155418

[0010] Patent Document 5: International Publication No. 2013 / 49541 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, when the methods described in Patent Documents 1 and 2 are applied to polyacetal resins, the above attempts have not achieved sufficient effects on the suppression of formaldehyde generation or product appearance such as gloss due to the heat generated during melt mixing and the influence of active sites on the surface of metal particles. Furthermore, for the resin composition described in Patent Document 3, no study has been conducted on the influence of the composition on the formaldehyde generation and the influence of the formaldehyde generation on product appearance such as gloss.

[0013] On the other hand, Patent Document 4 proposes a technology for the purpose of thermal stability of molded bodies and formaldehyde suppression. However, only a polyacetal resin composition to which a substance obtained by dispersing aluminum powder as a metal pigment in polyethylene is added is disclosed, and no study is conducted on the influence of formaldehyde on the glossiness, brightness and other product appearances of the obtained molded body. In addition, no sufficient effect is obtained on the glossiness, brightness and other product appearances. In addition, when an aluminum pigment is used to manufacture a molded body with high gloss as in the technology described in Patent Document 5, mold contamination caused by the pigment particles may sometimes occur. Therefore, in the above situation, a polyacetal resin composition is required that generates less formaldehyde during processing such as injection molding and has excellent appearance and weather resistance.

[0014] Therefore, an object of the present disclosure is to provide a polyacetal resin composition that can produce a molded product with less formaldehyde generation and excellent appearance and weather resistance, and can suppress mold contamination during molding.

[0015] Means used to solve problems

[0016] The present inventors have conducted intensive research and found that by adding an aluminum pigment to a polyacetal resin, wherein the aluminum pigment contains particles such as aluminum microparticles with a particle size of less than 1 μm in a specified amount and has a volume average particle size in a specific range, the following resin composition can be obtained: the resin composition can produce a molded product with less formaldehyde generation and excellent appearance and weather resistance, and can also suppress mold contamination during molding, thereby completing the present invention.

[0017] [1] The present invention discloses a polyacetal resin composition, characterized in that the polyacetal resin composition comprises: 100 parts by mass of (A) a polyacetal resin, and 0.1 parts by mass to 10 parts by mass of (B) an aluminum pigment,

[0018] The (B) aluminum pigment contains 0.1 to 2.0% by mass of particles having a particle size of 1 μm or less based on the total amount of the (B) aluminum pigment, and the (B) aluminum pigment has a volume average particle size of 3 to 40 μm.

[0019] [2] The polyacetal resin composition of the present disclosure preferably further contains (C) a lubricant.

[0020] [3] In the polyacetal resin composition of the present disclosure, it is preferred that the polyacetal resin composition contains 1 to 4 parts by mass of the (B) aluminum pigment relative to 100 parts by mass of the (A) polyacetal resin.

[0021] [Effects of the invention]

[0022] According to the present disclosure, it is possible to provide a polyacetal resin composition that can produce a molded product with less formaldehyde generation and excellent appearance and weather resistance, and can suppress mold contamination during molding. DETAILED DESCRIPTION

[0023] Hereinafter, a mode for implementing the present disclosure (hereinafter referred to as "the present embodiment") will be described in detail. The present disclosure is not limited to the following description, and can be implemented in various modifications within the scope of the gist thereof.

[0024] [Polyacetal resin composition]

[0025] The polyacetal resin composition of the present embodiment comprises: 100 parts by mass of (A) polyacetal resin, and 0.1 parts by mass to 10 parts by mass of (B) aluminum pigment, wherein the (B) aluminum pigment contains 0.1% by mass to 2.0% by mass of particles having a particle size of 1 μm or less, relative to the total amount of the (B) aluminum pigment, and the volume average particle size of the (B) aluminum pigment is 3 μm to 40 μm.

[0026] ((A) Polyacetal resin)

[0027] As the (A) polyacetal resin in the present embodiment, there is no particular limitation, and conventionally known polyacetals can be used. The (A) polyacetal resin can be used alone or in combination of multiple types. As the above-mentioned (A) polyacetal resin, there can be listed: a polyoxymethylene homopolymer substantially composed of oxymethylene units -(CH2O)- obtained by homopolymerization of cyclic oligomers such as formaldehyde, trioxymethylene or tetraoxymethylene; or a polyoxymethylene copolymer having a structure in which oxyalkylene units (1) represented by the following general formula (1) are randomly inserted into a chain containing oxymethylene units -(CH2O)-, obtained by copolymerization of formaldehyde and / or trioxymethylene with cyclic ethers and / or cyclic formals, etc.

[0028]

[0029] (In the above formula (1), R1 and R2 are each independently a hydrogen atom, an alkyl group or an aryl group, R1 and R2 may be the same or different, and n is an integer of 2 to 6.)

[0030] The polyoxymethylene copolymer as an example of the (A) polyacetal resin used in the present embodiment includes a branched polyoxymethylene copolymer having branched molecular chains and a polyoxymethylene block copolymer containing 50% by mass or more of oxymethylene repeating units and blocked with a different component.

[0031] The insertion ratio of the oxyalkylene unit (1) represented by the general formula (1) in the polyoxymethylene copolymer is preferably 0.01 mol to 50 mol, more preferably 0.03 mol to 20 mol, per 100 mol of the oxymethylene unit.

[0032] The alkyl group in the general formula (1) is preferably a linear, branched or cyclic alkyl group having 1 to 3 carbon atoms, and more preferably a linear alkyl group having 1 to 2 carbon atoms. The aryl group in the general formula (1) is preferably an aryl group having 6 to 8 carbon atoms, and -C= or -C- in the aryl group having 6 to 8 carbon atoms may be substituted by N, S or O.

[0033] Examples of the oxyalkylene unit (1) represented by the general formula (1) include oxyethylene units, oxypropylene units, oxytetramethylene units, oxybutylene units, oxyphenylethylene units, etc. Among these oxyalkylene units (1), oxyethylene units are more preferred from the viewpoint of improving the physical properties of the polyacetal resin composition.

[0034] The (A) polyacetal resin obtained by the homopolymerization or copolymerization is preferably subjected to a terminal stabilization treatment. Examples of the terminal stabilization treatment method include esterification, etherification, urethanization, etc. of the terminal hydroxyl group, or stabilization of the terminal unstable part by hydrolysis.

[0035] The (A) polyacetal resin subjected to terminal stabilization treatment is obtained, for example, by continuously supplying a polyoxymethylene copolymer obtained by copolymerization of formaldehyde and / or trioxymethylene with a cyclic ether and / or cyclic formal to a counter-rotating non-intermeshing twin-screw extruder in which a step of stabilization treatment of the molecular terminal immediately after polymerization is carried out, a step of injecting water or alcohol or a mixture thereof in a molten state and kneading, and a step of devolatilizing the injected vapor of the hydroxyl-containing compound such as water and free formaldehyde are released, and treatment is carried out. In addition, when injecting water or alcohol or a mixture thereof and kneading is carried out, it is preferable to add an alkaline substance such as triethylamine as a pH adjuster.

[0036] In the present embodiment, the MFR (melt flow rate; according to ASTM D57E, temperature condition: 190°C) of the polyacetal resin (A) is preferably 2.5 g / 10 min to 40 g / 10 min, more preferably 3 g / 10 min to 30 g / 10 min. By adjusting the MFR within the above range, the balance between the mechanical properties of the resin composition, the thermal stability during retention molding, and the amount of formaldehyde generated becomes good.

[0037] The (A) polyacetal resin in the present embodiment is preferably a polyoxymethylene copolymer into which oxymethylene units are inserted. The insertion ratio of the oxymethylene units is preferably 0.01 mol to 50 mol, more preferably 0.03 mol to 20 mol, per 100 mol of the oxymethylene units.

[0038] <(A) Stabilizer contained in polyacetal resin>

[0039] In the present embodiment, the polyacetal resin (A) preferably contains a stabilizer used in conventional polyacetal resins. In the present embodiment, the polyacetal resin (A) is preferably a copolymer, and when the polyacetal resin (A) is a copolymer, it is more preferred that the polyacetal copolymer resin contains a stabilizer used in conventional polyacetal resins.

[0040] Examples of the stabilizer include antioxidants, scavengers for scavenging formaldehyde or formic acid, hindered amine stabilizers and ultraviolet absorbers that function as weathering stabilizers. These may be used alone, but a combination of two or more thereof is preferred because a high effect is achieved.

[0041] As the antioxidant, hindered phenol antioxidants are preferred, and examples thereof include n-octadecyl 3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, n-octadecyl 3-(3'-methyl-5'-tert-butyl-4'-hydroxyphenyl)propionate, n-tetradecyl 3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, 1,6-hexanediol di(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), 1,4-butanediol di(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), and triethylene glycol di(3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate).

[0042] Other hindered phenol antioxidants include, for example, tetrakis(methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate)methane, 3,9-bis(2-(3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, N,N'-bis[3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionyl] Hexamethylenediamine, N,N'-tetramethylenebis[3-(3'-methyl-5'-tert-butyl-4-hydroxyphenyl)propionyl]diamine, N,N'-bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hydrazine, N-salicyloyl-N'-salicylidenehydrazine, 3-(N-salicyloyl)amino-1,2,4-triazole, N,N'-bis(2-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy)ethyl)oxalyldiamine.

[0043] Among the above-mentioned hindered phenol antioxidants, triethylene glycol di(3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate) and tetrakis(methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate)methane are preferred.

[0044] In the present embodiment, the amount of the hindered phenol antioxidant added is preferably in the range of 0.01 to 2 parts by mass, more preferably 0.02 to 1 part by mass, relative to 100 parts by mass of the (A) polyacetal resin. When the amount added is in the range of 0.01 to 2 parts by mass, the thermal stability of the polyacetal resin composition of the present embodiment during molding can be improved, resulting in a good polyacetal resin composition.

[0045] The scavenger is preferably a compound having the ability to capture formaldehyde or formic acid, and examples thereof include compounds and polymers containing formaldehyde-reactive nitrogen, fatty acid calcium salts, and hydroxides, inorganic acid salts, carboxylates, or alkoxides of alkali metals or alkaline earth metals.

[0046] Examples of the compound containing formaldehyde-reactive nitrogen include dicyandiamide, amino-substituted triazine, and a co-condensate of amino-substituted triazine and formaldehyde.

[0047] Examples of the amino-substituted triazines include guanamine (2,4-diamino-s-triazine), melamine (2,4,6-triamino-s-triazine), N-butylmelamine, N-phenylmelamine, N,N-diphenylmelamine, N,N-diallylmelamine, N,N'N"-triphenylmelamine, N-methylolmelamine, N,N'-dimethylolmelamine, N,N',N"-trimethylolmelamine, and benzoguanamine (2,4-diamino-6-phenyl-s-triazine). In addition, 2,4-diamino-6-methyl-s-triazine, 2,4-diamino-6-butyl-s-triazine, 2,4-diamino-6-benzyloxy-s-triazine, 2,4-diamino-6-butoxy-s-triazine, 2,4-diamino-6-cyclohexyl-s-triazine, 2,4-diamino-6-chloro-s-triazine, 2,4-diamino-6-mercapto-s-triazine, 2,4-diamino-6-amino-s-triazine (ammeline), 2-hydroxy-4,6-diamino-s-triazine (ammeline), and N,N,N′,N′-tetracyanoethylphenylguanamine can be mentioned.

[0048] Examples of the co-condensate of the amino-substituted triazine and formaldehyde include melamine-formaldehyde polycondensates.

[0049] Among the various additives mentioned above, dicyandiamide, melamine and melamine-formaldehyde polycondensate are preferred.

[0050] As an example of the above-mentioned scavenger, the above-mentioned polymer having formaldehyde-reactive nitrogen includes, for example: (i) polyamide resin, (ii) polymers obtained by polymerizing acrylamide and its derivatives or acrylamide and its derivatives with other vinyl monomers in the presence of metal alkoxides, (iii) polymers obtained by polymerizing acrylamide and its derivatives or acrylamide and its derivatives with other vinyl monomers in the presence of a free radical polymerization initiator, and (iv) polymers containing nitrogen atoms such as amines, amides, ureas and carbamates.

[0051] Examples of the polyamide resin include nylon 4-6, nylon 6, nylon 6-6, nylon 6-10, nylon 6-12, nylon 12, and copolymers thereof such as nylon 6 / 6-6, nylon 6 / 6-6 / 6-10, and nylon 6 / 6-12.

[0052] Examples of the polymer obtained by polymerizing acrylamide and its derivatives or acrylamide and its derivatives with other vinyl monomers in the presence of a metal alkoxide include poly-β-alanine copolymers.

[0053] These polymers or copolymers can be produced by the methods described in Japanese Patent Publication No. 6-12259 (U.S. Patent No. 5,015,707), Japanese Patent Publication No. 5-87096, Japanese Patent Publication No. 5-47568, and Japanese Patent Application Laid-Open No. 3-234729.

[0054] The fatty acid calcium salt as an example of the scavenger includes, for example, a calcium salt of a saturated fatty acid or an unsaturated fatty acid having 10 to 36 carbon atoms, and the fatty acid calcium salt may be substituted with a hydroxyl group.

[0055] Examples of the saturated fatty acid include capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, and hexatricarboxylic acid.

[0056] Examples of the unsaturated fatty acid include undecylenic acid, oleic acid, elaidic acid, docosenoic acid, erucic acid, brassylic acid, sorbic acid, linoleic acid, linolenic acid, arachidonic acid, and stearic acid.

[0057] Among these fatty acids, palmitic acid, stearic acid, and 12-hydroxystearic acid are particularly preferred.

[0058] Examples of the alkali metal or alkaline earth metal hydroxide, inorganic acid salt, carboxylate or alkoxide as the scavenger include hydroxides of sodium, potassium, magnesium, calcium or barium, and carbonates, phosphates, silicates, borates and carboxylates of the metals.

[0059] It should be noted that the carboxylate salts do not include the above-mentioned fatty acid calcium salts.

[0060] Examples of the carboxylic acid corresponding to the carboxylate include saturated aliphatic carboxylic acids or unsaturated aliphatic carboxylic acids having 10 to 36 carbon atoms, and these carboxylic acids may be substituted with a hydroxyl group.

[0061] Examples of the saturated aliphatic carboxylic acid include capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, and hexatricarboxylic acid.

[0062] Examples of the unsaturated aliphatic carboxylic acid include undecylenic acid, oleic acid, elaidic acid, docosenoic acid, erucic acid, brassylic acid, sorbic acid, linoleic acid, linolenic acid, arachidonic acid, and stearic acid.

[0063] Examples of the alkoxide include methoxides and ethoxides of the above-mentioned metals.

[0064] In the present embodiment, the addition amount of the above-mentioned compound containing formaldehyde reactive nitrogen and polymer, fatty acid calcium salt, hydroxide of alkali metal or alkaline earth metal, inorganic acid salt, carboxylate or alkoxide as an example of the above-mentioned scavenger is preferably in the range of 0.01 to 1 parts by mass, and more preferably 0.02 to 0.5 parts by mass, relative to 100 parts by mass of the (A) polyacetal resin. When the addition amount is 0.01 to 1 parts by mass, the thermal stability of the polyacetal resin composition of the present embodiment during molding processing can be improved, the amount of formaldehyde generated from the molded body can be reduced, and the heat aging resistance becomes better.

[0065] Examples of the weathering stabilizer include hindered amine stabilizers and ultraviolet absorbers.

[0066] Examples of the hindered amine stabilizer include piperidine derivatives having a sterically hindered group, such as piperidine derivatives containing an ester group, piperidine derivatives containing an ether group, piperidine derivatives containing an amide group, and high molecular weight piperidine derivative polycondensates.

[0067] Examples of the ester group-containing piperidine derivative include 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-phenylcarbamoyloxy-2,2,6,6-tetramethylpiperidine, bis(2,2,6,6-tetramethyl-4-piperidyl)oxalate, bis(2,2,6,6-tetramethyl-4-piperidyl)malonate, bis(1,2,2,6,6-tetramethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate, bis(2,2,6,6-tetramethyl-4-piperidyl)adipate, Di(1,2,2,6,6-pentamethyl-4-piperidinyl) adipate, Di(1-methyl-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, Di(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, Di(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate Benzene-1,3,5-tricarboxylic acid tris(2,2,6,6-tetramethyl-4-piperidinyl) ester, 1,2,3,4-butanetetracarboxylic acid tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) ester, and the like.

[0068] Examples of the ether group-containing piperidine derivative include 4-methoxy-2,2,6,6-tetramethylpiperidine, 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6,6-tetramethylpiperidine, and 1,2-bis(2,2,6,6-tetramethyl-4-piperidinyloxy)ethane.

[0069] Examples of the amide group-containing piperidine derivative include 4-(phenylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine and hexamethylene-1,6-dicarbamic acid bis(2,2,6,6-tetramethyl-4-piperidinyl) ester.

[0070] In addition, examples of the high molecular weight piperidine derivative polycondensate include: dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, a condensate of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol and tridecanol, and a condensate of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol and β,β,β',β'-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5.5]undecane)diethanol.

[0071] The above-mentioned various hindered amine stabilizers may be used alone or in combination of two or more.

[0072] Among them, the preferred hindered amine stabilizers are di(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, di(N-methyl-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, di(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and the condensation product of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol and β,β,β',β'-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro(5.5)undecane)diethanol.

[0073] In the present embodiment, the content of the hindered amine stabilizer is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 2 parts by mass, and even more preferably 0.1 to 1.5 parts by mass, based on 100 parts by mass of the (A) polyacetal resin.

[0074] In the present embodiment, the polyacetal resin (A) preferably further contains an ultraviolet absorber as a weathering stabilizer. This can improve the weather resistance (light stability) of a molded article obtained from the polyacetal resin composition of the present embodiment.

[0075] Examples of the ultraviolet absorber include benzotriazole compounds, benzophenone compounds, oxalic acid anilide compounds, and hydroxyphenyl-1,3,5-triazine compounds.

[0076] Examples of the benzotriazole compounds include benzotriazoles having a hydroxyl group and an alkyl group (preferably an alkyl group having 1 to 6 carbon atoms) substituted aryl group, such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, and 2-(2'-hydroxy-3',5'-diisoamylphenyl)benzotriazole; benzotriazoles having a hydroxyl group and an aralkyl group or an aryl group substituted aryl group, such as 2-[2'-hydroxy-3',5'-bis(α,α-dimethylbenzyl)phenyl]benzotriazole; and benzotriazoles having a hydroxyl group and an alkoxy group (preferably an alkoxy group having 1 to 12 carbon atoms) substituted aryl group, such as 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole.

[0077] Preferred benzotriazole compounds are benzotriazoles having a hydroxyl group and an aryl group having 6 to 10 carbon atoms (particularly a phenyl group) substituted with an alkyl group having 3 to 6 carbon atoms, and benzotriazoles having a hydroxyl group and an aryl group having 6 to 10 carbon atoms-substituted with an alkyl group having 1 to 6 carbon atoms (particularly a phenyl group substituted with an alkyl group having 1 to 4 carbon atoms).

[0078] Examples of the benzophenone compounds include benzophenones having a plurality of hydroxyl groups and benzophenones having a hydroxyl group and an alkoxy group (preferably an alkoxy group having 1 to 16 carbon atoms).

[0079] Examples of benzophenones having a plurality of hydroxyl groups include di-, tri- or tetrahydroxybenzophenones such as 2,4-dihydroxybenzophenone and benzophenones having a hydroxyl group and a hydroxyl-substituted aryl group or arylalkyl group such as 2-hydroxy-4-benzyloxybenzophenone.

[0080] Examples of benzophenones having a hydroxyl group and an alkoxy group include 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, and 2-hydroxy-4-methoxy-5-sulfobenzophenone.

[0081] Examples of the oxalic acid anilide compounds include N-(2-ethylphenyl)-N′-(2-ethoxy-5-tert-butylphenyl) oxalic acid diamide and N-(2-ethylphenyl)-N′-(2-ethoxyphenyl) oxalic acid diamide.

[0082] Examples of the hydroxyphenyl-1,3,5-triazine compounds include 2,4-diphenyl-6-(2-hydroxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2,4-dihydroxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-methoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-ethoxyphenyl)-1,3,5-triazine, 2,4-diphenyl- 6-(2-hydroxy-4-propoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-dodecyloxyphenyl)-1,3,5-triazine.

[0083] Among the above-mentioned compounds as ultraviolet absorbers, benzotriazole compounds are preferred, and 2-[2′-hydroxy-3′,5′-bis(α,α-dimethylbenzyl)phenyl]benzotriazole is more preferred.

[0084] In the present embodiment, the amount of the ultraviolet absorber added is preferably 0.1 to 5 parts by mass, more preferably 0.1 to 2 parts by mass, and even more preferably 0.1 to 1.5 parts by mass, relative to 100 parts by mass of the (A) polyacetal resin.

[0085] When the polyacetal resin composition of the present embodiment contains an ultraviolet absorber and a hindered amine stabilizer, the ratio of the hindered amine stabilizer to the ultraviolet absorber is preferably in the range of 10 / 90 to 80 / 20, more preferably in the range of 10 / 90 to 70 / 30, and further preferably in the range of 20 / 80 to 60 / 40 in terms of ultraviolet absorber / hindered amine stabilizer (mass ratio).

[0086] ((B) Aluminum pigment)

[0087] The metal particles after the shape processing include fine particles contained in the original raw material metal powder and fine particles generated by crushing a part of the raw material metal powder during the processing of the raw material metal powder.

[0088] When the content of particularly small particles with a particle size of less than 1 μm among these particles, i.e., "particles with a particle size of less than 1 μm" (hereinafter referred to as specific particles) is high in the metal particles, the VOC properties of the resin material made by adding the metal particles deteriorate, and mold contamination tends to occur during molding.

[0089] On the other hand, a resin material prepared by adding metal particles from which specific fine particles are removed after the above-mentioned shape processing in order to avoid such adverse effects cannot obtain sufficient glossiness.

[0090] The polyacetal resin composition of the present embodiment is obtained by using the following methods: after removing the specific particles after the above-mentioned shape processing, a method of intentionally adding a specific amount of specific particles; or a method of removing a part of the contained specific particles after the above-mentioned shape processing, etc. By these methods, the amount of specific particles contained in the metal particles can be adjusted to 0.1 mass % to 2.0 mass %. Therefore, for the resin material made by adding metal particles intentionally containing a specified amount of specific particles, the deterioration of VOC properties can be suppressed, and mold contamination during molding can be suppressed. In addition, a molded product with good gloss can be obtained.

[0091] In the polyacetal resin composition of the present embodiment, the amount of the specific fine particles is 0.1 to 2.0 mass %, preferably 0.3 to 1.5 mass %, more preferably 0.4 to 1.2 mass %, particularly preferably 0.5 to 1.0 mass % of the entire aluminum pigment.

[0092] When the amount of the specific fine particles is equal to or greater than the above lower limit, the glossiness is excellent. In addition, when the amount of the specific fine particles is equal to or less than the above upper limit, the deterioration of the VOC property of the obtained molded product and the contamination of the mold during molding can be suppressed.

[0093] In the present embodiment, the (B) aluminum pigment preferably has particles containing aluminum as a main component, and more preferably consists only of particles containing aluminum. It should be noted that the "main component" refers to a total amount of 70% by mass or more relative to the (B) aluminum pigment. The particles have, for example, a flat shape such as a coin or a flake.

[0094] When the (B) aluminum pigment (particles constituting the aluminum pigment) has a flat shape, the volume average particle size (D 50 ) is 3 μm to 40 μm, and the average particle thickness of the (B) aluminum pigment (particles constituting the aluminum pigment) is preferably 0.03 μm to 0.4 μm, and the average particle thickness is more preferably 0.08 μm to 0.4 μm. The (B) aluminum pigment can be used alone or in combination of two or more.

[0095] In this embodiment, the (B) aluminum pigment preferably has an appropriate oxide film on its surface. By having an appropriate oxide film, the high reflectivity unique to aluminum can be maintained, and the corrosion resistance and temporal stability of the metal particles can be maintained.

[0096] In addition, there is no particular restriction on the purity of the aluminum pigment (B), and other metals may be contained as impurities or alloy components as long as they do not hinder the effects of the present disclosure. Examples of impurities or alloy components include Si, Fe, Cu, Mn, Mg, Zn, etc. For example, relative to the total amount of the aluminum pigment (B), it is preferred that 70% to 95% by mass of aluminum is contained, and more preferably 78% to 92% by mass of aluminum is contained.

[0097] (B) Aluminum pigments are obtained, for example, by pre-classifying atomized powder, cutting powder, foil powder, vapor-deposited powder, or metal powder obtained by other methods by primary classification, wet-crushing the powder using a ball mill, a grinder, a planetary mill, a vibration mill, etc. in the presence of a processing medium including a processing aid and a solvent, sieving and classifying the powder in a wet state, and then performing solid-liquid separation using a filter press, etc. Thus, metal particles having a small number of concavo-convex fracture surfaces at the ends of the flakes can be produced.

[0098] Regarding the pulverizing medium used here, if an excessive amount is added, the oxygen content in the particles increases, so it is preferably as small as possible.

[0099] In the present embodiment, the shape of the aluminum pigment (B) is preferably a flat shape such as a coin or flake shape. The flat shape referred to herein refers to an average shape ratio [average particle thickness t / volume average particle diameter D 50 The value of ] is preferably 0.2 or less, more preferably 0.1 or less, and further preferably 0.05 or less. By adjusting the average aspect ratio within this range, the surface area of ​​the portion having a high reflectivity peculiar to the metal can be increased by adding a small amount of metal particles, so the brightness of the molded body can be effectively improved by a small amount of addition.

[0100] In the present embodiment, the content of the (B) aluminum pigment is 0.1 to 10 parts by mass, preferably 1 to 8 parts by mass, more preferably 1.5 to 7 parts by mass, and particularly preferably 2 to 6 parts by mass, based on 100 parts by mass of the polyacetal resin.

[0101] By adjusting the content of the aluminum pigment within the above range, the molded article of the resin composition of the present embodiment can better maintain rigidity and impact resistance, which are mechanical properties inherent to polyacetal resin, and can suppress the generation of formaldehyde and exhibit good gloss.

[0102] In this embodiment, (B) the volume average particle size (D 50) is 3 μm to 40 μm, preferably 4 μm to 35 μm, and more preferably 5 μm to 30 μm. When the volume average particle size of the aluminum pigment is in the range of 15 μm to 30 μm, the effect of inhibiting the generation of formaldehyde and improving the glossiness is particularly good, so it is particularly preferred. When the volume average particle size is in the range of 5 μm to 15 μm, the effect of improving weather resistance is particularly good, so it is particularly preferred. It should be noted that the volume average particle size (D 50 ) and the average particle thickness can be measured by the method described in the examples described later.

[0103] ((C) Lubricant)

[0104] The polyacetal resin composition of the present embodiment preferably further contains one or more (C) lubricants. Lubricants generally refer to substances that reduce the viscosity of the resin melt and help improve the demolding properties from the metal surface during molding. In the present embodiment, by adding the (C) lubricant, in addition to these functions and effects, a higher glossiness is obtained. These (C) lubricants can be used alone or in combination of multiple types.

[0105] The lubricant (C) in this embodiment is not limited to the following examples, and examples thereof include hydrocarbons, higher fatty acids, higher alcohols, aliphatic amides, metal soaps, etc. Among them, liquid paraffin is preferred as a hydrocarbon lubricant from the viewpoint of low reactivity with the polyacetal resin (A) and little influence on physical properties.

[0106] The amount of the lubricant (C) added in this embodiment is not particularly limited as long as it is within the range that does not hinder extrusion and injection molding. For example, it is preferably 0.01 to 0.5 parts by mass, more preferably 0.05 to 0.45 parts by mass, and particularly preferably 0.1 to 0.4 parts by mass relative to 100 parts by mass of the polyacetal resin (A). When the amount of the lubricant (C) added is within the above range, a molded body with high gloss can be obtained, and the extruder operation state during extrusion and the resin metering during injection molding become stable, which is preferred.

[0107] ((D) Formaldehyde inhibitor)

[0108] The polyacetal resin composition of the present embodiment preferably further contains one or more (D) formaldehyde inhibitors. Examples of the (D) formaldehyde inhibitors include aminotriazine compounds, guanamine compounds, urea compounds, and carboxylic acid hydrazide compounds. These (D) formaldehyde inhibitors may be used alone or in combination.

[0109] Examples of the aminotriazine compounds include melamine; melamine condensates such as melam, melem, and cyanocyanocyanamide; melamine resins such as melamine-formaldehyde resins; N-hydroxyarylalkylmelamine compounds such as N,N',N"-mono-, di-, tri-, tetra-, penta- or hexa-(o-, m- or p-hydroxyphenylmethyl)melamine; and the like.

[0110] Examples of the guanamine compounds include aliphatic guanamine compounds such as amylguanamine, hexylguanamine, heptylguanamine, octylguanamine, and stearylguanamine; alkylene biguanamines such as ethylenebiguanamine, propylenebiguanamine, butylenebiguanamine, amylenebiguanamine, hexylenebiguanamine, heptylenebiguanamine, and octylenebiguanamine; alicyclic guanamine compounds such as cyclohexylguanamine, norbornenylguanamine, cyclohexenylguanamine, norbornylguanamine, and functional group-substituted derivatives thereof; phenylguanamine, α- or β-naphthylguanamine and their functional group substituted derivatives and other aromatic guanamine compounds; o-phenyldiguanamine, m-phenyldiguanamine, p-phenyldiguanamine, naphthalenediguanamine, biphenyldiguanamine and other polyguanamines; phenylethylguanamine, β-phenylpropylguanamine, o-, m- or p-phenylenediamine, etc. aralkyl or aralkylene guanamines; guanamine compounds containing heteroatoms such as guanamines containing acetal groups, guanamines containing dioxane rings, guanamines containing tetraoxaspiro rings, guanamines containing isocyanuric acid rings, etc.; etc.

[0111] Examples of the functional group-substituted derivatives of the alicyclic guanamine compounds include derivatives in which the cycloalkane residue is substituted with one to three functional groups such as alkyl, hydroxyl, amino, acetylamino, nitrile, carboxyl, alkoxycarbonyl, carbamoyl, alkoxy, phenyl, cumyl, and hydroxyphenyl.

[0112] In addition, examples of the functional group-substituted derivatives of the aromatic guanamine compounds include derivatives in which the phenyl residue of benzoguanamine or the naphthyl residue of naphthylguanamine is substituted with one to five functional groups such as alkyl, hydroxyl, amino, acetylamino, nitrile, carboxyl, alkoxycarbonyl, carbamoyl, alkoxy, phenyl, cumyl, hydroxyphenyl, etc. Examples of such aromatic guanamine compounds include o-, m- or p-tolylguanamine, o-, m- or p-xylylguanamine, o-, m- or p-phenylphenylguanamine, o-, m- or p-hydroxyphenylguanamine, 4-(4′-hydroxyphenyl)phenylguanamine, o-, m- or p-nitrilephenylguanamine, 3,5-dimethyl-4-hydroxyphenylguanamine, and 3,5-di-tert-butyl-4-hydroxyphenylguanamine.

[0113] Examples of the acetal group-containing guanamines include 2,4-diamino-6-(3,3-dimethoxypropyl)-s-triazine and the like.

[0114] Examples of the dioxane ring-containing guanamines include [2-(4',6'-diamino-s-triazine-2'-yl)ethyl]-1,3-dioxane and [2-(4',6'-diamino-s-triazine-2'-yl)ethyl]-4-ethyl-4-hydroxymethyl-1,3-dioxane.

[0115] Examples of the tetraoxaspiro ring-containing guanamines include CTU-guanamine and CMTU-guanamine.

[0116] Examples of the isocyanuric acid ring-containing guanamines include 1,3,5-tris[2-(4',6'-diamino-s-triazine-2'-yl)ethyl]isocyanurate and 1,3,5-tris[3-(4',6'-diamino-s-triazine-2'-yl)propyl]isocyanurate.

[0117] Examples of the urea compound include chain urea compounds and cyclic urea compounds.

[0118] Examples of the chain urea compound include condensates of urea and formaldehyde such as biuret, biuret, and urea formaldehyde, and polyalkylene or arylene ureas such as polynonamethylene urea.

[0119] Examples of the cyclic urea compounds include hydantoins, 2-butylidene diurea, acetylene urea, mono-, di-, tri- or tetra-alkoxymethyl glycolurils such as mono-, di-, tri- or tetra-methoxymethyl glycolurils, cyanuric acid, isocyanuric acid, uric acid and ureaazole. Examples of the hydantoins include hydantoin, 5-methylhydantoin, 5-ethylhydantoin, 5-isopropylhydantoin, 5-phenylhydantoin, 5-benzylhydantoin, 5,5-dimethylhydantoin, 5,5-pentamethylenehydantoin, 5-methyl-5-phenylhydantoin, 5,5-diphenylhydantoin, 5-(o-, m- or p-hydroxyphenyl)hydantoin, 5-(o-, m- or p-aminophenyl)hydantoin, allantoin, 5-methylalantoin, and metal salts of aluminum salts of allantoin such as dihydroxyaluminum salt of allantoin.

[0120] Examples of the carboxylic acid hydrazide compound include aliphatic carboxylic acid hydrazide compounds, alicyclic carboxylic acid hydrazide compounds, and aromatic carboxylic acid hydrazide compounds.

[0121] Examples of the aliphatic carboxylic acid hydrazide compounds include monocarboxylic acid hydrazides such as lauric acid hydrazide, stearic acid hydrazide, 12-hydroxystearic acid hydrazide, and 1,2,3,4-butanetetracarboxylic acid hydrazide; and polycarboxylic acid hydrazides such as succinic acid monohydrazide or dihydrazide, glutaric acid monohydrazide or dihydrazide, adipic acid monohydrazide or dihydrazide, pimelic acid monohydrazide or dihydrazide, suberic acid monohydrazide or dihydrazide, azelaic acid monohydrazide or dihydrazide, sebacic acid monohydrazide or dihydrazide, dodecanedioic acid monohydrazide or dihydrazide, hexadecanedioic acid monohydrazide or dihydrazide, eicosanedioic acid monohydrazide or dihydrazide, and 7,11-octadecadiene-1,18-dicarboxylic acid hydrazide.

[0122] Examples of the alicyclic carboxylic acid hydrazide compounds include monocarboxylic acid hydrazides such as cyclohexanecarboxylic acid hydrazides, and polycarboxylic acid hydrazides such as dimer acid mono- or dihydrazides, trimer acid mono-, di- or trihydrazides, 1,2-, 1,3- or 1,4-cyclohexanedicarboxylic acid mono- or dihydrazides, and cyclohexanetricarboxylic acid mono-, di- or trihydrazides.

[0123] Examples of the aromatic carboxylic acid hydrazide compounds include monocarboxylic acid hydrazides such as benzoic acid hydrazide and its functional group substituted derivatives, α- or β-naphthoic acid hydrazide and its functional group substituted derivatives; isophthalic acid monohydrazide or dihydrazide, terephthalic acid monohydrazide or dihydrazide, 1,4- or 2,6-naphthalene dicarboxylic acid monohydrazide or dihydrazide, 3,3'-, 3,4'- or 4,4'-biphenyl dicarboxylic acid monohydrazide or dihydrazide, diphenyl ether dicarboxylic acid monohydrazide or dihydrazide, diphenylmethane dicarboxylic acid monohydrazide or dihydrazide. Mono- or dihydrazide, diphenylethanedicarboxylic acid mono- or dihydrazide, diphenoxyethanedicarboxylic acid mono- or dihydrazide, diphenylsulfonedicarboxylic acid mono- or dihydrazide, diphenylketonedicarboxylic acid mono- or dihydrazide, 4,4"-terphenyldicarboxylic acid mono- or dihydrazide, 4,4"'-tetraphenyldicarboxylic acid mono- or dihydrazide, 1,2,4-benzenetricarboxylic acid mono-, di- or trihydrazide, pyromellitic acid mono-, di-, tri- or tetrahydrazide, 1,4,5,8-naphthalenetetracarboxylic acid mono-, di-, tri- or tetrahydrazide and other polycarboxylic acid hydrazides, etc.

[0124] Examples of the benzoic acid hydrazide and its functional group-substituted derivatives include derivatives in which the phenyl residue of benzoic acid hydrazide is substituted with one to five functional groups such as alkyl groups, hydroxyl groups, acetoxy groups, amino groups, acetylamino groups, nitrile groups, carboxyl groups, alkoxycarbonyl groups, carbamoyl groups, alkoxy groups, phenyl groups, benzyl groups, cumyl groups, and hydroxyphenyl groups, such as o-, m- or p-methylbenzoic acid hydrazide, 2,4-, 3,4-, 3,5- or 2,5-dimethylbenzoic acid hydrazide, o-, m- or p-hydroxybenzoic acid hydrazide, 4-hydroxy-3-phenylbenzoic acid hydrazide, 4-acetoxy-3-phenylbenzoic acid hydrazide, 4-phenylbenzoic acid hydrazide, 4-(4'-phenyl)benzoic acid hydrazide, 4-hydroxy-3,5-dimethylbenzoic acid hydrazide, and 4-hydroxy-3,5-di-tert-butylbenzoic acid hydrazide.

[0125] Examples of the α- or β-naphthoic acid hydrazide and functional group-substituted derivatives thereof include 3-hydroxy-2-naphthoic acid hydrazide and 6-hydroxy-2-naphthoic acid hydrazide.

[0126] It should be noted that the above-mentioned (D) formaldehyde inhibitor can also be used in the form of being supported on a layered material or a porous material (hydrotalcite, montmorillonite, silica gel, alumina, titanium dioxide, zirconium dioxide, sepiolite, smectite, palygorskite, imogolite, zeolite, activated carbon, etc.).

[0127] As the formaldehyde inhibitor (D) used in the polyacetal resin composition of the present embodiment, aliphatic carboxylic acid hydrazide compounds and aromatic carboxylic acid hydrazide compounds are preferred, and aliphatic carboxylic acid hydrazide compounds are particularly preferred.

[0128] The content of the formaldehyde inhibitor (D) in the polyacetal resin composition of the present embodiment is preferably 0.01 to 5 parts by mass, more preferably 0.01 to 2 parts by mass, and even more preferably 0.02 to 1 part by mass relative to 100 parts by mass of the polyacetal resin (A). When the amount of the formaldehyde inhibitor (D) added is within the above range, sufficient formaldehyde inhibition effect can be obtained and mold deposit can be inhibited, which is preferred.

[0129] (Other ingredients)

[0130] The polyacetal resin composition of the present embodiment may contain various colorants as complementary color pigments as needed to further improve the appearance design. Examples of colorants include organic pigments and inorganic pigments, and there are no particular restrictions, and the colorants may be one or a combination of two or more.

[0131] Examples of the organic pigments include phthalocyanine pigments, condensed azo pigments, azo lake pigments, quinacridone pigments, diazine pigments, Oxazine pigments, isoindolinone pigments, condensed polycyclic pigments, etc.

[0132] Examples of the inorganic pigments include simple oxides such as zinc flower, titanium dioxide, red iron oxide, chromium oxide, and iron black; sulfides such as cadmium yellow, cadmium orange, and cadmium red; chromates such as chrome yellow, zinc yellow, and chrome vermilion; ferrocyanides such as iron blue; silicates such as ultramarine; carbon black, and mica-based pearlescent pigments.

[0133] The amount of the colorant added is preferably 0.0001 to 2 parts by mass, more preferably 0.0005 to 1 part by mass, relative to 100 parts by mass of the polyacetal resin (A). By setting the amount of the colorant added within the above range, the effect of improving the appearance design can be obtained without increasing the reduction in the mechanical strength of the molded body, especially the generation of formaldehyde by the polyacetal resin (A).

[0134] Furthermore, the polyacetal resin composition of the present embodiment may contain various inorganic fillers, other thermoplastic resins, softeners, crystal nucleating agents, release agents, and the like that have been conventionally used as needed within a range that does not impair the purpose of the present disclosure.

[0135] (Manufacturing method)

[0136] The polyacetal resin composition of the present embodiment can be obtained, for example, by melting and mixing a part of the above-mentioned raw materials using a commonly used melt-kneading machine, such as a kneader, a roll mill, a single-screw extruder, a twin-screw extruder, and a multi-screw extruder.

[0137] In the case of manufacturing the polyacetal resin composition of the present embodiment by melt-kneading, the temperature of the melt-kneading can be selected according to the melting point or softening point of the (A) polyacetal resin used. The temperature of the above-mentioned melt-kneading is preferably a temperature of 1°C to 100°C higher than the melting point or softening point of the (A) polyacetal resin, more preferably a temperature of 10°C to 60°C higher than the melting point or softening point of the (A) polyacetal resin, and further preferably a temperature of 20°C to 50°C higher than the melting point or softening point of the (A) polyacetal resin. The melting point or softening point of the (A) polyacetal resin can be obtained by differential scanning calorimetry (DSC) according to JIS K7121. In addition, in order to maintain quality and working environment, it is preferred to replace the system with an inert gas or degas using one or more exhaust ports.

[0138] When the (A) polyacetal resin is in a granular form, in order to uniformly maintain the dispersion state of each component including the (B) aluminum pigment in the (A) polyacetal resin, it is preferred to use a spreading agent as needed and add a stabilizer (antioxidant, formaldehyde or formic acid scavenger and weathering stabilizer, (D) formaldehyde inhibitor, etc.) in advance and then mix, then mix (B) aluminum pigment and (C) lubricant as needed, and then melt-knead.

[0139] In addition, when the (A) polyacetal resin is in a granular form, it is preferred that a part or all of the particles are crushed to form a powder, and a spreader is used as needed to mix a stabilizer (antioxidant, formaldehyde or formic acid scavenger and weather stabilizer, (D) formaldehyde inhibitor, etc.) with the powdered (A) polyacetal resin, and then (B) an aluminum pigment and (C) a lubricant as needed are mixed, followed by melt kneading.

[0140] Examples of the spreading agent include aliphatic hydrocarbons, aromatic hydrocarbons, modified products thereof, mixtures thereof (mineral oils, etc.), fatty acid esters of polyols, etc. In order to prevent damage to the (B) aluminum pigment in the blending step, it is preferably blended in a later step.

[0141] In addition, when manufacturing the polyacetal resin composition of the present embodiment, the (A) polyacetal resin and the stabilizer (selected from at least one of an antioxidant, a formaldehyde or formic acid scavenger, and a weathering stabilizer) may also be pre-melted and kneaded. A commonly used melt-kneading machine can be used for the pre-kneading. The temperature of the melt-kneading is selected according to the melting point or softening point of the (A) polyacetal resin used. The temperature of the melt-kneading is preferably 1°C to 100°C higher than the melting point or softening point of the (A) polyacetal resin, more preferably 10°C to 60°C higher than the melting point or softening point of the (A) polyacetal resin, and further preferably 20°C to 50°C higher than the melting point or softening point of the (A) polyacetal resin. As a melt-kneading machine, for example, a kneader, a roller mill, a single-screw extruder, a twin-screw extruder, and a multi-screw extruder can be cited. In order to maintain the quality and the working environment, it is preferred to replace the system with an inert gas or to degas using one or more exhaust ports.

[0142] (Molding body)

[0143] A molded product can be produced by molding the polyacetal resin composition of the present embodiment.

[0144] As a method for producing the above-mentioned molded body, known molding methods can be cited, for example: extrusion molding, injection molding, vacuum molding, blow molding, injection compression molding, decorative molding, gas-assisted injection molding, foam injection molding, low-pressure molding, ultra-thin wall injection molding (ultra-high-speed injection molding), in-mold composite molding (insert molding, substrate injection molding), etc. In particular, injection molding, injection compression molding, and a molding method combining these with in-mold composite molding are preferred from the viewpoints of quality, production stability, and economy.

[0145] Furthermore, by bonding the polyacetal resin composition of the present embodiment with various resins including rubber and / or elastomer (using methods such as ultrasonic bonding, high frequency bonding, hot plate bonding, hot press molding, multilayer injection molding, and multilayer blow molding), a molded product having two or more layers with desired characteristics and appearance can be manufactured. Thus, excellent properties (impact resistance, sliding properties, chemical resistance, etc.) can be imparted to each resin, and a molded product having an appearance with excellent design properties can be obtained.

[0146] (characteristic)

[0147] The amount of formaldehyde generated by the polyacetal resin composition of the present embodiment is preferably 3 mg / kg or less, more preferably 2.5 mg / kg or less.

[0148] In addition, the amount of formaldehyde generation can be measured by the method described in Examples described later.

[0149] The glossiness of the polyacetal resin composition of the present embodiment immediately after injection molding is preferably 60 or more, more preferably 70 or more.

[0150] (use)

[0151] The molded article of the polyacetal resin composition of the present embodiment can be used for interior and exterior parts with a mechanism part or a sliding part. For example, it can be used as any one of the parts selected from the group consisting of components possessed by office automation equipment, music / image or information equipment or communication equipment, industrial components possessed by office furniture or residential equipment, and automotive interior and exterior parts. In particular, it can be used as any one of the parts selected from the group consisting of handles, switches and buttons that require excellent appearance. In addition, in order to use the molded article obtained by the resin composition of the present embodiment as an appearance part, by using an embossing mold during molding or embossing the molded article to give the appearance design surface, the improvement effect of the appearance is shown, so it is preferred.

[0152] According to the polyacetal resin composition of the present embodiment, a molded product having gloss and less formaldehyde and good weather resistance can be obtained even if the surface is not processed by plating or coating. In addition, the molded product obtained by the polyacetal resin composition of the present embodiment has good appearance characteristics as described above, so it also has a good appearance in practice even if it is not coated. Therefore, an appearance with excellent appearance design can be effectively obtained without using a solvent. In addition, the polyacetal resin composition of the present embodiment has excellent production stability, can be manufactured under a good operating environment, and is also excellent in terms of cost and environment.

[0153] [Example]

[0154] Hereinafter, the present disclosure will be specifically described by way of examples, but the present disclosure is not limited to the examples described below. Hereinafter, raw material components used in the examples and comparative examples are shown.

[0155] <(A) Polyacetal resin>

[0156] As the polyacetal copolymer (a-1), "Tenac C 4513 (melting point 165° C.)" (manufactured by Asahi Kasei Corporation) was used.

[0157] <(B) Aluminum Pigments>

[0158] Aluminum particles obtained by the following method were used as aluminum pigments (b-1) to (b-6).

[0159] - Preparation of aluminum pigment (b-1) -

[0160] A ball mill with an inner diameter of 30 cm and a length of 35 cm was filled with a mixture of 250 g of atomized aluminum powder (volume average particle size: 3.2 μm), 1.2 kg of mineral spirits and 25 g of stearic acid, and the mixture was ground at 60 rpm for 10 hours using 15 kg of glass beads with a diameter of 3 mm (specific gravity: 2.6). After the grinding, the slurry in the mill was washed with mineral spirits and flowed out, and loaded onto a 400-mesh vibrating screen. The slurry that passed was allowed to stand for 30 minutes to separate the precipitate and the liquid phase, thereby obtaining a precipitate. Two volumes of mineral spirits were added to the precipitate, stirred and mixed, and allowed to stand for 30 minutes, and then the operation of separating the precipitate and the liquid phase was repeated 10 times to obtain an aluminum pigment precursor (b'-1).

[0161] -Preparation of aluminum particles (b'-0)-

[0162] 250 g of atomized aluminum powder (volume average particle size: 3.2 μm) was ground at 60 rpm for 20 hours using 15 kg of glass beads (specific gravity: 2.6) with an inner diameter of 30 cm and a length of 35 cm. The pulverized material was then classified using a cyclone classifier to obtain aluminum particles (b'-0) with a particle size of 1 μm or less (specifically, an average particle size of 0.5 μm) as specific particles.

[0163] The above-mentioned aluminum particles (b'-0) are added to the above-mentioned aluminum pigment precursor (b'-1) so that the aluminum particles (b'-0) account for 1% by mass of the entire aluminum pigment, and then 2 times the volume of mineral spirits are added. After stirring and mixing, the mixture is allowed to stand for 30 minutes to separate the precipitate and the liquid phase, and then filtered with a filter and concentrated to obtain an aluminum pigment (b-1) with a heating residue of 90%.

[0164] The particle size distribution of the obtained aluminum pigment (b-1) was measured using a laser diffraction particle size distribution measuring device (manufactured by Shimadzu Corporation, trade name "SALD-2300"), and the volume average particle size D of the aluminum pigment was calculated from the 50% value of the obtained particle size distribution. 50 Using mineral spirits as the measurement solvent, the aluminum pigment as the sample was ultrasonically dispersed for 3 minutes as a pretreatment. Result D 50 =10 μm. The average particle size of the aluminum fine particles (b′-0) was also measured by a laser diffraction particle size distribution analyzer (manufactured by Shimadzu Corporation, trade name “SALD-2300”).

[0165] - Preparation of aluminum pigments (b-2) to (b-3) -

[0166] Aluminum pigments (b-2) to (b-3) were prepared by performing the same operation as the aluminum pigment (b-1) and changing the amount of aluminum fine particles (b'-0) having a particle size of 1 μm or less (average particle size of 0.5 μm) added to the aluminum pigment precursor (b'-1), thereby obtaining aluminum pigments having different amounts of fine particles.

[0167] Aluminum pigment (b-2): D 50 =10 μm, and the aluminum fine particles (b′-0) account for 0.5% by mass of the entire aluminum pigment (b-2).

[0168] Aluminum pigment (b-3): D 50 =10 μm, and the aluminum fine particles (b′-0) account for 3.0% by mass of the entire aluminum pigment (b-3).

[0169] - Preparation of aluminum pigments (b-4) to (b-6) -

[0170] Aluminum pigments (b-4) to (b-6) were obtained by performing the same operation as the aluminum pigment (b-1) above, but changing the particle size of the atomized aluminum powder and the pulverization time, thereby obtaining aluminum pigments having different volume average particle sizes.

[0171] Aluminum pigment (b-4): D 50 = 6 μm, and the aluminum fine particles (b'-0) account for 1.0 mass % of the entire aluminum pigment.

[0172] Aluminum pigment (b-5): D 50 = 23 μm, and the aluminum fine particles (b′-0) account for 1.0 mass % of the entire aluminum pigment.

[0173] Aluminum pigment (b-6): D 50 =45 μm, and the aluminum fine particles (b'-0) account for 1.0 mass % of the entire aluminum pigment.

[0174] -Preparation of aluminum pigment (b-0)-

[0175] In addition, an aluminum pigment precursor (b'-1) was obtained by the same operation as the preparation method of the above aluminum pigment (b-1), and then 2 volumes of mineral spirits were added, stirred and mixed, and then left to stand for 30 minutes, and the precipitate and the liquid phase were separated, and then filtered with a filter and concentrated, thereby obtaining an aluminum pigment (b-0) with a heating residue of 90%. 50 =10 μm, and aluminum fine particles having a particle size of 1 μm or less, which are specific fine particles, were not detected.

[0176] <(C) Lubricant>

[0177] Liquid paraffin (c-1): trade name "Sumoil PS-260" (manufactured by Matsumura Petroleum Research Institute)

[0178] <(D) Formaldehyde Inhibitor>

[0179] Formaldehyde inhibitor (d-1): Sebacic acid dihydrazide (manufactured by Nippon Fine Chemicals Co., Ltd.)

[0180] Formaldehyde inhibitor (d-2): adipic acid dihydrazide (manufactured by Nippon Fine Chemicals Co., Ltd.)

[0181] Formaldehyde inhibitor (d-3): dodecanedioic acid dihydrazide (manufactured by Nippon Fine Chemicals Co., Ltd.)

[0182] <(2) Evaluation method>

[0183] <Confirming the occurrence of mold contamination (MD)>

[0184] The pellets produced in the examples and comparative examples described below were molded using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., trade name "IS-100GN") under the conditions of a barrel temperature of 220° C., an injection time of 15 seconds, a cooling time of 20 seconds, and a mold temperature of 77° C. to produce test pieces. The test pieces were produced using a mold having a length of 130 mm, a width of 110 mm, and a thickness of 3 mm.

[0185] The MD (mold deposit) in this evaluation refers to the MD (mold deposit) generated by the additives contained in the pellets and the fine particles in the aluminum pigment adhering to the surface of the test piece. The case where the generation of MD from the test piece to the mold surface cannot be confirmed by visual observation is judged as ◎, and the area of ​​the generated MD is less than 5mm. 2 The case is judged as ○, and the area of ​​the generated MD is greater than or equal to 5mm 2 And less than 10mm 2 The case is judged as △, and the area of ​​the generated MD is 10mm 2 The above situation is judged as ×.

[0186] <Measurement of brightness>

[0187] The pellets prepared in the examples and comparative examples described later were dried at 80°C for 3 hours, and then a 100 mm × 100 mm, 3 mm thick flat test piece was prepared using a 5 ounce molding machine (manufactured by Toshiba Machine Co., Ltd., trade name "IS-100GN") with a barrel temperature set to 200°C at a mold temperature of 77°C and a cooling time of 20 seconds.

[0188] The L* value at 25° was measured for the test piece using a multi-angle digital gloss meter (CM-512m3A: manufactured by Konica Minolta, Inc.).

[0189] <Weather resistance>

[0190] The pellets prepared in the examples and comparative examples described later were dried at 80° C. for 3 hours and then molded using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., trade name “IS-100GN”) under the conditions of a barrel temperature of 220° C., an injection time of 15 seconds, a cooling time of 20 seconds, and a mold temperature of 77° C., thereby preparing a test piece. The test piece was prepared using a mold having a length of 100 mm, a width of 100 mm, and a thickness of 3 mm.

[0191] The test piece was irradiated vertically with a 6-watt portable UV lamp (manufactured by UVP. LLC, trade name "UVM-57") from a distance of 150 mm in a dark room.

[0192] After irradiation was continued for 10 days, the L* value at 25° was measured by the same method as the above-mentioned measurement of brightness, and compared with the value immediately after the above-mentioned test piece was prepared.

[0193] <Glossiness>

[0194] The pellets produced in the examples and comparative examples described below were molded using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., trade name "IS-100GN") under the conditions of a barrel temperature of 220° C., an injection time of 15 seconds, a cooling time of 20 seconds, and a mold temperature of 77° C. to produce test pieces. The test pieces were produced using a mold having a length of 90 mm, a width of 50 mm, and a thickness of 2.5 mm.

[0195] The glossiness of the molded article was measured at an angle of 60° on the surface of the molded article using the test piece and a gloss meter IG-320 manufactured by Horiba, Ltd. in accordance with JIS Z8741.

[0196] It is generally believed that the higher the glossiness, the smoother the surface of the molded product and the higher the degree of conformity to the mold surface. The glossiness of the molded product was measured immediately after the molded product was obtained by injection molding and after the molded product was left to stand for 48 hours in a high temperature constant humidity machine "PL-2KT" manufactured by ESPEC CORP. at a temperature of 80°C and a humidity of 90%.

[0197] <Formaldehyde generation (VDA275)>

[0198] The pellets produced in the examples and comparative examples described below were molded using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., trade name "IS-100GN") under the conditions of a cylinder temperature of 220°C, an injection time of 15 seconds, a cooling time of 20 seconds, and a mold temperature of 77°C to produce test pieces.

[0199] Next, the amount of formaldehyde released from the test piece was determined by the following method (VDA275 method).

[0200] First, 50 mL of distilled water and a test piece (100 mm in length × 40 mm in width × 3 mm in thickness) were added to a 500 mL polyethylene container and sealed, and heated at 60°C for 3 hours. Then, formaldehyde in distilled water was reacted with acetylacetone in the presence of ammonium ions. The absorption peak of the reaction product at a wavelength of 412 nm was measured using a UV spectrometer, and the amount of formaldehyde generated (mg / kg) was determined.

[0201] <Preparation and Evaluation Results of Polyacetal Resin Composition>

[0202] [Example 1]

[0203] 100 parts by mass of polyacetal copolymer (a-1) and 0.08 parts by mass of sebacic acid dihydrazide (d-1) were mixed in a mixer, and then 3.0 parts by mass of aluminum pigment (b-1) were added and mixed. Using a single screw extruder with a 30 mm exhaust port, the mixture was melt-kneaded (melt-mixed) while degassing from the exhaust port under the conditions of a set temperature of 200°C, a rotation speed of 80 rpm, and a discharge volume of 10 kg / hour, thereby obtaining pellets. The obtained pellets were dried at 80°C for 3 hours, and then the above-mentioned evaluations were performed. The composition ratio and the evaluation results are shown in Table 1 below.

[0204] [Examples 2 to 12, 17 to 20, Comparative Examples 1 to 6, 9 to 11]

[0205] Compositions were prepared and evaluated in the same manner as in Example 1 except that (A) the polyacetal resin, (B) the aluminum pigment, and (D) the formaldehyde inhibitor were adjusted to the compositions shown in Table 1. The composition ratios and evaluation results are shown in Table 1 below.

[0206] [Example 13]

[0207] 100 parts by mass of polyacetal copolymer (a-1), 0.30 parts by mass of liquid paraffin (c-1), and 0.08 parts by mass of sebacic acid dihydrazide (d-1) were mixed in a mixer, and then 3.0 parts by mass of aluminum pigment (b-1) were added and mixed. The mixture was melt-kneaded (melt-mixed) while degassing from the exhaust port using a single screw extruder with a 30 mm exhaust port at a set temperature of 200°C, a rotation speed of 80 rpm, and a discharge volume of 10 kg / hour, thereby obtaining pellets. The obtained pellets were dried at 80°C for 3 hours, and then the above-mentioned evaluations were performed. The composition ratio and evaluation results are shown in Table 1 below.

[0208] [Examples 14 to 16, Comparative Examples 7, 8, and 12]

[0209] The same procedure as in Example 13 was carried out except that the (A) polyacetal resin, (B) aluminum pigment, (C) lubricant, and (D) formaldehyde inhibitor were adjusted to the compositions shown in Table 1. The composition ratios and evaluation results are shown in Table 1 below.

[0210]

[0211] As shown in the experimental results of Table 1 above, compared with Comparative Examples 1 to 3 and 7 using aluminum pigments without adding specific fine particles, Examples 1 to 20 using aluminum pigments (B) containing fine particles with a particle size of 1 μm or less in a predetermined amount have higher gloss and brightness, and the brightness after 10 days also maintains a high value. In particular, in Examples 13 to 16 in which liquid paraffin is also added as (C) a lubricant, higher gloss is obtained than in the case where no lubricant is used.

[0212] On the other hand, in Comparative Examples 4 to 6 and 8 using aluminum pigments in which the content of particles with a particle size of 1 μm or less (specific fine particles) exceeds the prescribed range, the VDA275 value is increased compared to Examples 1 to 20 using aluminum pigments containing particles with a particle size of 1 μm or less within the prescribed range, and mold contamination occurs during molding.

[0213] In Comparative Examples 9 to 12 using aluminum pigments having a volume average particle size outside the range of 3 μm to 40 μm, sufficient brightness could not be obtained, and slight mold contamination was observed during molding.

[0214] Industrial Applicability

[0215] The resin composition disclosed herein has industrial applicability as a material for a member for a design component.

Claims

1. A polyacetal resin composition, characterized in that The polyacetal resin composition comprises: 100 parts by mass of (A) polyacetal resin, and 0.1 to 10 parts by mass of (B) aluminum pigment, The (B) aluminum pigment contains 0.1 to 2.0% by mass of particles having a particle size of 1 μm or less based on the total amount of the (B) aluminum pigment, and the (B) aluminum pigment has a volume average particle size of 3 to 40 μm.

2. The polyacetal resin composition according to claim 1, wherein The (B) aluminum pigment contains 0.3% by mass to 1.5% by mass of particles having a particle size of 1 μm or less, based on the total amount of the (B) aluminum pigment.

3. The polyacetal resin composition according to claim 1 or 2, wherein The (B) aluminum pigment contains 0.4% by mass to 1.2% by mass of particles having a particle size of 1 μm or less, based on the total amount of the (B) aluminum pigment.

4. The polyacetal resin composition according to claim 1 or 2, wherein The (B) aluminum pigment contains 0.5% by mass to 1.0% by mass of particles having a particle size of 1 μm or less, based on the total amount of the (B) aluminum pigment.

5. The polyacetal resin composition according to claim 1 or 2, wherein The volume average particle size of the (B) aluminum pigment is 4 μm to 35 μm.

6. The polyacetal resin composition according to claim 1 or 2, wherein The volume average particle size of the (B) aluminum pigment is 5 μm to 30 μm.

7. The polyacetal resin composition according to claim 1 or 2, wherein The (B) aluminum pigment has a flat shape.

8. The polyacetal resin composition according to claim 7, wherein The average particle thickness of the (B) aluminum pigment is 0.03 μm to 0.4 μm.

9. The polyacetal resin composition according to claim 7, wherein The average particle thickness of the (B) aluminum pigment is 0.08 μm to 0.4 μm.

10. The polyacetal resin composition according to claim 7, wherein The value of average particle thickness / volume average particle diameter of the (B) aluminum pigment is 0.2 or less.

11. The polyacetal resin composition according to claim 7, wherein The value of average particle thickness / volume average particle diameter of the (B) aluminum pigment is 0.1 or less.

12. The polyacetal resin composition according to claim 7, wherein The value of average particle thickness / volume average particle diameter of the (B) aluminum pigment is 0.05 or less.

13. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition further includes (C) a lubricant.

14. The polyacetal resin composition according to claim 13, wherein The (C) lubricant is at least one selected from the group consisting of hydrocarbons, higher fatty acids, higher alcohols, aliphatic amides and metal soaps.

15. The polyacetal resin composition according to claim 13, wherein The (C) lubricant is liquid paraffin.

16. The polyacetal resin composition according to claim 13, wherein The amount of the lubricant (C) added is 0.01 to 0.5 parts by mass relative to 100 parts by mass of the polyacetal resin (A).

17. The polyacetal resin composition according to claim 13, wherein The amount of the lubricant (C) added is 0.05 to 0.45 parts by mass relative to 100 parts by mass of the polyacetal resin (A).

18. The polyacetal resin composition according to claim 13, wherein The amount of the lubricant (C) added is 0.1 to 0.4 parts by mass relative to 100 parts by mass of the polyacetal resin (A).

19. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition further comprises (D) a formaldehyde inhibitor.

20. The polyacetal resin composition according to claim 19, wherein The (D) formaldehyde inhibitor is at least one selected from the group consisting of aminotriazine compounds, guanamine compounds, urea compounds and carboxylic acid hydrazide compounds.

21. The polyacetal resin composition according to claim 19, wherein The formaldehyde inhibitor (D) is at least one selected from the group consisting of aliphatic carboxylic acid hydrazide compounds and aromatic carboxylic acid hydrazide compounds.

22. The polyacetal resin composition according to claim 19, wherein The formaldehyde inhibitor (D) is at least one selected from the group consisting of sebacic acid dihydrazide, adipic acid dihydrazide and dodecanedioic acid dihydrazide.

23. The polyacetal resin composition according to claim 19, wherein The content of the formaldehyde inhibitor (D) is 0.01 to 5 parts by mass relative to 100 parts by mass of the polyacetal resin (A).

24. The polyacetal resin composition according to claim 19, wherein The content of the formaldehyde inhibitor (D) is 0.01 to 2 parts by mass relative to 100 parts by mass of the polyacetal resin (A).

25. The polyacetal resin composition according to claim 19, wherein The content of the formaldehyde inhibitor (D) is 0.02 to 1 part by mass relative to 100 parts by mass of the polyacetal resin (A).

26. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition includes 1 to 8 parts by mass of the (B) aluminum pigment relative to 100 parts by mass of the (A) polyacetal resin.

27. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition includes 1.5 to 7 parts by mass of the (B) aluminum pigment relative to 100 parts by mass of the (A) polyacetal resin.

28. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition includes 2 to 6 parts by mass of the (B) aluminum pigment relative to 100 parts by mass of the (A) polyacetal resin.

29. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition includes 1 to 4 parts by mass of the (B) aluminum pigment relative to 100 parts by mass of the (A) polyacetal resin.

30. The polyacetal resin composition according to claim 1 or 2, wherein The (A) polyacetal resin is at least one selected from the group consisting of polyoxymethylene homopolymers and polyoxymethylene copolymers.

31. The polyacetal resin composition according to claim 30, wherein The polyoxymethylene copolymer is a polyoxymethylene copolymer having a structure in which an oxyalkylene unit represented by the following general formula (1) is randomly inserted into a chain containing an oxymethylene unit -(CH2O)-. In the above formula (1), R1 and R2 are each independently a hydrogen atom, an alkyl group or an aryl group. R1 and R2 may be the same as or different from each other. n is an integer of 2 to 6.

32. The polyacetal resin composition according to claim 30, wherein The polyoxymethylene copolymer has a structure in which oxyethylene units are randomly inserted into a chain containing an oxymethylene unit -(CH2O)-.

33. The polyacetal resin composition according to claim 32, wherein The insertion ratio of the oxyethylene unit is 0.01 mol or more and 50 mol or less relative to 100 mol of the oxymethylene unit.

34. The polyacetal resin composition according to claim 32, wherein The insertion ratio of the oxyethylene unit is 0.03 mol or more and 20 mol or less relative to 100 mol of the oxymethylene unit.

35. The polyacetal resin composition according to claim 1 or 2, wherein The (A) polyacetal resin is a polyacetal resin subjected to terminal stabilization treatment.

36. The polyacetal resin composition according to claim 1 or 2, wherein The melt flow rate of the polyacetal resin (A) measured at a temperature of 190° C. in accordance with ASTM D57E is 2.5 g / 10 min to 40 g / 10 min.

37. The polyacetal resin composition according to claim 1 or 2, wherein The melt flow rate of the polyacetal resin (A) measured at a temperature of 190° C. in accordance with ASTM D57E is 3 g / 10 min to 30 g / 10 min.

38. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition generates formaldehyde in an amount of 3 mg / kg or less.

39. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition generates formaldehyde in an amount of 2.5 mg / kg or less.

40. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition has a glossiness of 60 or more immediately after injection molding.

41. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition has a glossiness of 70 or more immediately after injection molding.

42. The polyacetal resin composition according to claim 1 or 2, wherein The polyacetal resin composition is evaluated as ◎ or ○ in the following mold deposit evaluation test, The pellets of the polyacetal resin composition were molded using an injection molding machine to prepare test pieces, and the generation of mold deposits on the mold surface was visually confirmed. ◎: No mold deposit can be visually confirmed on the mold surface; ○: The area of ​​mold deposit is less than 5mm 2 .