A method for preparing a random access memory magnetic rotation memory chip and a chip

By using the photolithography-etching-filling-grinding process in the SOT MRAM chip to increase the contact area between the SOT layer and the ferromagnetic layer, the problems of high critical current density and high power consumption are solved, and more efficient magnetic moment flipping is achieved. and faster writing speeds, meeting mass production requirements.

CN113793897BActive Publication Date: 2024-10-15SUZHOU BOJIA SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110953401.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-19
Publication Date
2024-10-15
Estimated Expiration
2041-08-19

AI Technical Summary

Technical Problem

Existing SOT MRAM chips have problems such as high critical current density for regulating magnetic moment flipping and high power consumption, and their production is difficult to meet mass production requirements.

Method used

The SOT layer is prepared using processes such as metal deposition, photolithography and etching, and is isolated by an insulating dielectric layer to increase the effective contact area between the SOT layer and the ferromagnetic layer, increase the torque effect of spin accumulation on the ferromagnetic layer, and reduce the flipping current density. , improve chip speed and reliability.

Benefits of technology

It effectively reduces the flipping current density, reduces chip energy consumption, increases writing speed, meets the process requirements of chip mass production, and improves magnetic performance and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113793897B_ABST
    Figure CN113793897B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a random access memory magnetic spin storage chip, comprising: preparing a SOT layer by metal deposition after completing a bottom electrode; preparing a groove by photolithography and etching; performing thin film deposition of a free layer and chemical mechanical grinding for surface flattening; then performing thin film deposition of a reference layer and an isolation layer of a magnetic tunneling structure; and preparing a top electrode. The present invention wraps the free layer of the magnetic tunneling structure by preparing the SOT layer, increases the torque effect of the effective current on it, reduces the current density required for flipping, reduces chip energy consumption, and increases the writing speed; the insulating dielectric layer can prevent the photoresist from reacting with the SOT layer, and the insulating dielectric layer can also serve as a stop layer for chemical mechanical flattening to increase the process window. Since the free layer is formed by a filling method, it is damage-free compared to traditional methods, which helps to improve the magnetic performance of the chip. The present invention provides a random access memory magnetic spin storage chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductors, and in particular to a preparation method of a random access memory magnetic rotation storage chip and the chip. Background Art

[0002] Memory is an important component of computer architecture, and has a decisive impact on the speed, integration and power consumption of computers. Semiconductor memory chips have been widely used in industrial and electronic equipment, household appliances, personal consumer electronics and defense equipment. Random Access Memory Magnetic Spin Memory Chip MRAM will gradually replace the current storage market dominated by DRAM, SRAM and other devices due to its excellent material performance, fast read and write speed, low energy consumption and non-volatility. As a representative of the next generation of memory chips, MRAM will make storage and computing integration and edge computing possible, making it possible to improve the performance of memory chips and a wide range of application scenarios.

[0003] However, as the feature size of semiconductor processes continues to shrink, traditional cache (Static Random Access Memory, SRAM) and main memory (Dynamic Random Access Memory, DRAM) based on complementary metal oxide semiconductor (Complementary Metal Oxide Semiconductor, CMOS) processes have encountered performance bottlenecks. In terms of power consumption, since the leakage current of CMOS transistors increases with the reduction of process size, the static power consumption of SRAM and DRAM is increasing. In terms of speed, the interconnection delay between the processor and the memory limits the main frequency of the system. An effective way to solve this problem is to build non-volatile cache and main memory so that the system can work in sleep mode without losing data, thereby eliminating leakage current and static power consumption.

[0004] MRAM can achieve a good compromise in terms of speed, area, number of writes and power consumption, so it is considered by the industry to be an ideal device for building the next generation of non-volatile cache and main memory. The basic storage unit of MRAM is MTJ (Magnetic Tunnel Junction).

[0005] The current STT-MRAM still has some drawbacks, such as the critical current density for regulating magnetic moment reversal is still relatively large, resulting in high power consumption. The next generation of new SOT MRAM chips use spin Hall effect (SHE) or inverse spin galvanic effect (iSGE) to convert the current flowing in the heavy metal layer with strong spin-orbit coupling into spin current, which diffuses into the ferromagnetic layer and exerts torque on the magnetic moment of the ferromagnetic layer to flip it. This chip has the advantages of low reversal current density and fast read and write speed, and is expected to become the development trend of the next single storage chip.

[0006] However, the chip speed of the SOT MRAM chip in the existing technology still has disadvantages, and the production still cannot meet the needs of chip mass production. Summary of the invention

[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for preparing a random access memory magnetic spin storage chip and a random access memory magnetic spin storage chip.

[0008] The technical solution of the present invention is summarized as follows:

[0009] In one aspect, the present invention provides a method for preparing a random access memory magnetic rotation memory chip, comprising:

[0010] S10, after the bottom electrode is completed, a SOT layer is prepared by metal deposition;

[0011] S20, preparing the groove by photolithography and etching; wherein the etching includes at least one of dry etching and wet etching;

[0012] S30, performing thin film deposition of the free layer and chemical mechanical polishing to planarize the surface;

[0013] S40, then performing thin film deposition of a reference layer and an isolation layer of the magnetic tunneling structure;

[0014] S50. Preparation of top electrode.

[0015] Furthermore, it also includes S11, growing an insulating dielectric layer, wherein the insulating dielectric layer is grown on the upper part of the SOT layer and is used to isolate the SOT layer from the photoresist; the insulating dielectric layer includes silicon nitride and / or silicon oxide.

[0016] Furthermore, S20 includes: spin coating of photoresist to form a coating layer, then exposure and removal of the photoresist, and then an etching process to open a core area of ​​a subsequent magnetic tunneling structure to form a groove.

[0017] Furthermore, step S30 includes filling the free layer into the groove by metal deposition, removing the excess portion, and performing chemical mechanical polishing using the insulating dielectric layer as a stop layer.

[0018] Furthermore, the free layer includes CoFeB; and the isolation layer includes MgO or Al2O3.

[0019] Furthermore, step S30 also includes: after the free layer is prepared, high temperature annealing is performed and then solidification is performed.

[0020] Furthermore, step S50 also includes filling the surrounding gaps to protect and insulate the circuit, and the filling material used is an insulating material; the filling material includes a low-k material.

[0021] Accordingly, the present invention also provides a random access memory magnetic spin memory chip, which is prepared by the random access memory magnetic spin memory chip preparation method as described above, comprising:

[0022] A magnetic tunneling structure, comprising a free layer, a reference layer and an isolation layer, wherein the magnetic tunneling structure is used to read and write data by changing its flip state;

[0023] A bottom electrode, carrying a magnetic tunneling structure;

[0024] The SOT layer is located at the top, bottom or middle of the free layer in the magnetic tunneling structure;

[0025] The top electrode is located on the magnetic tunneling structure and is used for circuit layout and wiring.

[0026] Furthermore, it also includes an insulating dielectric layer, which is located on the upper part of the SOT layer and isolates the SOT layer from the photoresist.

[0027] Furthermore, a groove is provided on the SOT layer, the groove is prepared by photolithography and etching, and the groove is used to fill the free layer.

[0028] Compared with the prior art, the beneficial effect of the present invention is that: the present invention provides a method for preparing a random access memory magnetic spin storage chip, and the free layer of the magnetic tunneling structure is wrapped by preparing a SOT layer, thereby increasing the torque effect of the effective current on it, effectively reducing the current density required for flipping, reducing chip energy consumption, and increasing the writing speed.

[0029] By using photolithography-etching-filling-grinding, the effective contact area between the SOT layer and the ferromagnetic layer is increased, and the torque effect of spin accumulation on the ferromagnetic layer is further enhanced, thereby increasing the chip speed and meeting the process requirements for chip mass production.

[0030] The insulating dielectric layer can prevent the photoresist from reacting with the SOT layer, thereby preventing the photoresist from being poisoned. The insulating dielectric layer can also serve as a stop layer for chemical mechanical planarization, thereby increasing the process window.

[0031] Since the free layer is formed by a filling method, while the traditional method is formed by an etching method, which will cause damage to its side wall, thereby affecting the magnetic performance, the present invention does not have such damage, which helps to improve the magnetic performance of the chip.

[0032] In the subsequent etching process of the magnetic tunneling structure, it is necessary to use an etching method to form a top electrode, a reference layer RF (reference layer), and an isolation layer (barrier). Since the traditional method has no insulating dielectric layer, etching will damage the SOT layer. Due to the protective effect of the insulating dielectric layer on the SOT layer, the etching process window of the present invention is larger. Therefore, a certain amount of over etching can be performed subsequently to remove the metal residue generated on the side wall during the main etching process, solve the short circuit problem caused by the metal deposition residue during etching, and improve the chip yield.

[0033] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. The specific implementation of the present invention is given in detail by the following embodiments and their accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0035] Figure 1 It is a structural schematic diagram of a random access memory magnetic rotation storage chip of the present invention;

[0036] Figure 2 It is a schematic cross-sectional structure diagram of a random access memory magnetic rotation storage chip of the present invention;

[0037] Figure 3a-3h A diagram showing the preparation process of a random access memory magnetic rotation memory chip of the present invention;

[0038] Figure 4 The present invention is a schematic diagram of a random access memory magnetic rotation storage chip during transition etching.

[0039] Figure numerals: 1, bottom electrode; 2, SOT layer; 31, free layer; 32, reference layer; 33, isolation layer; 4, top electrode; 5, insulating dielectric layer; 10, metal residue. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with the accompanying drawings, and the aforementioned and other purposes, features, aspects and advantages of the present invention will become more obvious, so that those skilled in the art can implement it with reference to the text of the specification. In the accompanying drawings, for the sake of clarity, the shapes and sizes can be enlarged, and the same reference numerals will be used in all figures to indicate the same or similar parts. In the following description, words such as center, thickness, height, length, front, back, rear, left, right, top, bottom, upper, lower, etc. are based on the orientation or position relationship shown in the accompanying drawings. In particular, "height" is equivalent to the size from top to bottom, "width" is equivalent to the size from left to right, and "depth" is equivalent to the size from front to back. These relative terms are for the convenience of explanation and are generally not intended to require specific orientation. Terms related to attachment, connection, etc. (for example, "connection" and "attachment") refer to the relationship between these structures directly or indirectly fixed or attached to each other through intermediate structures, and movable or rigid attachment or relationship, unless otherwise explicitly stated.

[0041] Next, the present invention is further described in conjunction with the accompanying drawings and specific embodiments. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment. It should be understood that the terms such as "having", "including" and "comprising" used herein do not specify the existence or addition of one or more other elements or their combinations.

[0042] The core part of the magnetic tunnel junction is a sandwich structure formed by two ferromagnetic metal layers sandwiching a tunnel barrier layer. One of the ferromagnetic layers is called the reference layer (Reference Layer) or the pinned layer (Pinned Layer), and its magnetization is fixed along the easy axis (Easy-Axis). The other ferromagnetic layer is called the free layer (Free Layer), and its magnetization has two stable orientations, which are parallel or anti-parallel to the reference layer, respectively. This will put the magnetic tunnel junction in a low resistance state or a high resistance state. The two resistance states can represent binary data "0" and "1" respectively, which is the basic principle of MRAM storage. This phenomenon is called the tunnel magnetoresistance effect (Tunnel Magnetoresistance, TMR).

[0043] The principle of SOT is to use the spin Hall effect (SHE) or inverse spin galvanic effect (iSGE) to convert the current flowing in the heavy metal layer with strong spin-orbit coupling into a spin current, which diffuses into the ferromagnetic layer and exerts a torque on the magnetic moment of the ferromagnetic layer to flip it. When the ferromagnetic layer is in a parallel state (parallel), the resistance is low; when the ferromagnetic layer is in a non-parallel state (anti-parallel), the resistance is high. Among them, MTJ is the key core structure for chip reading and writing, mainly including a free layer (FL), a reference layer (FL) and a barrier. The pure spin current generated by the Hall effect generated by the SOT layer and the interface Rashba effect or the spin accumulation of a certain orientation at the interface will exert a torque on the adjacent ferromagnetic layer, accelerating the reversal of the free layer. Compared with STT-MRAM, SOT-MRAM has a smaller write current density and faster read and write speed. The inventors have found that enhancing the torque effect of the SOT layer on the ferromagnetic layer is crucial to improving chip performance and increasing chip speed. Based on the above content, the present invention provides a method for preparing a random access memory magnetic spin storage chip.

[0044] like Figure 1-4 As shown, a method for preparing a random access memory magnetic rotation memory chip of the present invention comprises:

[0045] S10, after the bottom electrode 1 (BE1 and BE2) is completed, the SOT layer 2 is prepared by metal deposition. Figure 3a .

[0046] S11, the growth of the insulating dielectric layer, the insulating dielectric layer is grown on the upper part of the SOT layer 2, and is used to isolate the SOT layer 2 from the photoresist. Otherwise, the SOT layer material will react with the photoresist, causing photoresist poisoning. This will cause a short circuit and affect chip reliability. It can also prevent the SOT layer from being damaged by subsequent processes, and the insulating dielectric layer can protect the SOT layer. Reference Figure 3b The insulating dielectric layer includes silicon nitride and / or silicon oxide, but is not limited to these two materials.

[0047] S20, preparing the groove by photolithography and etching; wherein the etching includes at least one of dry etching and wet etching;

[0048] S30, performing thin film deposition and chemical mechanical polishing (CMP) of the free layer 31 to planarize the surface;

[0049] S40, then depositing the reference layer 32 and the isolation layer 33 of the magnetic tunneling structure 3; Figure 3g .

[0050] S50 , preparation of top electrode 4 .

[0051] Since SOT MRAM requires a SOT layer to use the SHE effect to flip the state of the free layer in the MTJ, and the torque size and efficiency of the electrons in the SOT layer on the free layer directly affect the device performance of the MTJ, it is very important to improve the SHE effect by optimizing the chip structure and the preparation method. When preparing the SOT layer, the present invention adopts the steps of photolithography-etching-filling-grinding, and further improves the torque effect of spin accumulation on the ferromagnetic layer by increasing the effective contact area between the SOT layer and the ferromagnetic layer, thereby improving the chip speed and meeting the process requirements of chip mass production.

[0052] In step S10, the SOT layer can be made of heavy metals, but can also be made of, but not limited to, 2D materials such as tungsten sulfide WS2 or graphene. The material has a very strong electrical conductivity. Figure 3a The SOT layer is connected to MOS tubes and other devices through circuit layout and wiring after the bottom electrode (BE1 and BE2) to form a write bit line, which is used to provide current and voltage for SOT-MRAM. The MTJ structure is used to read and write data by changing its flip state. The top electrode (TE) is interconnected by copper to form a read bit line.

[0053] Specifically, S20 includes: spin coating of photoresist to form a coating layer, then performing exposure and removing the photoresist, and then performing an etching process to open the core area of ​​the subsequent magnetic tunneling structure 3 to form a groove. Specifically, refer to Figure 3c , perform spin coating of photoresist and SOC material or BARC material, refer to Figure 3d , followed by mask alignment (overlay) and exposure processes, and photoresist removal, refer to Figure 3e , an etching process is used to open the subsequent MTJ core area, and then an etching process is performed to etch the dielectric insulation layer and the SOT layer mask opening area.

[0054] Step S30 includes filling the free layer 31 into the groove by metal deposition, removing the excess part, and performing chemical mechanical polishing with the insulating dielectric layer as a stop layer to ensure that unnecessary free layer residues are removed and the process window is expanded. Figure 3f .

[0055] Step S30 also includes: after the free layer is prepared, high temperature annealing is performed to solidify the free layer, and surface gas treatment (such as nitrogen, hydrogen and oxygen, etc.) is performed.

[0056] In step S40, the materials of the reference layer and the fixed layer include but are not limited to CoFeB and CoPt respectively, and a double-layer structure with an intercalation layer such as MgO-Ru-MgO can be used to further increase the spin coupling effect. The free layer includes CoFeB; the isolation layer 33 includes MgO or Al2O3.

[0057] Step S50 also includes etching of the MTJ structure and the top electrode 4, see Figure 3h The method also includes filling the surrounding gaps to protect the circuit and provide insulation isolation. The filling material used is an insulating material. The filling material includes oxide or low-k material to protect the circuit and provide insulation isolation.

[0058] It should be pointed out that the epitaxial growth method, coating process, sputtering process and etching process described in the above-mentioned manufacturing method should be understood as that the growth method can be selected from but not limited to metal organic chemical vapor deposition (MOCVD), molecular beam epitaxy (MBE) or magnetron sputtering; the coating process includes making a photoresist mask pattern on the sample by ultraviolet lithography technology, wherein the etching process can be selected from but not limited to dry etching or wet etching, and should also include degumming treatment, and dry etching includes inductively coupled plasma etching or BCl3-based plasma etching, but is not limited to this; the corrosive liquid used in wet etching includes any one or a combination of two or more of hydrochloric acid, hydrofluoric acid, nitric acid, sulfuric acid and BOE corrosive agent, but is not limited to this; the degumming treatment includes any one of cleaning with a plasma cleaner, processing with a plasma degumming machine, processing with a chlorine-based plasma or cleaning with UV light, or a combination of two or more processing methods, but is not limited to this.

[0059] The conditions of the dry ICP etching process are as follows: ICP coil power 500-1000W, source power 120-300W, source gas Cl2 and He 25sccm and 10sccm respectively, etching time Second.

[0060] Accordingly, refer to Figure 1-2 and Figure 4 The present invention also provides a random access memory magnetic spin memory chip, which is prepared by the random access memory magnetic spin memory chip preparation method as described above, comprising:

[0061] A magnetic tunneling structure 3, comprising a free layer 31 (FL), a reference layer 32 (RL) and an isolation layer 33 (barrier), wherein the magnetic tunneling structure 3 is used to read and write data by changing its flip state;

[0062] The bottom through hole is used to connect the bottom metal connection and the bottom electrode. At the same time, it is used to connect the top metal connection and the bottom metal connection in the logic area for the layout and wiring of the logic area circuit.

[0063] The bottom electrode 1 is located on the bottom through hole and carries the magnetic tunneling structure 3; wherein the bottom electrode 1 (BE1 and BE2) is then connected to devices such as MOS tubes through circuit layout and wiring to form a write bit line for providing current and voltage for the SOT-MRAM.

[0064] The SOT layer 2 is located at the top, bottom or middle of the free layer 31 in the magnetic tunneling structure 3, forming a sandwich structure to promote the flipping of the free layer. The SOT layer is generally composed of heavy metal materials and graphene and other materials, which require the material to have extremely strong electrical conductivity.

[0065] The top electrode 4 is located on the magnetic tunneling structure 3 and is used for circuit layout and wiring. The top electrode (TE) is interconnected by copper to form a read bit line.

[0066] It also includes an insulating dielectric layer 5, which is located on the upper part of the SOT layer 2 to isolate the SOT layer 2 from the photoresist. Otherwise, the SOT layer material will react with the photoresist, causing photoresist poisoning. Causing a short circuit and affecting chip reliability. And it can prevent the SOT layer from being damaged by subsequent processes, and the insulating dielectric layer protects the SOT layer. Therefore, the etching process window is large, so excessive etching at a certain angle can be performed later to remove the metal residue 10 generated on the side wall during the main etching process, solve the short circuit problem caused by metal deposition residues during etching, and improve chip yield. The dielectric insulating material is generally made of silicon nitride or silicon oxide, but is not limited to these two materials. Reference Figure 4 .

[0067] The SOT layer 2 is provided with a groove, which is prepared by photolithography and etching methods, and is used to fill the free layer 31 .

[0068] The free layer is formed by metal deposition and filling, and then the surface is flattened by chemical mechanical polishing. The dielectric insulating layer can be used as a stop layer for polishing.

[0069] The present invention provides a method for preparing a random access memory magnetic spin storage chip, in which a free layer of a magnetic tunneling structure is wrapped by preparing a SOT layer, thereby increasing the torque effect of an effective current on it, effectively reducing the current density required for flipping, reducing chip energy consumption, and increasing the writing speed.

[0070] By using photolithography-etching-filling-grinding, the effective contact area between the SOT layer and the ferromagnetic layer is increased, and the torque effect of spin accumulation on the ferromagnetic layer is further enhanced, thereby increasing the chip speed and meeting the process requirements for chip mass production.

[0071] The insulating dielectric layer can prevent the photoresist from reacting with the SOT layer, thereby preventing the photoresist from being poisoned. The insulating dielectric layer can also serve as a stop layer for chemical mechanical planarization, thereby increasing the process window.

[0072] Since the free layer is formed by a filling method, while the traditional method is formed by an etching method, which will cause damage to its side wall, thereby affecting the magnetic performance, the present invention does not have such damage, which helps to improve the magnetic performance of the chip.

[0073] In the subsequent etching process of the magnetic tunneling structure, the top electrode, reference layer RF (reference layer), and isolation layer (barrier) need to be formed by etching. The traditional method has no insulating dielectric layer, and etching will damage the SOT layer. Due to the protective effect of the insulating dielectric layer on the SOT layer, the etching process window of the present invention is larger, so a certain amount of over etching can be performed later to remove the metal residue 10 generated on the side wall during the main etching process. It should be emphasized that over etching with an inclined angle (10 to 30 degrees) is helpful for removing metal residues, solving the short circuit problem caused by metal deposition residues, and improving chip yield.

[0074] It should be noted that the sequence of the embodiments of the present invention described above is for description only and does not represent the advantages and disadvantages of the embodiments. The above describes specific embodiments of this specification. Other embodiments are within the scope of the appended claims. In some cases, the actions or steps recorded in the claims can be performed in an order different from that in the embodiments and still achieve the desired results. In addition, the processes depicted in the drawings do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.

[0075] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the device and electronic device embodiments, since they are basically similar to the method embodiments, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiments.

[0076] The above description has fully disclosed the specific embodiments of the present invention. It should be pointed out that any changes made by those skilled in the art to the specific embodiments of the present invention do not deviate from the scope of the claims of the present invention. Accordingly, the scope of the claims of the present invention is not limited to the above specific embodiments.

Claims

1. A method for preparing a random access memory magnetic rotation memory chip, It is characterized in that include: S10, after the bottom electrode (1) is completed, a SOT layer (2) is prepared by metal deposition; S11, growing an insulating dielectric layer, the insulating dielectric layer being grown on the upper part of the SOT layer (2) and being used to isolate the SOT layer (2) from the photoresist; the insulating dielectric layer comprising silicon nitride and / or silicon oxide; S20, preparing the groove by photolithography and etching; wherein the etching includes at least one of dry etching and wet etching; S30, performing thin film deposition and chemical mechanical polishing of the free layer (31) to planarize the surface; S40, then performing thin film deposition of a reference layer (32) and an isolation layer (33) of the magnetic tunneling structure (3); S50, preparation of top electrode (4); Wherein, the S20 comprises: spin coating of photoresist to form a coating layer, then exposure and removal of the photoresist, and then etching to open the core area of ​​the subsequent magnetic tunneling structure (3) to form a groove.

2. The method for preparing the random access memory magnetic rotation memory chip according to claim 1, It is characterized in that Step S30 includes filling the free layer (31) into the groove by metal deposition, removing the excess portion, and performing chemical mechanical polishing using an insulating dielectric layer as a stop layer.

3. The method for preparing the random access memory magnetic rotation memory chip according to claim 1, It is characterized in that The free layer includes CoFeB; the isolation layer (33) includes MgO or Al 2 O 3 .

4. The method for preparing the random access memory magnetic rotation memory chip according to claim 1, It is characterized in that Step S30 also includes: after the free layer is prepared, high temperature annealing is performed and then solidification is performed.

5. The method for preparing the random access memory magnetic rotation memory chip according to claim 1, It is characterized in that Step S50 also includes filling the surrounding gaps to protect the circuit and provide insulation isolation. The filling material used is an insulating material; the filling material includes a low-k material.

6. A random access memory magnetic rotation storage chip, It is characterized in that The method for preparing a random access memory magnetic rotation memory chip according to claim 1 comprises: A magnetic tunneling structure (3) comprising a free layer (31), a reference layer (32) and an isolation layer (33), wherein the magnetic tunneling structure (3) is used to read and write data by changing its flip state; A bottom electrode (1) carrying a magnetic tunneling structure (3); The SOT layer (2) has a groove on its surface, and a portion of the free layer (31) located in the magnetic tunneling structure (3) is filled in the groove; The top electrode (4) is located on the magnetic tunneling structure (3) and is used for circuit layout and wiring.

7. The random access memory magnetic rotation storage chip as claimed in claim 6, It is characterized in that It also comprises an insulating dielectric layer, which is located on the upper part of the SOT layer (2) and isolates the SOT layer (2) from the photoresist.

8. The random access memory magnetic rotation storage chip as claimed in claim 6, It is characterized in that The SOT layer (2) is provided with a groove, the groove is prepared by photolithography and etching methods, and the groove is used to fill the free layer (31).