Silicon dioxide-carbon composite material and method for producing the same

By using amorphous silica and carbon porous composite materials from silica-based plants, the problem of low affinity between silica and rubber materials in the prior art is solved, and an efficient rubber material filler is realized. Reduces manufacturing costs and improves performance.

CN113795463BActive Publication Date: 2024-11-12KUBOTA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080033604.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-10
Filing Date
2020-04-28
Publication Date
2024-11-12
Estimated Expiration
2040-04-28

AI Technical Summary

Technical Problem

In the prior art, rubber material fillers rich in carbon and silica using chaff have low affinity with rubber material due to the hydrophilicity of silica, and expensive silane coupling agents are required to improve philtrum. However, silane coupling agents may coking at high temperatures, and carbon black is derived from petroleum, which has environmental and cost problems.

Method used

Amorphous silica and carbon porous composite materials from silica-based plant resources are used to gasify the carbon in the resource materials through the gasification process, and the ungasified resource materials residues are recovered as silica-carbon Composite material, achieving high affinity without the need for silane coupling agents.

Benefits of technology

High affinity with rubber components is achieved, manufacturing costs are reduced, coking problems of silane coupling agents are avoided, and the rolling resistance and wear resistance of the material are improved by optimizing the structure of the carbon porous body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113795463B_ABST
    Figure CN113795463B_ABST
Patent Text Reader

Abstract

Provided are a silica-carbon composite material and a method for producing the same, which does not require the use of a silane coupling agent, improves the affinity between silica and rubber materials, and fully utilizes the properties of carbon and silica. The silica-carbon composite material uses a resource material from silicic acid plants as a raw material and contains a composite composed of amorphous silica and a carbon porous body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a silicon dioxide-carbon composite material and a method for producing the same. Background Art

[0002] Millions of tons of rice husks are produced around the world every year, but until now they have been mostly treated as waste. In recent years, people have noticed that rice husks are rich in carbon and silica and have begun to promote their use as fillers in rubber materials.

[0003] It is known that rubber is generally reinforced by adding carbon black, thereby greatly improving its fatigue resistance and wear resistance. In addition, compared with carbon black, silica has good low loss and anti-wet skid properties, so it is used as the above-mentioned filler to reduce tire rolling resistance, etc.

[0004] Regarding the technology of using rice husk as the above-mentioned filler, for example, there are known technologies such as: a technology of mixing a rubber composition containing rice husk carbon, or a rubber composition mixed with rice husk carbon and silica particles, into a tire to improve rolling resistance, etc.; a technology of incorporating a tread rubber composition containing rice husk carbon and a silane coupling agent into a tire to improve ice driving performance and wear resistance; a technology of using a rubber reinforcing material with rice husk carbon as a main component to improve the durability of tires, etc. (Patent Documents 1 to 8).

[0005] In addition, there is also known a technique of applying a rubber composition obtained by coating the surface of carbon black with silica by chemical treatment to a tire or the like (Patent Document 9).

[0006] [Prior art literature]

[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-114251 (published on May 28, 2009)

[0008] Patent Document 2: Japanese Patent Application Publication No. 2009-114252 (published on May 28, 2009)

[0009] Patent Document 3: Japanese Patent Application Publication No. 2009-114253 (published on May 28, 2009)

[0010] Patent Document 4: Japanese Patent Application Publication No. 2009-114254 (published on May 28, 2009)

[0011] Patent Document 5: Japanese Patent Application Publication No. 2009-114255 (published on May 28, 2009)

[0012] Patent Document 6: Japanese Patent Application Publication No. 2009-114257 (published on May 28, 2009)

[0013] Patent Document 7: Japanese Patent Application Publication No. 2011-68784 (published on April 7, 2011)

[0014] Patent Document 8: Japanese Patent Application Publication No. 2013-155254 (published on August 15, 2013)

[0015] Patent document 9: Japanese Patent Application Publication No. 9-118837 (published on May 6, 1997) Summary of the invention

[0016] [Problems to be solved by the invention]

[0017] As described above, many fillers for rubber materials have been developed using the property of rice husks that they are rich in carbon and silica. Carbon has a high affinity with rubber materials, but silica has a low affinity with rubber materials due to its hydrophilicity. Therefore, the fillers disclosed in Patent Documents 1 to 8 use a silane coupling agent that chemically bonds the rubber material to the surface of silica particles in order to improve the affinity.

[0018] However, silane coupling agents are expensive and require a large amount of compounding, which leads to a problem of increased manufacturing costs of tires, etc. In addition, since silane coupling agents contain sulfur molecules, when the processing temperature is increased, a so-called scorching problem occurs.

[0019] As described above, it is preferable to use a silane coupling agent to improve the affinity. However, taking the above-mentioned problems into consideration, it can be said that a filler which can exhibit the above affinity as good as that when a silane coupling agent is used even when no silane coupling agent is used is more preferable.

[0020] Patent Document 9 discloses that the surface of carbon black is treated with silicon dioxide by dispersing carbon black in water and utilizing a wet reaction between a metal silicate and an acid, so that the filler has a structure after the treatment. The filler can exhibit excellent physical properties due to the structure.

[0021] However, from the perspective of treating the surface with silica, if there is no silane coupling agent, the filler will aggregate due to the interaction between silanols, and sufficient dispersibility cannot be ensured. In addition, since carbon black is a petroleum product and is surface treated with silica, there are problems such as obstacles to natural symbiosis sustainability and increased energy costs in terms of the environment and cost.

[0022] In view of this, one aspect of the present invention is to provide a silica-carbon composite material and a method for producing the same, in which the affinity between silica and a rubber material can be improved and the properties of carbon and silica can be fully utilized regardless of whether a silane coupling agent is used in combination.

[0023] [Technical means to solve the problem]

[0024] In order to solve the above-mentioned problems, a silica-carbon composite material according to one aspect of the present invention and a method for producing a silica-carbon composite material according to one aspect of the present invention include the following inventions.

[0025] [1] A silica-carbon composite material, which is made from a resource material derived from silicic acid plants and contains a composite body composed of amorphous silica and a carbon porous body.

[0026] [2] A method for producing a silicon dioxide-carbon composite material, comprising:

[0027] A gasification step of supplying superheated steam to the resource material derived from silicate plants to gasify a portion of carbon contained in the resource material;

[0028] In the recovery step, the resource material residue remaining as a solid component without being gasified in the gasification step is recovered as a silica-carbon composite material.

[0029] [Effects of the Invention]

[0030] According to one aspect of the present invention, there is provided a material obtained from a resource material derived from a silicate plant, which has a high affinity with a rubber component even if it contains silica, and which can exhibit the same performance as a conventional composition containing carbon and silica, regardless of whether or not a silane coupling agent is used in combination. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The diagram schematically shows the structure of an example of a gasification furnace that can be used to implement the gasification step in the method for producing a silicon dioxide-carbon composite material according to one embodiment of the present invention.

[0032] Figure 2 This is a graph showing changes in the BET specific surface area of ​​the silica-carbon composite material according to one embodiment of the present invention, which was obtained by using rice stalks and husks and changing the gasification rate in the gasification step accordingly in the examples.

[0033] Figure 3 is Figure 2 In addition to the results shown above, a graph showing the results when sawdust, bamboo, and stem bark were used is also shown.

[0034] Figure 4 This is a graph showing the composition of gas and resource material residue when the gasification rate in the gasification step is set to 30% to 90% in the Examples.

[0035] Figure 5 It is a graph showing the husk composition, the amount of resource material residue yield when the gasification rate is 30% to 90%, and the resource material residue composition.

[0036] Figure 6 This is a SEM observation result (magnification 100 times) of the silicon dioxide-carbon composite material that has not been pulverized.

[0037] Figure 7 This is a SEM observation result (magnification 500 times) of the silicon dioxide-carbon composite material that has not been pulverized.

[0038] Figure 8 This is a SEM observation result of a silica-carbon composite material that has been pulverized to have an average particle size (D50) of about 1 μm.

[0039] Fig. 9 Observed at 14 times magnification Figure 8 SEM photograph of the large blocky particles shown.

[0040] Fig.10 Yes Figure 8 The results of mapping analysis of large bulk particles are shown.

[0041] Fig.11 Yes Figure 8 The graph showing the result of mapping analysis of the small house-shaped particles is a SEM photograph of the house-shaped small particles observed at a magnification of 14 times.

[0042] Fig.12 Shows Figure 8 The mapping analysis results of the room-shaped granules are shown.

[0043] Fig.13 This is a photograph showing that the silicon dioxide-carbon composite material according to one embodiment of the present invention has amphiphilic molecular properties.

[0044] <Description of Reference Numerals>

[0045] 1: Gasification unit.

[0046] 2: Gas reforming section.

[0047] 100: Gasifier. DETAILED DESCRIPTION

[0048] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto. The present invention is not limited to the various schemes described below, and various changes can be made within the scope directly or indirectly disclosed in the specification. Embodiments obtained by appropriately combining the technical means respectively disclosed in different embodiments are also included in the technical scope of the present invention. In addition, unless otherwise specified in this specification, "A to B" indicating a numerical range means "above A and below B". In addition, "mass" and "weight", "mass %" and "weight %" are regarded as synonyms.

[0049] [Embodiment 1. Silica-carbon composite material]

[0050] (1) Silica-carbon composite materials

[0051] The silica-carbon composite material according to one embodiment of the present invention uses a resource material (biomass) derived from silicic acid plants as a raw material, and includes a composite body composed of amorphous silica and a carbon porous body.

[0052] Resource materials from silicic acid plants can be obtained from silicic acid plants, and are not particularly limited as long as they are materials containing carbon and amorphous silica. Examples include rice husks, rice stalks, wheat stalks, bamboo, sawdust, stem bark, wood chips, grass, etc. The silica-carbon composite material of one embodiment of the present invention can be prepared, for example, by the method for producing a silica-carbon composite material of one embodiment of the present invention described later.

[0053] The "amorphous silica" refers to silica in a non-crystalline state. Crystalline silica is not good because it may induce cancer in humans. The silica in this state contained in the resource material has an amorphous structure. If the resource material is provided to a water-gas shift reaction at a high temperature of about 950°C, there is a risk of partial crystallization of the silica, and then as described later, the silica-carbon composite material of one embodiment of the present invention can be prepared at a temperature below 800°C. Therefore, the silica-carbon composite material of one embodiment of the present invention does not contain crystalline silica.

[0054] The "carbon porous body" refers to carbon having a plurality of pores on the surface and inside and having a network structure formed by connecting these pores. In addition, the "composite composed of amorphous silica and a carbon porous body" refers to a composite material formed by amorphous silica and a carbon porous body in an inseparable manner, and does not refer to a simple mixture thereof.

[0055] As shown in the examples described below, the silica-carbon composite material of one embodiment of the present invention was observed using a scanning electron microscope (SEM) to show that a large number of small room-shaped particles were agglomerated and attached to large bulk particles. In addition, the silica-carbon composite material of one embodiment of the present invention was analyzed using an electron probe micro X-ray analyzer (EPMA) to show that the bulk particles contained more carbon, the room-shaped particles contained more silica, and the block particles and the room-shaped particles were not composed of a single carbon component or a single silica component. Based on these results, it can be said that the silica-carbon composite material of one embodiment of the present invention contains a composite composed of amorphous silica and a carbon porous body.

[0056] The numerous pores on the surface and inside of the carbon porous body capture and adsorb amorphous silica, thereby forming a silica-carbon composite material according to one embodiment of the present invention. In addition, the adsorbed amorphous silica is not easy to be separated from the carbon porous body. As a result, the silica-carbon composite material according to one embodiment of the present invention, although containing amorphous silica that is originally hydrophilic and has a low affinity with the rubber component, can show high affinity with respect to the rubber component regardless of whether a silane coupling agent is used in combination.

[0057] Furthermore, the silica-carbon composite material according to one embodiment of the present invention can exhibit properties equivalent to or better than those obtained when a silane coupling agent is used in combination with a mixture of amorphous silica and carbon, even when no silane coupling agent is used in combination as in the examples described below.

[0058] Therefore, according to one embodiment of the present invention, a filler for a rubber component that exhibits excellent physical properties can be provided regardless of whether a silane coupling agent is used in combination.

[0059] In 100% by mass of the silica-carbon composite material of one embodiment of the present invention, the content of the composite composed of amorphous silica and carbon porous body is preferably 50% by mass or more, more preferably 70% by mass or more, and most preferably 100% by mass. When the content is 50% by mass or more, the silica-carbon composite material can be mixed into rubber products such as tires to give full play to the expected characteristics brought by amorphous silica and carbon.

[0060] The silicon dioxide-carbon composite material according to one embodiment of the present invention may also contain other components such as potassium, sodium, iron, phosphorus, etc. in addition to the composite.

[0061] Preferably, 10% by mass or more and 70% by mass or less of carbon contained in the resource material is contained in the silicon dioxide-carbon composite material according to one embodiment of the present invention.

[0062] As shown in the embodiments described below, the carbon contained in the resource material includes carbon discharged by gasification and carbon remaining in the silicon dioxide-carbon composite material without gasification. In this specification, the ratio of the weight of gasified carbon to the weight of carbon in the resource material is referred to as "gasification rate". By adjusting the gasification rate, the amount of residual carbon in the silicon dioxide-carbon composite material can be adjusted, and as a result, the BET specific surface area of ​​the silicon dioxide-carbon composite material can be optimized.

[0063] If 10% by mass or more and 70% by mass or less of carbon contained in the resource material is contained in the silicon dioxide-carbon composite material of one embodiment of the present invention, the BET specific surface area of ​​the silicon dioxide-carbon composite material can reach 100 m 2 / g and above 900m 2 / g or less.

[0064] The BET specific surface area of ​​the silicon dioxide-carbon composite material according to one embodiment of the present invention is preferably 100 m 2 / g and above 900m 2 In addition, the BET specific surface area is preferably 100 m 2 / g and above and 350m 2 / g or less.

[0065] Among the aforementioned resources from silicate plants, rice stalks, husks and wheat stalks contain more ash, about 20% by weight, while bamboo, sawdust, stem bark, wood chips and grass contain less ash, about several% by weight.

[0066] Therefore, the BET specific surface area of ​​the silicon dioxide-carbon composite material will be different depending on the type of the resource material used as the raw material. 2 / g and above 900m 2 This embodiment of having a carbon content of 0.1 wt% or less is suitable for improving the affinity between amorphous silica and the rubber component, and the carbon in this embodiment has a porous form suitable for forming a composite with amorphous silica.

[0067] In addition, regarding the silicon dioxide-carbon composite material using at least one resource material selected from rice stalks, rice husks and wheat stalks as raw materials, the BET specific surface area is 100m 2 / g and above and 350m 2 / g or less is easier to achieve. The ash content of these resource materials is high, so more amorphous silica can form a complex with carbon to achieve this solution. Therefore, if you want to use more amorphous silica, the above solution is more effective.

[0068] The average particle size (D50) of the silica-carbon composite material of one embodiment of the present invention is preferably 0.1 μm or more and 10 μm or less. The average particle size (D50) of the silica-carbon composite material is not particularly limited, and for example, the silica-carbon composite material can be crushed after preparation to adjust the D50 according to the application.

[0069] According to the above scheme, the average particle size (D50) is 0.1 μm or more and 10 μm or less, and in the silicon dioxide-carbon composite material, the carbon part can ensure reinforcement and wear resistance, and the silicon dioxide part can ensure low loss and wet skid resistance, so it can be well applied to low fuel consumption tire filler and other uses. From this point of view, the average particle size (D50) is preferably 0.1 μm or more and 5 μm or less, and particularly preferably 0.1 μm or more and 3 μm or less.

[0070] Here, the average particle size (D50) refers to a value measured by a laser refraction / scattering particle size distribution analyzer.

[0071] The silica-carbon composite material of one embodiment of the present invention preferably has amphipathic properties. As mentioned above, although the silica-carbon composite material contains amorphous silica, it has superior affinity with respect to the rubber component. As shown in the examples described below, a mixture of silica and carbon black remains in a two-phase separation state after being added to toluene and distilled water, while the silica-carbon composite material forms a stable emulsion. In this way, it is confirmed that the silica-carbon composite material of one embodiment of the present invention has amphipathic properties.

[0072] According to the above scheme, the affinity between silica and rubber components is improved, and rubber products such as tires can be manufactured without using a silane coupling agent. That is, a significant reduction in manufacturing costs and improvement in the efficiency of the manufacturing process can be expected.

[0073] In addition, the silica-carbon composite material of one embodiment of the present invention has amphiphilic molecular properties, so it can be said that the original hydrophilicity of the silica contained therein is maintained. Therefore, the silica-carbon composite material of one embodiment of the present invention can fully maintain the following characteristics brought about by the hydrophilicity of silica: the affinity between the tire rubber component and the wet road surface can be improved by, for example, the silanol group, thereby increasing the adhesive friction coefficient.

[0074] (2) Additives for polymer materials

[0075] The additive for polymer materials (hereinafter also referred to as "additive") according to one embodiment of the present invention contains the silicon dioxide-carbon composite material according to one embodiment of the present invention. The additive can be used as an additive for polymer materials such as resins, artificial leathers, artificial fibers, and elastomers. The polymer material can be one or more.

[0076] The resin may be a thermoplastic resin or a thermosetting resin. In addition, the elastomer may be a rubber component (thermosetting elastomer) or a thermoplastic elastomer (TPE). As the rubber component, for example, the rubber components described in the "Rubber Composition" section described later can be used. As the thermoplastic elastomer, various thermoplastic elastomers such as styrene-based, olefin-based, vinyl chloride-based, urethane-based, ester-based, and amide-based elastomers may be used.

[0077] Furthermore, if black coloring is not a problem, the above additives can also be used as additives for resin or rubber.

[0078] By adjusting the amount of the additive added and mixing it with the polymer material, the strength, heat resistance and other resistances of the polymer material can be improved. In addition, the additive is an effective recycling of waste resource materials, so the consumption of mineral resources used as additives can be suppressed.

[0079] The additive can also give the polymer material new functions. For example, when it is used as an additive for a rubber composition, it can increase the content of silica in the rubber composition, thereby improving the insulation of the rubber composition. The additive can also improve the processability of the polymer material. In addition, by using the additive as a functional extender, it is possible to maintain superior properties while reducing the manufacturing cost of rubber products, etc. When the additive is used as an additive for a resin product, it also has the advantage of lightweighting the product because the silica-carbon composite material contains a carbonaceous porous body and the bulk specific gravity of the silica-carbon composite material is small.

[0080] From the viewpoint of giving full play to the effect of the silicon dioxide-carbon composite material as much as possible, the content of the silicon dioxide-carbon composite material in the additive is preferably 50% by mass or more, more preferably 70% by mass or more, and particularly preferably 90% by mass or more. The content may also be 100% by mass. That is, the additive may also be the silicon dioxide-carbon composite material itself. In addition, from the viewpoint of suppressing the decline of other physical properties of the product, the content is preferably 90% by mass or less, more preferably 70% by mass or less, and particularly preferably 50% by mass or less.

[0081] Components other than the silica-carbon composite material that the additive may contain include, for example, mineral-derived amorphous silica, carbon black, calcium carbonate, clay minerals such as talc, and the like.

[0082] In addition, the additive is preferably added in an amount of 5 phr to 100 phr, more preferably 10 phr to 50 phr relative to the polymer material. If black coloring is not a problem, the additive can also be used in cosmetics, food, coatings, and other applications other than polymer materials.

[0083] (3) Rubber composition

[0084] A rubber composition according to an embodiment of the present invention contains a rubber component and a polymer material additive according to an embodiment of the present invention, wherein the content of the polymer material additive is 3 phr to 140 phr based on the rubber component.

[0085] As described above, the additive of one embodiment of the present invention contains the silica-carbon composite material of one embodiment of the present invention. Whether or not a silane coupling agent is used in the silica-carbon composite material, the affinity between silica and the rubber component is improved. Therefore, the additive can be preferably used as a component of the rubber composition.

[0086] The rubber component is not particularly limited. For example, natural rubbers such as SIR20, RSS#1, RSS#3, TSR20, deproteinized natural rubber (DPNR), and high-purity natural rubber (HPNR); isoprene rubber, butadiene rubber, styrene butadiene rubber, butene rubber, halogenated butene rubber, acrylonitrile butadiene rubber, acrylonitrile-styrene-butadiene copolymer rubber, chloroprene rubber, ethylene-propylene copolymer rubber, styrene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, isoprene-butadiene copolymer rubber, polyvinyl sulfone chloride, acrylic rubber, epichlorohydrin rubber, silicone rubber, and urethane rubber can be used alone or in combination of two or more.

[0087] The rubber component may be produced by various polymerization methods such as emulsion polymerization and solution polymerization, and may have a structure having a modified group at the terminal.

[0088] In the rubber composition of one embodiment of the present invention, the content of the additive of one embodiment of the present invention is preferably 3 phr or more, more preferably 5 phr or more, and particularly preferably 10 phr or more. When the content is 10 phr or more, the tire etc. made using the rubber composition can fully exert the expected properties brought by amorphous silica and carbon.

[0089] Here, “phr” is an abbreviation for “parts per hundred rubber” and means the blending amount relative to 100 parts by weight of the rubber component.

[0090] In addition, the content is preferably 140 phr or less, more preferably 120 phr or less, and particularly preferably 100 phr or less. When the content is 140 phr or less, there is a tendency that the negative effects on the molding processability caused by the increase in the viscosity of the rubber composition can be suppressed, and the expected properties brought by the amorphous silica and carbon can be fully exhibited.

[0091] The rubber composition of one embodiment of the present invention may contain, in addition to the polymer material additive and rubber component of one embodiment of the present invention, admixtures generally used in the rubber industry. As such admixtures, for example, carbon black, silica, calcium carbonate, clay, talc and other fillers; sulfenamide vulcanization accelerators, guanidine vulcanization accelerators, hydrozincite and other vulcanization accelerators (auxiliaries); processing aids such as stearic acid; silane-based, titanate-based coupling agents; amine-based, phenol-based anti-aging agents; reinforcing materials; softeners; plasticizers; tackifiers; anti-rapid vulcanization agents; and the like.

[0092] The content of the additives is not particularly limited, but the total amount of fillers such as carbon black and silica used in the rubber composition according to one embodiment of the present invention is preferably 10 phr to 100 phr.

[0093] The rubber composition of one embodiment of the present invention can be prepared by kneading the polymer material additive of one embodiment of the present invention, the rubber component, and the admixture used as required, and then vulcanizing it. The kneading can be performed by a kneading machine such as a Banbury mixer, a kneader, or a gap roll mill.

[0094] As shown in the examples described below, the rubber composition of one embodiment of the present invention exhibits the same effects as the rubber composition produced using silica, carbon black and a silane coupling agent in various physical properties. That is, the rubber composition of one embodiment of the present invention can be produced at low cost and can exhibit sufficient strength and low rolling resistance, etc., so it can be said that the rubber composition is a composition that can be used very well for rubber products such as tires.

[0095] (4) Rubber products

[0096] The rubber product of one embodiment of the present invention contains the rubber composition of one embodiment of the present invention. Since the rubber composition has the aforementioned superior properties, the rubber product can also have the properties. In addition, since the silica-carbon composite material of one embodiment of the present invention does not contain a silane coupling agent, the price of the rubber product itself can be reduced. That is, the rubber product of one embodiment of the present invention can be said to be a superior product with both high performance and low price.

[0097] The rubber product can be manufactured, for example, by the following method: the rubber composition of one embodiment of the present invention is processed by extrusion or the like in an unvulcanized state, and molded by a common method, and then heated and pressurized in a vulcanizer to obtain a rubber product.

[0098] Examples of the rubber products include tires, rubber tracks, anti-vibration rubber, rubber belts, rubber tubes, rubber rings, seals, shoe soles, oil seals, diaphragms, rubber leather, and rubber cloth. These rubber products maintain excellent mechanical strength and low tanδ values, and thus can exert the following effects, for example: tires and rubber tracks with reduced rolling resistance can reduce fuel consumption; surface pressure on the connection parts of seals and rubber tubes with increased reaction elasticity can be maintained; and vibration resistance and buffering can be improved.

[0099] [Embodiment 2: Method for producing a silicon dioxide-carbon composite material according to an embodiment of the present invention]

[0100] A method for producing a silicon dioxide-carbon composite material according to one embodiment of the present invention comprises:

[0101] a gasification step of supplying superheated steam to the resource material derived from silicate plants to gasify a portion of carbon contained in the resource material; and

[0102] In the recovery step, the resource material residue remaining as a solid component without being gasified in the gasification step is recovered as a silica-carbon composite material.

[0103] (1) Gasification process

[0104] The following, combined Figure 1 , first, the gasification process will be described. Figure 1 The gasifier 100 is a schematic diagram of an example of a gasifier that can be used to perform a gasification process. The gasifier 100 is a two-stage cylindrical shape, and includes a gasification section 1 and a gas reforming section 2 .

[0105] The resource material is composed of a combustible component (organic component) and ash (inorganic component). In addition, the combustible component is generally divided into carbon and components other than carbon (hydrogen, nitrogen, oxygen, etc.), and the ash contains potassium as a trace component, but most of it is silicon dioxide (SiO2). After the resource material is supplied to the gasification process, a part of the carbon contained in the resource material is converted into gas (carbon monoxide and hydrogen) through the water-gas shift reaction shown in formula (1).

[0106] C+H2O→CO+H2 (1)

[0107] During the reaction, almost all of the combustible components in the resource material except carbon are transferred to the gas. In addition, depending on the conditions of the gasification process, carbon will be distributed to the gas and the resource material residue (gasification ash). The resource material residue is the part that is not gasified in the gasification process and remains in the form of a solid component. If the carbon contained in the resource material is assumed to be 100% by mass, the distribution rate of carbon to the gas is the gasification rate. Most of the ash (silicon dioxide) will be transferred to the resource material residue. Therefore, the lower the gasification rate, the more resource material residue can be produced from the same amount of resource material, and the higher the carbon concentration in the resource material residue.

[0108] like Figure 1 As shown, the resource material derived from silicate plants is first supplied to the gasification unit 1 by a screw pusher, and superheated steam is also supplied to the gasification unit 1. That is, by supplying superheated steam to the resource material derived from silicate plants, part of the carbon contained in the resource material is gasified.

[0109] The superheated steam is a gasifying agent for gasifying the resource material, and converts a portion of the carbon in the resource material into carbon monoxide and hydrogen by the reaction shown in the above formula (1). On the other hand, the carbon distributed in the resource material residue is activated by the superheated steam to become a carbon porous body, and the composite formed by the carbon porous body and silicon dioxide becomes the silicon dioxide-carbon composite material of one embodiment of the present invention.

[0110] The temperature of the superheated steam may be 100° C. or higher, and more preferably 300° C. or higher. When the temperature of the superheated steam is 100° C. or higher, the superheated steam having a temperature corresponding to the supply amount of the resource material supplied to the gasification unit 1 can be used after adjusting the supply amount of the superheated steam. As a result, the speed (gasification speed) at which the resource material is gasified can be preferably adjusted.

[0111] By adjusting the gasification rate of the resource material, the gasification rate can be adjusted, and as a result, the specific surface area of ​​the silicon dioxide-carbon composite material can reach the aforementioned preferred value. As shown in the embodiments described below, regardless of the type of the resource material, when the gasification rate is about 40% or more and 60% or less, the specific surface area of ​​the silicon dioxide-carbon composite material is the largest.

[0112] From the viewpoint of performing the gasification at a preferred speed and making the gasification rate about 40% or more and 60% or less, the temperature of the superheated water vapor is preferably 700°C or less, more preferably 600°C or less, and particularly preferably 500°C or less. Here, when the temperature of the superheated water vapor is 700°C or less, the temperature is sufficiently lower than the phase transition temperature of the crystallization of silicon dioxide. In addition, the residence time of the resource material in the gasifier 100 is sufficiently short, being 30 seconds or less. Therefore, in the gasification process, the silicon dioxide in the resource material will not be crystallized.

[0113] When the superheated steam is supplied to the gasification unit 1, it is more preferable to supply an oxidant together with the superheated steam. The water-gas shift reaction shown in formula (1) is an endothermic reaction, so a heat source is required to maintain the temperature inside the gasifier 100 at a specified value, and by supplying an oxidant, a part of the resource material reacts with the oxidant to generate heat. Therefore, the temperature inside the gasifier 100 can be easily maintained at a specified value without introducing external energy such as electric heat. Here, the maintenance of the specified temperature value can be achieved simply by supplying superheated steam, but it is easier to achieve the maintenance by using an oxidant.

[0114] The resource material residue will rise inside the gasification part 1 together with the gas (carbon monoxide and hydrogen) generated in the gasification process. The oxidant is, for example, air, oxygen, a mixed gas of oxygen and an inert gas, etc., and by adding the oxidant, the linear flow rate of the above-mentioned gas can be increased, thereby shortening the residence time of the resource material residue in the gasification furnace 100. The type of the inert gas is not particularly limited. In terms of volume ratio, the mixing ratio of oxygen to the inert gas is preferably 1:1 to 1:4.

[0115] From the viewpoint of performing the gasification at a preferred rate and making the gasification rate about 40% to 60%, the atmosphere temperature during the gasification step is preferably 700° C. or less, more preferably 600° C. or less, and particularly preferably 500° C. or less.

[0116] The superheated water steam can be obtained, for example, by high-frequency heating of water under normal pressure. Figure 1Although not shown, the superheated water vapor may be supplied to the inside of the gasification section 1 from, for example, a nozzle head of a water vapor supply section provided below the gasification section 1. In addition, the oxidant may be supplied to the inside of the gasification section 1 from, for example, a nozzle head of an oxidant supply section provided below the gasification section 1.

[0117] From the viewpoint of making the carbon in the resource material have appropriate activity, the volume ratio of the supply amount of the superheated steam supplied to the gasification unit 1 to the amount of carbon in the resource material is preferably 1 or more, more preferably 1.25 or more, and particularly preferably 1.5 or more.

[0118] From the viewpoint of optimizing the gasification rate, optimizing the residence time of the resource material residue, and performing the gasification process in an atmosphere of a specified temperature, the supply amount of the oxidant supplied to the gasification section 1 preferably satisfies: the volume ratio of oxygen in the oxidant to the amount of carbon in the resource material is less than 0.3, more preferably less than 0.2, and particularly preferably less than 0.15.

[0119] (2) Recycling process

[0120] In the recovery process, the resource material residue, i.e., the silicon dioxide-carbon composite material, is recovered. The resource material residue is moved to the gas reformer 2 together with the gas (carbon monoxide and hydrogen) generated in the gasification process. In the gas reformer 2, the carbon monoxide generated in the gasification process is subjected to a water-gas shift reaction to adjust the ratio of carbon monoxide to hydrogen.

[0121] When the buoyancy of the resource material residue becomes greater than the gravity, the mixture of the gas after the ratio adjustment and the resource material residue ("synthesis gas" in the figure) is discharged from the gas reforming unit 2 and sent to the separation mechanism (not shown). Then, the separation mechanism separates the resource material residue from the mixture and recovers it as a silicon dioxide-carbon composite material according to an embodiment of the present invention. As the separation mechanism, for example, a cyclone centrifuge can be used.

[0122] Preferably, a tar decomposition step is further included between the gasification step and the recovery step, wherein the tar contained in the resource material residue obtained in the gasification step is decomposed by placing the resource material residue in an atmosphere with a higher temperature than that of the gasification step. The quality of the silica-carbon composite material can be further improved by the tar decomposition step.

[0123] The temperature in the gas reforming section 2 can be increased by adjusting the temperature and / or supply amount of the superheated steam, adding an oxidant, etc., thereby creating the “atmosphere having a higher temperature than that of the gasification step”.

[0124] From the viewpoint of not promoting gasification and only efficiently decomposing tar, the "atmosphere at a higher temperature than the gasification process" is preferably an atmosphere exceeding 700° C. and below 800° C. That is, the tar decomposition process is preferably performed in an atmosphere exceeding 700° C. and below 800° C. If the oxidant is added, it means that the linear flow velocity of the gas is increased, thereby shortening the residence time of the resource material residue in the gasifier 100.

[0125] Here, as long as the gasification process is carried out in a high temperature atmosphere exceeding 700°C, the residual tar after the gasification process is small, thereby eliminating the tar decomposition process. However, in order to adjust the BET specific surface area of ​​the silica-carbon composite material to a desired value by the gasification rate of the resource material, the atmosphere temperature during the gasification process is preferably lower. At this time, it means that there will be more tar remaining in the resource material residue, and it is preferred to have a tar decomposition process.

[0126] The manufacturing method can manufacture the silicon dioxide-carbon composite material of one embodiment of the present invention. Whether the silicon dioxide-carbon composite material of one embodiment of the present invention is successfully manufactured can be confirmed by the following methods, etc.: using SEM to observe the resource material residue obtained in the recovery process to confirm whether a composite composed of amorphous silicon dioxide and carbon porous body is formed; as shown in the examples described below, confirm whether the resource material residue has amphiphilic molecular properties.

[0127] The silicon dioxide-carbon composite material recovered in the recovery process can be crushed as needed to adjust the average particle size (D50), and the properties of the composite can be maintained even after crushing. The crushing can be appropriately carried out using a conventionally known crusher. The preferred average particle size (D50) is the same as the above content.

[0128] The present invention includes the following aspects.

[0129] [1] A silica-carbon composite material, which is made from a resource material derived from silicic acid plants and contains a composite body composed of amorphous silica and a carbon porous body.

[0130] [2] The silica-carbon composite material according to [1], wherein 10% by mass or more and 70% by mass or less of the carbon contained in the resource material is contained in the silica-carbon composite material.

[0131] [3] The silicon dioxide-carbon composite material as described in [1] or [2], wherein the BET specific surface area is 100 m 2 / g and above 900m 2 / g or less.

[0132] [4] The silicon dioxide-carbon composite material as described in [3], wherein the BET specific surface area is 100 m2 / g and above and 350m 2 / g or less.

[0133] [5] The silica-carbon composite material according to any one of [1] to [4], wherein the average particle size (D50) is 0.1 μm or more and 10 μm or less.

[0134] [6] The silicon dioxide-carbon composite material as described in any one of [1] to [5], which has amphiphilic molecular properties.

[0135] [7] An additive for a polymer material, comprising the silicon dioxide-carbon composite material described in any one of [1] to [6].

[0136] [8] A rubber composition comprising a rubber component and the polymer material additive described in [7], wherein the content of the polymer material additive is 3 phr to 140 phr relative to the rubber component.

[0137] [9] A rubber product comprising the rubber composition described in [8].

[0138]

[10] A method for producing a silicon dioxide-carbon composite material, comprising: a gasification step of supplying superheated steam to a resource material derived from a silicate plant to gasify a portion of carbon contained in the resource material; and

[0139] In the recovery step, the resource material residue remaining as a solid component without being gasified in the gasification step is recovered as a silica-carbon composite material.

[0140]

[11] A method for manufacturing a silicon dioxide-carbon composite material as described in

[10] , wherein the gasification process and the recovery process further include: a tar decomposition process, which decomposes the tar contained in the resource material residue by placing the resource material residue obtained in the gasification process in an atmosphere with a higher temperature than that of the gasification process.

[0141] The present invention is not limited to the above-mentioned embodiments, and various changes can be made within the scope directly or indirectly disclosed in the specification. Embodiments obtained by appropriately combining technical means respectively disclosed in different embodiments are also included in the technical scope of the present invention.

[0142] [Example]

[0143] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples, but the present invention is not limited thereto.

[0144] [Example 1]

[0145] (Relationship between gasification rate and BET specific surface area of ​​silica-carbon composite material)

[0146] In this example, the gasification process in the method for manufacturing a silicon dioxide-carbon composite material according to one embodiment of the present invention was carried out with various types of resource materials as the object under the condition of correspondingly changing the gasification rate, and the BET specific surface area of ​​the obtained resource material residue (silicon dioxide-carbon composite material) was measured.

[0147] The resource materials, such as rice stalks, rice husks, sawdust, bamboo or bark, are supplied to the Figure 1 The gasification part 1 of the gasifier 100 shown in the figure is supplied with superheated steam at 400-700°C, wherein the volume ratio of the superheated steam to the carbon content in the resource material is 1-1.5, and air is also injected, wherein the volume ratio of oxygen in the air to the carbon content in the resource material is 0.1, and the temperature inside the gasification part 1 is changed accordingly within the range of 500-700°C, thereby adjusting the gasification rate.

[0148] In addition, air was injected into the gas reforming section 2, wherein the volume ratio of oxygen in the air to carbon in the resource material was 0.05. The temperature of the gas reforming section 2 was controlled at 800°C.

[0149] Next, a mixture of the gas obtained through the water-gas shift reaction and the resource material residue is discharged from the gas reforming unit 2 .

[0150] Next, a cyclone centrifuge was used to separate the resource material residue from the mixture and use it as a silicon dioxide-carbon composite material.

[0151] For each resource material used, the amount of resource material supplied, the carbon concentration of the resource material supplied, the cyclone outlet gas amount, and the carbon concentration of the cyclone outlet gas (the total value of the concentrations of CO, CO2, and CH4) were measured, and the gasification rate was calculated according to the following formula (2).

[0152] Gasification rate (%) = (amount of gas at cyclone outlet × carbon concentration of gas at cyclone outlet) / (amount of resource material supplied × carbon concentration of resource material supplied) × 100 (2)

[0153] The BET specific surface area of ​​the silica-carbon composite material was measured using a laser refraction / scattering particle size distribution analyzer (manufactured by Microtrac BEL Co., Ltd.) and plotted on a graph having the gasification rate as the horizontal axis and the BET specific surface area as the vertical axis.

[0154] Figure 2 and Figure 3This is a graph showing changes in the BET specific surface area of ​​the silica-carbon composite material according to one embodiment of the present invention, which is obtained by changing the gasification rate in the gasification step. Figure 2 The results are shown when rice stalks and husks were used. Figure 3 is Figure 2 In addition to the results shown above, a graph showing the results when sawdust, bamboo, and stem bark were used is also shown.

[0155] Here, unlike rice stalks and husks containing about 20% ash by weight, sawdust, bamboo, and stem bark have a relatively low ash content of about several % by weight, so the ratio of carbon to the total weight of the raw material is relatively high. Therefore, under the same gasification rate, the BET specific surface area can be increased when using sawdust, bamboo, and stem bark compared to the scheme using rice stalks and husks. From this point of view, Figure 3 The left vertical axis is used to express the BET specific surface area of ​​the silica-carbon composite material made of rice stalks and husks, and the right vertical axis is used to express the BET specific surface area of ​​the silica-carbon composite material made of sawdust, bamboo and stem bark.

[0156] like Figure 2 As shown in Figure 2, when rice stalks and husks are used as raw materials, the BET specific surface area of ​​the silicon dioxide-carbon composite material is the largest when the gasification rate is around 50% (40-60%). Figure 3 As shown, when sawdust, bamboo and stem bark are used as raw materials, the BET specific surface area of ​​the silicon dioxide-carbon composite material is the largest when the gasification rate is around 50% (40-60%).

[0157] It is clear from the above results that the BET specific surface area of ​​the silica-carbon composite material can be adjusted by adjusting the gasification rate regardless of the type of resource material. Figure 2 and Figure 3 The silicon dioxide-carbon composite materials having the BET specific surface areas shown all belong to the silicon dioxide-carbon composite materials according to one embodiment of the present invention.

[0158] [Example 2]

[0159] (Relationship between gasification rate and yield and composition of silica-carbon composite material)

[0160] As mentioned above, the lower the gasification rate of the gasification process, the more resource material residue, that is, the amount of the silica-carbon composite material in one embodiment of the present invention, that can be obtained from the same amount of resource material, and the higher the carbon concentration in the silica-carbon composite material. In this regard, in this embodiment, the experimental bench was used to analyze the changes in the yield and composition of the silica-carbon composite material when the gasification rate was changed to various values.

[0161] Regarding the composition of rice husks, we quantitatively analyzed the combustible content, ash content, carbon concentration, silica concentration, and potassium concentration of rice husks collected from 10 regions across Japan, and took the average values ​​of each. The combustible content is the percentage of weight loss after the rice husks are spread thinly on a magnetic dish and heated at 800°C for 2 hours in an electric muffle furnace, and the ash content is the value obtained by subtracting the combustible content from 100. The carbon concentration was analyzed using a CHN decoder, the silica concentration was analyzed using an alkali dissolution-gravimetric method, and the potassium concentration was analyzed using an acid decomposition-atomic absorption method.

[0162] At each gasification rate in the range of 30 to 90%, the carbon transferred to the gas at a ratio corresponding to the gasification rate was regarded as the carbon contained in the combustible component, and the elements other than carbon transferred in their entirety to the gas in the gasifier were regarded as the elements other than carbon contained in the combustible component. The silicon dioxide and potassium transferred in their entirety to the resource material residue were regarded as the silicon dioxide and potassium contained in the ash. Based on this assumption, the amount and composition of the resource material residue under the condition of a gasification rate of 30 to 90% were calculated.

[0163] Figure 4 and Figure 5 This is a graph showing the results of determining the amount and composition of the resource material residue when the gasification rate of the gasification process is changed accordingly. Figure 4 This is a graph showing the composition of gas and resource material residue when the gasification rate is 30% to 90%. Figure 5 It is a graph showing the husk composition, the amount of resource material residue yield when the gasification rate is 30% to 90%, and the resource material residue composition.

[0164] For example, Figure 5 As shown in FIG. 1 , when the gasification rate is 90%, the average yield of the resource material residue per ton of husk is 235 kg, and the carbon concentration of the resource material residue is 16% by weight. On the other hand, as the gasification rate decreases, the yield and carbon concentration increase. When the gasification rate is 60%, the average yield per ton of husk is 349 kg, and the carbon concentration is 44%, and when the gasification rate is 50%, the average yield per ton of husk is 387 kg, and the carbon concentration is 49%.

[0165] It is obvious from the above results that the lower the gasification rate, the more resource material residue can be produced from the same amount of resource material, that is, the amount of silica-carbon composite material of one embodiment of the present invention, and the higher the carbon concentration in the silica-carbon composite material.

[0166] [Example 3]

[0167] (1) Confirmation of the composite composed of amorphous silicon dioxide and carbon by SEM

[0168] Using rice husk as a raw material, the gasification rate was adjusted to 70% in Example 1, and a silicon dioxide-carbon composite material according to an embodiment of the present invention was manufactured under this condition, and the composite material was observed using a SEM. Figure 6 and Figure 7 This is the SEM observation result of the silicon dioxide-carbon composite material that has not been crushed. Figure 6 This is the observation result at a magnification of 100 times. Figure 7 This is the observation result at a magnification of 500 times. Figure 8 This is a SEM observation result of a silica-carbon composite material that has been pulverized to have an average particle size (D50) of about 1 μm.

[0169] Here, the pulverization treatment was performed as follows: using a planetary ball mill (manufactured by FRITSCH), resource material residues and agate beads having a diameter of 10 mm were placed in an agate container and pulverized for 5 minutes.

[0170] like Figures 6 to 8 As shown, the silicon dioxide-carbon composite material has a random shape derived from the husk shape as a whole. In addition, in particular, in the silicon dioxide-carbon composite material after the pulverization process, it can be clearly observed that a large number of small house-shaped particles are condensed and attached to the block-like large particles.

[0171] (2) Mapping analysis using electron probe microanalyzer (EPMA)

[0172] The pulverized silica-carbon composite material used in the above column (1) was analyzed by EPMA. Figure 8 The specific part shown was subjected to mapping analysis to investigate the main components of the specific part. As EPMA, SEM-EPMA 8530F (manufactured by JEOL Ltd.) was used.

[0173] Fig. 9 Observed at 14 times magnification Figure 8 The SEM photograph of the large block particles is shown, in which the cross-marked area is the area where mapping analysis was performed. Fig.10 The mapping analysis results of the blocky large particles are shown.

[0174] in addition, Fig.11 Observed at 14 times magnification Figure 8 The SEM photograph of the room-shaped small particles is shown, in which the cross mark is the location where mapping analysis was performed. Fig.12 The mapping analysis results of the room-shaped small particles are shown.

[0175] The measurement conditions for mapping analysis are shown in Fig.10 and Fig.12 In. Fig.10As shown in FIG. 1 , it can be seen that the large block particles contain more (75.54 mass %) carbon (C). Fig.12 As shown, it can be seen that the small house-shaped particles contain a large amount (65.67% by mass) of silicon dioxide (Si, O). However, the large block particles and the small house-shaped particles are not composed of a single carbon component or a single silicon dioxide component. In other words, it is confirmed that the large block particles and the small house-shaped particles are composite particles formed by carbon and amorphous silicon dioxide.

[0176] [Example 4]

[0177] (Amphiphilic Molecular Properties of the Silica-Carbon Composite Material According to One Embodiment of the Present Invention)

[0178] In this example, it was confirmed that the silicon dioxide-carbon composite material according to one embodiment of the present invention has amphiphilic molecular properties.

[0179] As a silica-carbon composite material according to one embodiment of the present invention, a silica-carbon composite material made from rice husks and containing 45% by mass of carbon and 55% by mass of amorphous silica is used, and its composition is determined by the aforementioned mapping analysis.

[0180] Prepare 2 screw-cap bottles (volume 13.5 ml), add 5 ml of toluene and 5 ml of distilled water to both screw-cap bottles. Then, add 0.1 g of the silica-carbon composite material to one screw-cap bottle. In the other screw-cap bottle, add 0.0055 g of commercially available silica (Zeosil 1165MP manufactured by Rhodia) and 0.045 g of commercially available carbon black (ASTM number: N220) as comparison objects. That is, the silica-carbon composite material has the same ratio of components as the comparison object. Next, irradiate each screw-cap bottle with ultrasound for 10 minutes and then let it stand for 1 day.

[0181] 〔Table 1〕

[0182]

[0183] ※The information in brackets is the distribution ratio of the substance

[0184] The results are shown in Table 1 and Fig.13 shown. Fig.13 : This is a photograph showing that the silicon dioxide-carbon composite material according to one embodiment of the present invention has amphiphilic molecular properties. The left side is a screw-cap bottle to which the silicon dioxide-carbon composite material according to one embodiment of the present invention is added, and the right side is a screw-cap bottle to which a comparison object is added.

[0185] In the case of the silica-carbon composite material according to one embodiment of the present invention, toluene and distilled water remain in an emulsion state even after standing for 1 day. On the other hand, in comparison, the liquid is separated into two phases, i.e., the hydrophilic silica is separated into the water phase (lower phase), and the hydrophobic carbon black is separated into the oil phase (upper phase). It is obvious from this result that the silica-carbon composite material according to one embodiment of the present invention is not a simple mixture of silica and carbon, but is formed into a complex composed of amorphous silica and carbon, thereby showing amphiphilic molecular properties.

[0186] [Example 5]

[0187] (Physical properties of the rubber composition according to one embodiment of the present invention)

[0188] (1) Preparation of rubber composition, etc.

[0189] In this example, the components shown in Table 2 were kneaded with the components shown in Table 2 to prepare test pieces of the rubber composition according to one embodiment of the present invention, and various physical properties thereof were measured.

[0190] 〔Table 2〕

[0191]

[0192] The "silicon dioxide-carbon composite material" in the table refers to a silica-carbon composite material according to one embodiment of the present invention, which is prepared using rice husk as a raw material and adjusting the gasification rate to 70% in Example 1. In the table, the values ​​"1μm", "3μm", and "5μm" are the average particle sizes (D50) of the silica-carbon composite material. The average particle size (D50) is a value measured using a laser refraction and scattering particle size distribution measuring device (manufactured by Microtrac BEL Co., Ltd.). "Nipsil VN-3" is a conventionally known silica product. The values ​​in Table 2 are the weight parts of each component relative to 100 parts by weight of RSS#1 (natural rubber). Columns such as "Ratio 1" indicate the blending components of the comparison composition used in Comparative Example 1, etc., and columns such as "Actual 1" indicate the blending components of the rubber composition used in Example 1, etc.

[0193] The preparation process of the rubber composition of the embodiment is as follows. A LABOPLASTOMILL (registered trademark) Banbury mixer B600 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) was used for the following single kneading and mixing. First, the natural rubber was single kneaded for 20 seconds. Secondly, the silica-carbon composite material, anti-aging agent, microcrystalline wax and stearic acid of one embodiment of the present invention were added to the single kneaded natural rubber and mixed for 30 seconds. As shown in Table 2, a silane coupling agent was also added to Examples 1 to 3, 7, and 9.

[0194] Carbon black was added to the obtained kneaded product and kneaded for 30 seconds, and then washed and kneaded for another 30 seconds. The obtained kneaded product was washed again, and then heated to 160°C ± 3°C and kneaded for more than 60 seconds, and then the kneaded product was discharged from the mixer. The obtained kneaded product was referred to as kneaded product 1.

[0195] When preparing the mixed material 1, the initial setting temperature of the stirrer was 80° C. and the rotor speed was 60 to 100 rpm.

[0196] After the kneaded product 1 was passed through the rollers, it was cooled at room temperature. Then, zinc oxide, sulfur and a vulcanization accelerator were added to the kneaded product 1, and the mixture was kneaded for more than 90 seconds while being heated to 115°C ± 3°C, and then discharged from the mixer. The obtained kneaded product was referred to as kneaded product 2.

[0197] When preparing the kneaded product 2, the initial setting temperature of the stirrer was 80°C, and the rotor speed was 40 to 100 rpm. The blending ratio was the same as that when preparing the kneaded product 1.

[0198] Here, in Comparative Example 1, silica and a silane coupling agent were used instead of the silica-carbon composite material according to one embodiment of the present invention, and in Comparative Example 2, carbon black was used alone instead of the silica-carbon composite material according to one embodiment of the present invention.

[0199] The kneaded material 2 was press-molded at a pressing temperature of 160° C. for a pressing time shown in Table 3 using an electric hot press manufactured by Ohtake Machinery Industry Co., Ltd., thereby producing a test piece.

[0200] 〔Table 3〕

[0201] Real 1 Real 2 Reality 3 Reality 4 Reality 5 Actual 6 Real 7 Actual 8 Actual 9 Actual 10 2mmt piece (minute) 5 5 5 5 5 4 5 5 5 6 Wear test piece (minutes) 10 10 10 10 10 9 10 10 10 11

[0202] In the table, the column "wear test piece" indicates the pressurization time of the test piece used in the post-Payne effect measurement test, and the column "2mmt piece" indicates the pressurization time of the test piece used in the durometer hardness test.

[0203] (2) Physical property measurement

[0204] Next, the tests (a) to (f) below were carried out using the prepared test pieces.

[0205] (a) Vulcanization test

[0206] The vulcanization degree test was conducted under the following conditions based on Japanese Industrial Standard JIS J 6300-2, 2001 "Unvulcanized rubber - Physical properties - Part 2: Determination of vulcanization properties by oscillating vulcanization testing machine".

[0207] <Test conditions>

[0208] Test method: Impact mode vulcanization test method A (torsion oscillation type flat plate impact mode vulcanization test)

[0209] Test temperature: 160℃

[0210] Test time: 30 minutes

[0211] Amplitude angle: ±1°

[0212] Oscillation frequency: 1.67Hz (100cpm)

[0213] Tester used: VR3110 FDR tester manufactured by Ueshima Manufacturing Co., Ltd.

[0214] (b) Mooney viscosity test

[0215] The Mooney viscosity was measured under the following conditions based on JIS K 6300-1, 2005 "Unvulcanized rubber - Physical properties - Part 1: Viscosity and scorch time by Mooney viscometer".

[0216] <Test conditions>

[0217] Test temperature: 100℃

[0218] Rotor type: L-shaped

[0219] Testing machine used: Shimadzu Mooney Viscometer SMV-301RT manufactured by Shimadzu Corporation

[0220] (c) Durometer hardness test

[0221] Based on JIS K 6253-3, 2012 "Rubber, vulcanized and thermoplastic - Methods for determination of hardness - Part 3: Hardness measured by a durometer", a durometer hardness test was conducted under the following conditions.

[0222] <Test conditions>

[0223] Test piece preparation method: After the test piece is prepared by press forming, it is punched out.

[0224] Test piece shape: sheet (3 test pieces with a thickness of about 2 mm are stacked)

[0225] Test equipment: ASKER rubber hardness tester (hardness tester) type A manufactured by Kobunshi Keiki Co., Ltd.

[0226] (d) Tensile test

[0227] The tensile test was conducted under the following conditions based on JIS K 6251, 2010 “Rubber, vulcanized and thermoplastic rubber – Methods for determination of tensile properties”.

[0228] <Test conditions>

[0229] Test piece preparation method: After preparing the test piece by pressurized vulcanization, punching is performed

[0230] Test piece shape: No. 3 dumbbell

[0231] Test piece collection direction: parallel to the texture

[0232] Number of test pieces: 3

[0233] Measurement temperature: 23°C

[0234] Test speed: 500mm / min

[0235] Testing machine used: AUTOGRAPH EZ-LX, 1kN, precision universal testing machine manufactured by Shimadzu Corporation

[0236] Testing machine capacity: load cell type, 1kN

[0237] (e) Tensile test

[0238] Based on JIS K 6252:2007 “Rubber, vulcanized and thermoplastic rubber-Determination of tensile strength”, a tensile test was carried out under the following conditions.

[0239] <Test conditions>

[0240] Test piece preparation method: After the test piece is prepared by press forming, it is punched out.

[0241] Test piece shape: Angle shape without cuts

[0242] Test piece collection direction: perpendicular to the texture

[0243] Number of test pieces: 5

[0244] Test temperature: 23℃

[0245] Test speed: 500mm / min

[0246] Testing machine used: Auto Graph EZ-LX, a precision universal testing machine manufactured by Shimadzu Corporation, 1kN

[0247] Testing machine capacity: load cell type, 1kN

[0248] (f) Determination of Payne effect after vulcanization

[0249] Based on ISO 13145:2012 "Rubber-Determination of viscosity and stress relaxation using a rotorless sealed shear rheometer", the Payne effect after vulcanization was measured under the following conditions.

[0250] <Test conditions>

[0251] Measurement items: Dynamic shear storage modulus G', dynamic shear loss modulus G", loss tangent tanδ

[0252] Test machine used: RPA2000 manufactured by ALPHA TECHNOLOGIES

[0253] Measurement process: as shown in Table 4. In the dynamic deformation measurement under condition 4, the measurement was terminated at the time point when the torque limit was exceeded.

[0254] 〔Table 4〕

[0255] condition Temperature(℃) Measurement time (min) Dynamic deformation (%) Frequency (Hz) Exam Preparation 1 160 0 - - Ready 2 160 4~6 0 0 Delay 3 60 10 0.07 0.5 Timed 4 60 - 0.07→650 0.5 Strain sweep

[0256] The results are shown in Table 5. In Comparative Example 1, amorphous silica and carbon black were blended into natural rubber, and a silane coupling agent was used to improve the affinity of amorphous silica to natural rubber. That is, the composition used in Comparative Example 1 is a composition obtained by blending amorphous silica into a rubber component by a method widely used in the past.

[0257] In the table, the "minimum torque" corresponding to the vulcanization test is an indicator of the viscosity of the rubber composition, and the "maximum torque" is an indicator of the strength of the rubber composition. In addition, T10 represents the ease of curing of the rubber composition, which is an indicator of processing safety and productivity. If this time is too short, it means that production is difficult. In addition, the longer T10 is, the more difficult it is to start vulcanization. T90 represents the molding time of the rubber composition.

[0258] Mooney viscosity is an indicator of the processability of the rubber composition. The smaller its value, the easier it is to process. Durometer hardness is an indicator of the hardness of the rubber composition. The larger its value, the higher its strength. "Tb×Eb" corresponding to the tensile test is the product of tensile strength and elongation. "Tensile product" represents the fracture energy of the rubber composition. The larger its value, the greater the energy required to destroy the rubber composition. "M100" is the stress required to stretch the rubber composition by 100%, and "M300" is the stress required to stretch the rubber composition by 300%. "M300 / M100" is an indicator of the dispersibility of the filler in the rubber component. The larger its value, the better the dispersibility.

[0259] The tear strength is an index that expresses how difficult it is for a rubber composition to tear when subjected to concentrated stress. The Payne effect is an index of the fuel efficiency when a rubber composition is used in a tire, and the smaller the value, the better the fuel efficiency.

[0260] 〔Table 5〕

[0261]

[0262] In Examples 1 to 3, a silane coupling agent was added to the silica-carbon composite material according to one embodiment of the present invention, and in Examples 4 to 6, the same silica-carbon composite material as in Examples 1 to 3 was used, but no silane coupling agent was added. In addition, a silane coupling agent was also added in Examples 7 and 8, and no silane coupling agent was added in Examples 9 and 10.

[0263] As can be seen from Table 5, the test results of Examples 1 to 3, 7, and 9 are equivalent to those of Comparative Example 1. In addition, the test results of Examples 4 to 6, 8, and 10 are equivalent to those of Examples 1 to 3, 7, and 9, respectively.

[0264] Although the blending amount of the silica-carbon composite material was changed in each of Examples 1 to 3 and Examples 4 to 6, it can be seen that even if the blending amount was increased, there was no significant decrease in tensile strength with the increase in the blending amount. In addition, the tensile strength values ​​of Examples 1 and 4, where the blending amount was 10 parts by weight, exceeded the tensile strength value of Comparative Example 1.

[0265] That is, it is clear that the silica-carbon composite material according to one embodiment of the present invention can exhibit strength equal to or better than that of a conventional rubber composition using amorphous silica, and can fully exhibit the characteristics required of a rubber composition such as the Payne effect. In particular, according to the results of Examples 4 to 6, 8, and 10, it can be seen that when the silica-carbon composite material according to one embodiment of the present invention is used, satisfactory results can be obtained in terms of the strength and characteristics without using a silane coupling agent.

[0266] If the silica-carbon composite material is a mixture consisting simply of silica and carbon, then in the absence of a silane coupling agent, the affinity of silica for carbon will decrease, and therefore it is believed that it will not show the results of Examples 4 to 6, 8, and 10. That is, it can be said that the reason for the results of Examples 4 to 6, 8, and 10 is that the amorphous silica and carbon in the silica-carbon composite material do not exist in a simple mixed state, but form a complex.

[0267] [Industrial Applicability]

[0268] The invention can be preferably used for rubber products such as tires.

Claims

1. A method for producing a silicon dioxide-carbon composite material having amphiphilic molecular properties, in, The method for preparing the silicon dioxide-carbon composite material having amphiphilic molecular properties comprises: a gasification step of supplying superheated steam at a temperature of 100° C. to 700° C. and an oxidant to a resource material derived from a silicic acid plant, thereby gasifying a portion of carbon contained in the resource material at a gasification rate of 40% to 60%; and a recovery step of recovering the resource material residue remaining as a solid component that has not been gasified in the gasification step as a silicon dioxide-carbon composite material; The resource material resides in the gasification furnace during the gasification step for 30 seconds or less.

2. The method for producing the amphiphilic silicon dioxide-carbon composite material according to claim 1, in, The recycling process is the following process: The resource material residue is moved to the gas reforming section together with the gas generated in the gasification process, and the gas reforming section is used to perform a water-gas shift reaction on the carbon monoxide generated in the gasification process. When the buoyancy of the resource material residue is greater than the gravity, the mixture of the gas obtained through the water-gas shift reaction and the resource material residue is discharged from the gas reforming section and sent to a separation mechanism, and the separation mechanism is used to separate the resource material residue from the mixture and recover it as a silicon dioxide-carbon composite material.

3. A method for producing an amphiphilic silicon dioxide-carbon composite material according to claim 1 or 2, in, The gasification process and the recovery process also include: The tar decomposition step is to decompose the tar contained in the resource material residue obtained in the gasification step by placing the resource material residue in an atmosphere having a higher temperature than that in the gasification step.

4. The method for producing the amphiphilic silicon dioxide-carbon composite material according to claim 3, in, In the tar decomposition step, an oxidizing agent is supplied.

5. A method for producing a rubber composition, in, The method for producing a rubber composition comprises the steps of kneading at least a polymer material additive containing an amphiphilic silica-carbon composite material produced by the production method according to any one of claims 1 to 4 and a rubber component and then vulcanizing the mixture.

6. A silicon dioxide-carbon composite material having amphiphilic molecular properties, in, The silicon dioxide-carbon composite material having amphiphilic molecular properties is a silicon dioxide-carbon composite material having amphiphilic molecular properties produced by the production method according to any one of claims 1 to 4. The silicon dioxide-carbon composite material having amphiphilic molecular properties is made of a resource material derived from silicic acid plants and contains a composite body composed of amorphous silicon dioxide and a carbon porous body.

7. The silicon dioxide-carbon composite material having amphiphilic molecular properties according to claim 6, in, The BET specific surface area of ​​the silicon dioxide-carbon composite material with amphiphilic molecular properties is 100 m 2 / g and above 900m 2 / g or less.

8. The silicon dioxide-carbon composite material having amphiphilic molecular properties according to claim 7, in, The BET specific surface area is 100 m 2 / g and above and 350m 2 / g or less.

9. The silicon dioxide-carbon composite material having amphiphilic molecular properties according to claim 6, in, The average particle size D50 of the amphiphilic silica-carbon composite material is 0.1 μm or more and 10 μm or less.

10. An additive for polymer materials, in, The polymer material additive contains the silicon dioxide-carbon composite material having amphiphilic molecular properties as claimed in any one of claims 6 to 9.

11. A rubber composition, in, The rubber composition contains a rubber component and the polymer material additive according to claim 10, The content of the polymer material additive is 3 phr or more and 140 phr or less relative to the rubber component.

12. A rubber product, in, The rubber product contains the rubber composition according to claim 11.