A NiCo2O4@wood ear carbon aerogel composite material and its preparation method and application
By combining NiCo2O4 nanostructure on the fungus carbon aerogel, adjusting the morphology and impedance matching, the problem of insufficient absorption performance of low-frequency electromagnetic waves in the existing technology is solved, and efficient low-frequency electromagnetic wave absorption is achieved, satisfying 4G and 5G communications and military use Radar demand.
Patent Information
- Application Number
- CN202111288005.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-11-02
AI Technical Summary
The existing technology is difficult to develop materials with high-efficiency low-frequency electromagnetic wave absorption performance, especially in the 4G and 5G communication technology and military radar bands. There is little research on the morphology adjustment of traditional carbon materials and biomass materials and the geometric morphology of composite materials, resulting in absorption. Inadequate wave performance.
By combining and distributing NiCo2O4 nanostructures in situ on the fungus carbon aerogel, NiCo2O4@ fungus carbon aerogel composites are prepared by heat treatment and hydrothermal synthesis methods, and their morphology and impedance matching characteristics are adjusted to achieve efficient absorption of low-frequency electromagnetic waves. .
It realizes composite materials with excellent wave absorption performance in the low frequency band (2-8GHz), meets the needs of wireless communications and military radar for low frequency electromagnetic wave absorption, and provides a stable and controllable preparation method and efficient absorption performance.
Smart Images

Figure CN113840529B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to electromagnetic absorption materials in the field of functional materials, and particularly to a NiCo 2 O 4 @agar carbon aerogel composite material, its preparation method and application. This composite material can be obtained through simple heat treatment and in-situ chemical synthesis, and has stable and excellent low-frequency electromagnetic wave absorption performance. Background Art
[0002] At present, the rapid development of wireless communication and the continuous popularization of intelligent driving vehicles have brought convenience to the fast-paced society. While enjoying these conveniences, a large number of electronic devices have greatly increased electromagnetic radiation, causing serious electromagnetic pollution problems. Subsequently, there are harms to human health and the natural environment, as well as interference to other devices, and even affecting national security or causing major accidents. Considering the effective purification of harmful electromagnetic waves, researchers have successfully developed a series of electromagnetic wave absorption materials. Currently, the research mainly focuses on the absorption of high-frequency electromagnetic waves, such as the X and Ku bands (8 - 18 GHz). However, the development of 4G and 5G communication technologies means that the development of efficient electromagnetic wave absorbers in the low-frequency band (2 - 8 GHz) has become a key research direction in the field of electromagnetic pollution protection. In addition, the working frequency bands of various military radars have gradually expanded to the low-frequency range. Therefore, it is very necessary to develop new electromagnetic wave absorbers that can achieve efficient absorption at low frequencies.
[0003] Due to the stability, light weight, and good electrical conductivity of carbonaceous materials, their research as electromagnetic wave absorbers has received increasing attention. In addition to the usual one-dimensional carbon materials (carbon fibers and carbon nanotubes) and two-dimensional carbon materials (graphene oxide and MXene), three-dimensional porous carbon materials are also potential candidate materials, such as expandable graphite and carbon aerogels. Moreover, many biomass materials have also been explored as excellent templates for preparing new porous carbon materials. Specifically, biomass contains a large amount of organic matter and has various unique structural forms. After high-temperature pyrolysis treatment, it can be used as an effective matrix for electromagnetic wave absorbers. More importantly, a series of advantages such as availability, rich sources, environmental friendliness, and renewable nature have greatly enhanced its practical value. So far, most of the research on biomass-derived carbon absorbers has focused on the control of carbonization temperature and composition, while the geometric morphology of composite materials has rarely been studied. It has been found that morphology regulation is an effective way to obtain the best wave absorption performance. Therefore, adjusting the morphology of biomass-derived carbon-based composite materials may provide inspiration for further improving their wave absorption performance.
[0004] In addition, the microwave absorption performance of single-component material systems is limited by impedance mismatch. To achieve outstanding microwave absorption performance, carbon materials need to be combined with magnetic loss materials to optimize impedance matching. Spinel ferrites have been extended to various fields due to their high conductivity, abundant resources, environmental friendliness, and low cost. In addition, their low Snell's limit, moderate saturation magnetization, appropriate low-frequency natural resonance, and dual loss mechanisms make them have good development in the field of microwave absorption, especially in the low-frequency range. Nickel cobaltite (NiCo 2 O 4 ) is a typical spinel ferrite and is a popular absorption material due to its advantages such as a designable morphology, large magnetic anisotropy, and strong polarization ability. The above theories and experiments predict that NiCo2O4 can be used to improve the limitations of pure carbon absorbers.
[0005] Here, we fabricated four different morphologies of nickel cobalt precursors (dandelion-like, sea urchin-like, tremella-like, and rose-like) on Auricularia carbon aerogels, and after annealing, we obtained C@NiCo 2 O 4 hybrids (C@NCO) with the same expected morphologies. By adjusting the morphology, the electromagnetic parameters, attenuation ability, and impedance matching characteristics were successfully controlled, and excellent microwave absorption performance was achieved: at 4.88 GHz, the minimum reflection loss (RL) was -54.6 dB, the thickness was 4.09 mm, and the effective absorption bandwidth (EAB) covered 5.7 GHz at 1.85 mm. The absorber achieved strong electromagnetic wave absorption in the S and C bands and also met the requirements for effective absorption in the X and Ku bands. The outstanding microwave absorption performance benefited from the combined effects of dipole polarization, interfacial polarization, magnetic loss, conduction loss, and antenna structure. This work provides inspiration for the development of high-performance electromagnetic wave absorption materials with tunable effective frequencies, especially in low frequencies such as the C and S bands.
[0006] In summary, the development of a simple method for preparing a NiCo 2 O 4 @Auricularia carbon aerogel composite material is of great significance for the development and production of microwave absorption materials. Summary of the Invention
[0007] To solve the technical problems existing in the prior art, the present invention provides a NiCo2O4@Auricularia carbon aerogel composite material, its preparation method, and its application.
[0008] The technical solution adopted by the present invention is a NiCo 2 O 4 @Auricularia carbon aerogel composite material. The composite material uses Auricularia carbon aerogel of biomass-derived porous carbon as the raw material, and NiCo is uniformly distributed in-situ on the Auricularia carbon aerogel 2O 4 Nanostructure.
[0009] The present invention also provides a NiCo 2 O 4 A method for preparing a wood ear carbon aerogel composite material comprises the following steps:
[0010] Step A1: Dissolve 1 mmol nickel nitrate hexahydrate, 2 mmol cobalt nitrate hexahydrate, and 12 mmol additive in 30 ml deionized water and stir for 10 minutes to form a uniform NiCo 2 O 4 Solution;
[0011] Step A2: Add the wood ear carbon aerogel to the uniform solution obtained in A1, continue stirring for 6 hours, pour into 50 ml polytetrafluoroethylene lining, put into a stainless steel autoclave, heat to 120°C by hydrothermal heating, keep warm for 6 hours, and then cool to room temperature;
[0012] Step A3: The product prepared in step A2 was filtered and washed three times with deionized water and anhydrous ethanol respectively, and placed in an oven at 60° C. for 24 hours.
[0013] Step A4: heat-treat the product obtained in step A3 in air at a temperature of 350°C, a heating rate of 1°C / min, a holding time of 120 minutes, and then cool to room temperature in the furnace.
[0014] Preferably, the additive is one of urea and hexamethylenetetramine.
[0015] Preferably, 6 mmol of ammonium fluoride may be added in step A1.
[0016] The method for preparing the wood ear carbon aerogel of the present invention comprises the following steps:
[0017] Step B1: ultrasonically clean the fungus with deionized water and anhydrous ethanol for 3 times, each time for 10 minutes, and place it in a 60°C oven to dry for 24 hours;
[0018] Step B2: Soak the fungus obtained in step B1 in 60 ml of deionized water for 1 hour, then transfer it to a polytetrafluoroethylene-lined container, put it into a stainless steel autoclave, heat it to 120° C. by hydrothermal heating, keep it warm for 10 hours, and then cool it to room temperature to obtain a fungus gel solution;
[0019] Step B3: ultrasonically treating the fungus gel solution obtained in step B2 for 2 hours, freezing the obtained uniform gel at -85°C overnight, and vacuum freeze-drying for 72 hours to obtain fungus aerogel;
[0020] Step B4: heat-treating the wood ear aerogel obtained in step B3 in an inert gas atmosphere at a temperature of 600° C., a heating rate of 5° C. / min, and a holding time of 120 min, and then cooling to room temperature to obtain wood ear carbon aerogel.
[0021] Preferably, the wood ear carbon aerogel and NiCo 2 O 4 The mass ratio of the solution is 1:1.
[0022] Preferably, the inert gas in step B4 is one of argon and nitrogen.
[0023] At the same time, the present invention provides a NiCo 2 O 4 @The application of wood ear carbon aerogel composite materials in low frequency electromagnetic wave absorption.
[0024] The present invention has the following advantages: using wood ear aerogel as raw material, obtaining biomass-derived porous carbon by pyrolysis carbonization method, and then in-situ compounding uniformly distributed NiCo on carbon aerogel by two-step experiments of hydrothermal and heat treatment in air. 2 O 4 Nanostructure. By regulating the synthesis reagents, NiCo with different nanomorphologies was rationally constructed. 2 O 4 @Auricularia aerogel-derived carbon composite material (C@NCO) has high-efficiency low-frequency electromagnetic wave absorption performance. Experiments have shown that the preparation method of the composite material is stable and controllable, simple and easy to operate, and the prepared composite material has strong absorption at low frequencies, a wide effective absorption band and a thin absorption thickness, which meets the requirements of the current society where wireless communication technology is prevalent for low-frequency and high-efficiency absorption of electromagnetic wave absorbing materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 .XRD patterns of Examples 1-4 and Comparative Examples. DETAILED DESCRIPTION
[0026] The present invention will be further described in detail below in conjunction with the embodiments of the accompanying drawings. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention and do not have any limiting effect on the present invention.
[0027] The present invention provides the following specific implementation schemes, discloses the performance of various combination embodiments, and analyzes the role of various experimental parameters in the system. Therefore, it should be considered that this patent specifically records and discloses all possible combinations of the technical solutions.
[0028] Embodiment 1:
[0029] In this embodiment, the product obtained is NiCo2 O 4 @Auricularia aerogel composite material.
[0030] The above NiCo 2 O 4 The preparation method of the wood ear aerogel composite material is as follows:
[0031] (1) The fungus was ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 minutes, and then placed in a 60°C oven for 24 hours;
[0032] (2) Soaking the fungus obtained in step (1) in 60 ml of deionized water for 1 hour, then transferring it to a 100 ml polytetrafluoroethylene-lined autoclave, placing it in a stainless steel autoclave, heating it to 120° C. by hydrothermal heating, keeping it warm for 10 hours, and then cooling it to room temperature to obtain a fungus gel solution;
[0033] (3) ultrasonically treating the wood ear gel solution obtained in step (2) for 2 hours, freezing the obtained uniform gel at -85°C overnight, and vacuum freeze-drying for 72 hours to obtain wood ear aerogel;
[0034] (4) heat treating the fungus aerogel obtained in step (3) in an argon atmosphere at a temperature of 600°C, a heating rate of 5°C / min, a holding time of 120min, and cooling to room temperature to obtain fungus carbon aerogel;
[0035] (5) Dissolve 1mmol nickel nitrate hexahydrate, 2mmol cobalt nitrate hexahydrate, and 12mmol urea in 30ml deionized water and stir for 10min to form a uniform NiCo 2 O 4 Solution;
[0036] (6) Adding the wood ear carbon aerogel obtained in step (4) to the uniform solution obtained in step (5), the wood ear carbon aerogel and NiCo 2 O 4 The mass ratio of the solution is 1:1; continue stirring for 6 hours, pour into 50 ml of polytetrafluoroethylene lining, put into a stainless steel autoclave, heat to 120°C by hydrothermal heating, keep warm for 6 hours, and then cool to room temperature;
[0037] (7) The product prepared in step (6) was filtered and washed three times with deionized water and anhydrous ethanol respectively, and placed in an oven at 60° C. for 24 hours;
[0038] (8) The product obtained in step (7) was heat treated in air at a temperature of 350°C, a holding time of 120 min, a heating rate of 1°C / min, and then cooled to room temperature in the furnace.
[0039] The above-obtained product was tested as follows:
[0040] (A) The irradiation source is Cu-Kα ( λ =1.54 Å) was used to determine the crystal structure of the sample.
[0041] (B) Electromagnetic parameters of complex permittivity and complex permeability were measured by the coaxial line method using a 3672B-S vector network analyzer in the frequency range of 2-18 GHz. Test sample preparation: The product was uniformly dispersed in paraffin wax, accounting for 50% of the total weight, and then pressed into a ring (outer diameter: 7.0 mm, inner diameter 3.04 mm).
[0042] Embodiment 2:
[0043] In this embodiment, the product obtained is NiCo 2 O 4 @Auricularia aerogel composite material.
[0044] The above is NiCo 2 O 4 The preparation method of the wood ear aerogel composite material is as follows:
[0045] (1) The fungus was ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 minutes, and then placed in a 60°C oven for 24 hours;
[0046] (2) Soaking the fungus obtained in step (1) in 60 ml of deionized water for 1 hour, then transferring it to a 100 ml polytetrafluoroethylene-lined autoclave, placing it in a stainless steel autoclave, heating it to 120° C. by hydrothermal heating, keeping it warm for 10 hours, and then cooling it to room temperature to obtain a fungus gel solution;
[0047] (3) ultrasonically treating the wood ear gel solution obtained in step (2) for 2 hours, freezing the obtained uniform gel at -85°C overnight, and vacuum freeze-drying for 72 hours to obtain wood ear aerogel;
[0048] (4) heat treating the fungus aerogel obtained in step (3) in an argon atmosphere at a temperature of 600°C, a heating rate of 5°C / min, a holding time of 120min, and cooling to room temperature to obtain fungus carbon aerogel;
[0049] (5) Dissolve 1mmol nickel nitrate hexahydrate, 2mmol cobalt nitrate hexahydrate, 12mmol urea and 6mmol ammonium fluoride in 30ml deionized water and stir for 10min to form a uniform NiCo 2 O 4 Solution;
[0050] (6) Adding the wood ear carbon aerogel obtained in step (4) to the uniform solution obtained in step (5), the wood ear carbon aerogel and NiCo 2 O 4 The mass ratio of the solution was 1:1. After stirring for 6 hours, the mixture was poured into a 50 ml polytetrafluoroethylene-lined autoclave, placed in a stainless steel autoclave, heated to 120°C by hydrothermal heating, kept at this temperature for 6 hours, and then cooled to room temperature.
[0051] (7) The product prepared in step (6) was filtered and washed three times with deionized water and anhydrous ethanol respectively, and placed in an oven at 60° C. for 24 hours;
[0052] (8) The product obtained in step (7) was heat treated in air at a temperature of 350°C, a holding time of 120 min, a heating rate of 1°C / min, and then cooled to room temperature in the furnace.
[0053] The above-prepared product was tested, and the testing method and testing content were exactly the same as those in Example 1.
[0054] Embodiment 3:
[0055] In this embodiment, the product obtained is NiCo 2 O 4 @Auricularia aerogel composite material.
[0056] The above is NiCo 2 O 4 The preparation method of the wood ear aerogel composite material is as follows:
[0057] (1) The fungus was ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 minutes, and then placed in a 60°C oven for 24 hours;
[0058] (2) Soaking the fungus obtained in step (1) in 60 ml of deionized water for 1 hour, then transferring it to a 100 ml polytetrafluoroethylene-lined autoclave, placing it in a stainless steel autoclave, heating it to 120° C. by hydrothermal heating, keeping it warm for 10 hours, and then cooling it to room temperature to obtain a fungus gel solution;
[0059] (3) ultrasonically treating the wood ear gel solution obtained in step (2) for 2 hours, freezing the obtained uniform gel at -85°C overnight, and vacuum freeze-drying for 72 hours to obtain wood ear aerogel;
[0060] (4) heat treating the fungus aerogel obtained in step (3) in an argon atmosphere at a temperature of 600°C, a heating rate of 5°C / min, a holding time of 120min, and cooling to room temperature to obtain fungus carbon aerogel;
[0061] (5) Dissolve 1mmol nickel nitrate hexahydrate, 2mmol cobalt nitrate hexahydrate, and 12mmol urotropine in 30ml deionized water and stir for 10min to form a uniform NiCo 2 O 4 Solution;
[0062] (6) Adding the wood ear carbon aerogel obtained in step (4) to the uniform solution obtained in step (5), the wood ear carbon aerogel and NiCo 2 O 4 The mass ratio of the solution was 1:1. After stirring for 6 hours, the mixture was poured into a 50 ml polytetrafluoroethylene-lined autoclave, placed in a stainless steel autoclave, heated to 120°C by hydrothermal heating, kept at this temperature for 6 hours, and then cooled to room temperature.
[0063] (7) The product prepared in step (6) was filtered and washed three times with deionized water and anhydrous ethanol respectively, and placed in an oven at 60° C. for 24 hours;
[0064] (8) The product obtained in step (7) was heat treated in air at a temperature of 350°C, a holding time of 120 min, a heating rate of 1°C / min, and then cooled to room temperature in the furnace.
[0065] The above-prepared product was tested, and the testing method and testing content were exactly the same as those in Example 1.
[0066] Embodiment 4:
[0067] In this embodiment, the product obtained is NiCo 2 O 4 @Auricularia aerogel composite material.
[0068] The above is NiCo 2 O 4 The preparation method of the wood ear aerogel composite material is as follows:
[0069] (1) The fungus was ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 minutes, and then placed in a 60°C oven for 24 hours;
[0070] (2) Soak 4 g of the fungus obtained in step (1) in 60 ml of deionized water for 1 hour, then transfer to a 100 ml polytetrafluoroethylene-lined autoclave, place in a stainless steel autoclave, heat to 120° C. by hydrothermal heating, keep warm for 10 hours, and then cool to room temperature to obtain a fungus gel solution;
[0071] (3) ultrasonically treating the wood ear gel solution obtained in step (2) for 2 hours, freezing the obtained uniform gel at -85°C overnight, and vacuum freeze-drying for 72 hours to obtain wood ear aerogel;
[0072] (4) heat treating the fungus aerogel obtained in step (3) in an argon atmosphere at a temperature of 600°C, a heating rate of 5°C / min, a holding time of 120min, and cooling to room temperature to obtain fungus carbon aerogel;
[0073] (5) Dissolve 1mmol nickel nitrate hexahydrate, 2mmol cobalt nitrate hexahydrate, 12mmol urotropine and 6mmol ammonium fluoride in 30ml deionized water and stir for 10min to form a uniform NiCo 2 O 4 Solution;
[0074] (6) Adding the wood ear carbon aerogel obtained in step (4) to the uniform solution obtained in step (5), the wood ear carbon aerogel and NiCo 2 O 4 The mass ratio of the solution was 1:1. After stirring for 6 hours, the mixture was poured into a 50 ml polytetrafluoroethylene-lined autoclave, placed in a stainless steel autoclave, heated to 120°C by hydrothermal heating, kept at this temperature for 6 hours, and then cooled to room temperature.
[0075] (7) The product prepared in step (6) was filtered and washed three times with deionized water and anhydrous ethanol respectively, and placed in an oven at 60° C. for 24 hours;
[0076] (8) The product obtained in step (7) was heat treated in air at a temperature of 350°C, a holding time of 120 min, a heating rate of 1°C / min, and then cooled to room temperature in the furnace.
[0077] The above-prepared product was tested, and the testing method and testing content were exactly the same as those in Example 1.
[0078] Comparative Example:
[0079] In this embodiment, the prepared product is a fungus aerogel composite material.
[0080] The preparation method of the fungus aerogel composite material is as follows:
[0081] (1) The fungus was ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 minutes, and then placed in a 60°C oven for 24 hours;
[0082] (2) Soak 4 g of the fungus obtained in step (1) in 60 ml of deionized water for 1 hour, then transfer to a 100 ml polytetrafluoroethylene-lined autoclave, place in a stainless steel autoclave, heat to 120° C. by hydrothermal heating, keep warm for 10 hours, and then cool to room temperature to obtain a fungus gel solution;
[0083] (3) ultrasonically treating the wood ear gel solution obtained in step (2) for 2 hours, freezing the obtained uniform gel at -85°C overnight, and vacuum freeze-drying for 72 hours to obtain wood ear aerogel;
[0084] (4) The fungus aerogel obtained in step (3) was heat treated in an argon atmosphere at a temperature of 600° C., a heating rate of 5° C. / min, and a holding time of 120 min, and then cooled to room temperature to obtain the fungus carbon aerogel.
[0085] The above-prepared product was subjected to XRD. Figure 1 shown.
[0086] Table 1 The phase composition of the materials prepared in Examples 1-4 and the microwave absorbing properties of the prepared materials are shown below.
[0087]
[0088] The symbols in Table 1 have the following meanings:
[0089] RL - reflection loss; RL min —Minimum reflection loss.
[0090] Phase analysis: Figure 1 As shown, after heat treatment, Examples 1-4 and Comparative Examples all contain typical amorphous carbon diffraction peaks. 2 O 4 After nanostructure, the composite materials prepared in Examples 1-4 are composed of carbon, NiCo 2 O 4 It consists of two physical phases.
[0091] Wave absorption performance analysis: As can be seen from Table 1, the minimum RL value of the product C@NCO-S obtained in Example 1 is -54.6dB, and the maximum effective absorption bandwidth (RL<-10dB) is 5.7GHz. The RL value of the C@NCO-S sample obtained in Example 2 is -46.3 dB, and the corresponding EAB value is 3.1 GHz. The product obtained in Example 3 also exhibits effective absorption performance, with an RL of -16.5 dB. The maximum RL of the product obtained in Example 4 is -53.8 dB, which has good wave absorption performance. It can be seen that the product obtained in Example 1 exhibits excellent wave absorption performance and has great application potential.
[0092] In summary, NiCo with excellent microwave absorption performance can be prepared by simple heat treatment and chemical in-situ synthesis reaction. 2 O 4 @Auricularia aerogel composites. In particular, the process parameters can stably and efficiently prepare NiCo 2 O4 @Auricularia aerogel composite materials can effectively adjust their absorbing properties, which greatly promotes industrial production and is of great significance for the widespread application and development of absorbing materials.
[0093] The above embodiments provide a systematic and detailed description of the technical solution of the present invention. It should be understood that the above embodiments are only specific embodiments of the present invention and are not intended to limit the present invention. Any modification, supplement or equivalent replacement made within the scope of the principles of the present invention shall be included in the protection scope of the present invention.
Claims
1. A NiCo 2 O 4 @Auricularia carbon aerogel composite material, It is characterized in that The composite material uses the wood ear carbon aerogel of biomass-derived porous carbon as the raw material, and NiCo is evenly distributed on the wood ear carbon aerogel in situ. 2 O 4 Nanostructures; The NiCo 2 O 4 The preparation method of the wood ear carbon aerogel composite material comprises the following steps: Step A1: Dissolve 1 mmol nickel nitrate hexahydrate, 2 mmol cobalt nitrate hexahydrate, and 12 mmol additive in 30 ml deionized water and stir for 10 minutes to form a uniform NiCo 2 O 4 Solution, wherein the additive is one of urea and hexamethylenetetramine; Step A2: Adding the wood ear carbon aerogel to the uniform solution obtained in step A1, the wood ear carbon aerogel and NiCo 2 O 4 The mass ratio of the solution was 1:
1. After stirring for 6 hours, the solution was poured into a 50 ml polytetrafluoroethylene liner and placed in a stainless steel autoclave. The temperature was raised to 120°C by hydrothermal heating, kept at this temperature for 6 hours, and then cooled to room temperature. Step A3: The product prepared in step A2 was filtered and washed three times with deionized water and anhydrous ethanol respectively, and placed in a 60° C. oven for drying for 24 hours; Step A4: heat-treating the product obtained in step A3 in air at a temperature of 350° C., a heating rate of 1° C. / min, a holding time of 120 minutes, and cooling to room temperature in the furnace; The method for preparing wood ear carbon aerogel comprises the following steps: Step B1: ultrasonically clean the fungus with deionized water and anhydrous ethanol for 3 times, each time for 10 minutes, and place it in a 60°C oven to dry for 24 hours; Step B2: Soak the fungus obtained in step B1 in 60 ml of deionized water for 1 hour, then transfer it to a polytetrafluoroethylene liner, put it into a stainless steel autoclave, heat it to 120° C. by hydrothermal heating, keep it warm for 10 hours, and then cool it to room temperature to obtain a fungus gel solution; Step B3: ultrasonically treating the fungus gel solution obtained in step B2 for 2 hours, freezing the obtained uniform gel at -85°C overnight, and vacuum freeze-drying for 72 hours to obtain fungus aerogel; Step B4: heat-treating the wood ear aerogel obtained in step B3 in an inert gas atmosphere at a temperature of 600° C., a heating rate of 5° C. / min, and a holding time of 120 min, and then cooling to room temperature to obtain wood ear carbon aerogel.
2. A NiCo according to claim 1 2 O 4 @Auricularia carbon aerogel composite material, It is characterized in that In the step A1, 6 mmol of ammonium fluoride may also be added.
3. A NiCo according to claim 1 2 O 4 @Auricularia carbon aerogel composite material, It is characterized in that The inert gas in step B4 is one of argon and nitrogen.
4. NiCo according to any one of claims 1 to 3 2 O 4 @The application of wood ear carbon aerogel composite materials in low frequency electromagnetic wave absorption.
Citation Information
Patent Citations
Ferrum oxidate nano magnetic material and method for preparing the same
CN101117241A
Method for synthesizing floriform cobalt magnetic powder by mixed solvent thermal method
CN102363219A
Bimetallic-organic-framework-based derived porous carbon / multi-wall carbon nanotube nano composite absorbing material and preparation method thereof
CN108834389A
Ferroferric oxide-nanoporous carbon nanocomposite and preparation method and application thereof
CN109494038A
Magnetic carbon nanofiber aerogel wave-absorbing material and preparation method
CN110809395A