A method for identifying solid electrolyte materials
The analysis of the diffraction peak position and peak strength of LLZO materials through XRD tests solves the problems of complex testing and difficult identification in the prior art, and achieves rapid identification of room temperature ionic conductivity of LLZO materials and accurate judgment of Ga or Fe doping. Simplified the material testing process.
Patent Information
- Application Number
- CN202111129815.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-09-26
AI Technical Summary
In the prior art, the room temperature ionic conductivity test of LLZO materials is complex and difficult to operate, and it is difficult to quickly identify whether it contains Ga or Fe doping, which affects the selection of material testing.
The diffraction peak position and peak strength of the material are analyzed through XRD test, combined with standard PDF card comparison, quickly judge the phase structure and crystallinity of the material, and then identify its room temperature ionic conductivity, and determine whether it contains Ga or Fe doping.
It realizes a quick and concise identification of the room temperature ionic conductivity of LLZO materials, reduces the difficulty of operation, and accurately determines whether the material contains Ga or Fe doping, providing convenient material testing and selection.
Smart Images

Figure HDA0003280090560000011 
Figure HDA0003280090560000012 
Figure HDA0003280090560000013
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemistry, and in particular to a method for identifying a solid electrolyte material. Background Art
[0002] At present, lithium garnet is widely used in solid electrolyte materials. The general chemical formula of garnet is A3B2(SiO4)3, where A and B are divalent and trivalent cations respectively. Its space group is No.230Ia-3d, belonging to the body-centered cubic crystal system. In its crystal structure, the [BO6] octahedron is connected to six [SiO4] tetrahedra at the same vertices, and the tetrahedron is connected to four octahedra at the same vertices to construct its three-dimensional skeleton. The A position is the dodecahedral void in the skeleton, which is generally occupied by cations with larger ionic radius. If Li replaces Si, its chemical formula becomes A3B2(LiO4)3, which is lithium garnet. In order to balance the electric charge, the valence states of A and B can be adjusted at this time. At present, the lithium garnet with relatively high room temperature ionic conductivity is mainly Li7La3Zr2O 12 The room temperature ionic conductivity of the system based on (LLZO) can exceed 0.2mS / cm, and the highest value reported so far has reached 1.5mS / cm, showing high comprehensive performance.
[0003] The study found that LLZO has two phase structures. One is the tetragonal phase, whose room temperature ionic conductivity is only 10 -6 S / cm, mainly because its phase structure makes it difficult for lithium ions to migrate, resulting in low conductivity. Another phase structure of LLZO is the cubic phase. + It is easier to migrate in the cubic phase structure, so the cubic phase of LLZO generally has a higher room temperature ionic conductivity, which can reach 10 -4 ~10 -3 S / cm. Furthermore, in addition to the No.230Ia-3d space group structure, such as Al, Ta, Nb or W doped LLZO, the cubic phase structure also has a No.220I-43d space group structure, that is, Ga or Fe doped LLZO. In the No.220I-43d space group structure, Li + There are more choices for migration paths, so it can show higher room temperature ionic conductivity. Therefore, the room temperature ionic conductivity performance of LLZO materials will be affected by different phase structures. On the other hand, as a kind of ceramic material, the crystallinity of LLZO solid electrolyte material will also affect the ionic conductivity of the material.
[0004] The ionic conductivity test process of LLZO solid electrolyte materials has high requirements on operators and relies on the operator's experience. The test steps are cumbersome and any improper operation of any step cannot accurately obtain the ionic conductivity test results. Therefore, if the room temperature ionic conductivity performance of LLZO materials with different structures, different components and different sintering conditions can be quickly identified, reducing the difficulty of operation will greatly facilitate the testers in material testing and selection.
[0005] However, the room temperature ionic conductivity test of LLZO materials in the prior art often requires the preparation of dense blocks and then testing using an electrochemical workstation. Although it can obtain accurate specific values of room temperature ionic conductivity, the preparation of dense blocks not only has a long production cycle, but also requires precise process parameter control in the preparation process of the blocks, which requires extremely high experience and is not suitable for general personnel to operate. In addition, if you want to further understand the component structure of LLZO materials with high room temperature ionic conductivity performance, especially whether it contains Ga or Fe doping, you need to use other chemical methods for identification. Summary of the invention
[0006] In view of the shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a method for identifying solid electrolyte materials. By performing a simple XRD test on LLZO system materials and analyzing the XRD peak position and peak intensity, it is possible to simply and effectively determine whether the material has a high room temperature ionic conductivity, thereby providing a fast and concise method for quickly identifying whether different LLZO system materials have high room temperature ionic conductivity. Another purpose of the present invention is to provide a method for quickly identifying whether a solid electrolyte material with high room temperature ionic conductivity performance is doped with Ga or Fe.
[0007] The technical solution of the present invention is as follows:
[0008] A method for identifying a solid electrolyte material, wherein the solid electrolyte material is a lithium garnet solid electrolyte material, comprising the following steps:
[0009] The solid electrolyte material to be tested is made into a powder material suitable for XRD testing;
[0010] Perform XRD detection to obtain XRD diffraction peak results;
[0011] Compare the XRD diffraction peak results with the standard PDF card. If other diffraction peaks other than those on the standard PDF card appear, it is determined that the phase structure of the solid electrolyte material under test does not meet the standard, otherwise it meets the standard.
[0012] For the tested solid electrolyte material with a phase structure that meets the standard, if the ratio of the strongest peak intensity of its diffraction peak to the background peak intensity is greater than a preset multiple, it is determined that the crystallinity of the tested solid electrolyte material meets the standard, otherwise it is considered not to meet the standard;
[0013] For the solid electrolyte materials that meet the crystallinity standards, the room temperature ionic conductivity of the solid electrolyte materials is identified based on the ratio of the peak intensities of the highest peaks at different diffraction peaks after deducting the background intensity and the peak position of the strongest peak.
[0014] Furthermore, in the process of identifying the room temperature ionic conductivity performance of the solid electrolyte material being tested, the peak intensities of the highest peaks at 2θ=16.8±0.5° and 34.0±0.5° of the solid electrolyte material being tested after deducting the background intensity are defined as I A and I B , when 0.85≤I A / I B ≤0.95 and 2θ=34.0±0.5° is the strongest peak, the room temperature ionic conductivity of the solid electrolyte material under test exceeds 0.6mS / cm; or, the peak intensities of the highest peaks at 2θ=16.8±0.5° and 31.0±0.5° of the solid electrolyte material under test after deducting the background intensity are defined as I C and I D , when 0.75≤I C / I D When ≤0.90 and 2θ=31.0±0.5° is the strongest peak, the room temperature ionic conductivity of the solid electrolyte material being tested exceeds 0.8 mS / cm.
[0015] Furthermore, the chemical formula of the solid electrolyte material to be tested is Li 7-3x-y+z A x LqCy 2-y B y O 12+z / 2 , where A is a trivalent metal element, B is a pentavalent metal element, 0≤x≤0.4, 0≤y≤0.8, 0≤z≤0.2;
[0016] or,
[0017] The chemical formula of the solid electrolyte material to be tested is Li 7-3x-2w+z A x LqCy 2-w C w O 12+z / 2 , wherein A is a trivalent metal element, C is a hexavalent metal element, 0≤x≤0.4, 0≤w≤0.7, 0≤z≤0.2.
[0018] Furthermore, the process of preparing the solid electrolyte material to be tested into a powder material suitable for XRD testing includes:
[0019] The solid electrolyte material to be tested is ground and sieved to make a powder material suitable for XRD testing.
[0020] Furthermore, the screening is through a 60-200 mesh sieve.
[0021] Furthermore, the process of performing XRD detection includes:
[0022] The powder material suitable for XRD test made of the solid electrolyte material to be tested is filled and flattened on the standard sample table for XRD detection.
[0023] Furthermore, the detection angle range of the XRD detection is 10-60°.
[0024] Furthermore, the card number of the standard PDF card is JCPDS 80-0457.
[0025] Furthermore, the preset multiple is 20.
[0026] A method for identifying components of a solid electrolyte material, wherein the solid electrolyte material is a lithium garnet solid electrolyte material, comprising the following steps:
[0027] The solid electrolyte material to be tested is made into a powder material suitable for XRD testing;
[0028] Perform XRD detection to obtain XRD diffraction peak results;
[0029] Compare the XRD diffraction peak results with the standard PDF card. If other diffraction peaks other than those on the standard PDF card appear, it is determined that the phase structure of the solid electrolyte material under test does not meet the standard, otherwise it meets the standard.
[0030] For the tested solid electrolyte material with a phase structure that meets the standard, if the ratio of the strongest peak intensity of its diffraction peak to the background peak intensity is greater than a preset multiple, it is determined that the crystallinity of the tested solid electrolyte material meets the standard, otherwise it is considered not to meet the standard;
[0031] For the tested solid electrolyte material with qualified crystallinity, the peak intensities of the highest peaks at 2θ=16.8±0.5° and 31.0±0.5° of the tested solid electrolyte material after deducting the background intensity are defined as I C and I D , when 0.75≤I C / I DWhen ≤0.90 and 2θ=31.0±0.5° is the strongest peak, and the spatial point group structure of the solid electrolyte material being tested is No.220I-43d, then its components contain Ga or Fe doping.
[0032] The beneficial effects of the present invention are as follows: the present invention only needs to perform a simple and easy XRD test, and by analyzing the XRD peak position and peak intensity, the room temperature ionic conductivity performance of the tested LLZO material can be quickly and concisely identified, thereby providing great convenience for testers to perform material testing and selection. In addition, based on basically the same test method, the present invention can also quickly identify whether the tested solid electrolyte material with high room temperature ionic conductivity performance contains Ga or Fe doping, which also provides convenience for testers to quickly grasp the component characteristics of the tested LLZO material. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is the XRD pattern of the sample in Example 1;
[0034] Figure 2 is the XRD pattern of the sample in Example 2;
[0035] Figure 3 is the XRD pattern of the sample in Example 3;
[0036] Figure 4 is the XRD pattern of the sample of Example 4;
[0037] Figure 5 is the XRD pattern of the sample in Example 5;
[0038] Figure 6 is the XRD pattern of the sample in Example 6;
[0039] Figure 7 is the XRD pattern of the sample of Example 7;
[0040] Figure 8 is the XRD pattern of the sample in Example 8;
[0041] Fig. 9 is the XRD pattern of the sample of Example 9;
[0042] Fig.10 This is the XRD pattern of the sample in Example 10. DETAILED DESCRIPTION
[0043] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0044] The method for identifying a solid electrolyte material described in the present invention comprises the following steps:
[0045] (1) grinding and sieving the LLZO system solid electrolyte powder material to prepare a powder material suitable for XRD testing, specifically, passing through a 60-200 mesh sieve;
[0046] (2) Place the sieved powder on the standard sample table and fill it up and flatten it. It is not recommended to use a micro or trace sample test table to avoid insufficient diffraction peak intensity collected by the XRD detector;
[0047] (3) In order to complete the detection quickly, the XRD detection angle range can be set to 10-60°. The corresponding X-ray scanning speed can be set according to different models of X-ray diffractometers, which can generally be less than 15° / min;
[0048] (4) Analyze the XRD diffraction peak results of the test:
[0049] a. First, it is necessary to determine whether there are obvious impurities. This can be identified by comparing with the standard PDF card (card number is JCPDS 80-0457). If other diffraction peaks appear, it is determined that the phase structure does not meet the standard, otherwise it meets the standard;
[0050] b. Under the premise that the phase structure meets the standard, if the peak intensity of the strongest diffraction peak exceeds a certain multiple (such as 20 times) of the background peak intensity, it can be considered that the crystallinity of the LLZO system material meets the standard and meets the requirements, otherwise it does not meet the standard. For LLZO system materials whose crystallinity does not meet the standard, you can return to step (3) to adjust the parameter settings of the XRD test and retest to determine whether its crystallinity meets the requirements.
[0051] (5) Since the diffraction peak intensity directly reflects the change in ion occupancy in the crystal structure and can directly reflect this difference in performance, under the premise that the crystallinity determined in step (4) meets the standard, the room temperature ionic conductivity performance of the solid electrolyte material under test can be identified based on the ratio of the peak intensities of the highest peaks of the solid electrolyte material under test after deducting the background intensity and the peak position of the strongest peak at different diffraction peak positions of the solid electrolyte material under test, specifically:
[0052] a. The peak intensities of the highest peaks at 2θ = 16.8 ± 0.5° and 34.0 ± 0.5° after deducting the background intensity are defined as I A and I B , or the peak intensities of the highest peaks at 2θ=16.8±0.5° and 31.0±0.5° after deducting the background intensity are defined as I C and I D .
[0053] b. When 0.85≤I A / I B≤0.95, and 2θ=34.0±0.5° is the strongest peak, the LLZO system solid electrolyte at this time has a higher room temperature ionic conductivity, specifically exceeding 0.6 mS / cm.
[0054] When 0.75≤I C / I D ≤0.90, and 2θ=31.0±0.5° is the strongest peak. At this time, the LLZO system solid electrolyte has a higher room temperature ionic conductivity, specifically exceeding 0.8 mS / cm.
[0055] The identification method of the solid electrolyte material is applicable to the following lithium garnet solid electrolyte material LLZO, whose chemical formula is Li 7-3x-y+z A x LqCy 2-y B y O 12+z / 2 (A is a trivalent metal element, B is a pentavalent metal element, 0≤x≤0.4, 0≤y≤0.8, 0≤z≤0.2) or Li 7-3x-2w+z A x LqCy 2-w C w O 12+z / 2 (A is a trivalent metal element, C is a hexavalent metal element, 0≤x≤0.4, 0≤w≤0.7, 0≤z≤0.2).
[0056] The identification method of the solid electrolyte material of the present invention is further described below in conjunction with the accompanying drawings and examples.
[0057] Example 1
[0058] Li 6.4 LqCy 1.4 Nb 0.6 O 12 The powder of the components was sintered at 1250°C for 1 hour, ground through a 100-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten, and then subjected to XRD testing. The 2θ test range of XRD was 10-60°, and the X-ray scanning speed was 4° / min.
[0059] XRD test results are as follows Figure 1 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =12912,I B =13785,I C =12912,I D =12565, background peak intensity IBG <400, so the strongest peak-to-peak strength is I B / I BG >20, the crystallinity also meets the requirements. A / I B =0.94, I C / I D =1.03, which meets 0.85≤I A / I B ≤0.95 and the strongest peak corresponds to 2θ=33.977° in the range of 34.0±0.5°. Therefore, according to this test result, it can be determined that the room temperature ionic conductivity of this component material under the sintering conditions can reach the requirement of more than 0.6mS / cm.
[0060] To verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare a dense block. The room temperature ionic conductivity was tested using an electrochemical workstation, and the accurate room temperature ionic conductivity was measured to be 0.76 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0061] Example 2
[0062] The same composition as in Example 1 was added 6.4 LqCy 1.4 Nb 0.6 O 12 The powder was sintered at 1000°C for 6 h and XRD test was performed according to the XRD test method of Example 1. The XRD test results are shown in Figure 2 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =10368,I B =7685,I C =10368,I D =7011, background peak intensity I BG <300, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.35,I C / I D =1.48, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I DThe ratio of ≤0.90, that is, they are not in the corresponding optimal value region, indicating that the room temperature ionic conductivity of the component material under the sintering condition is low and does not meet the requirement of 0.6 mS / cm or above. This example shows that the sintering condition of 1000°C sintering for 6 hours cannot make the component material have a higher room temperature ionic conductivity.
[0063] In order to verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare dense blocks, and their room temperature ionic conductivity was tested using an electrochemical workstation. The accurate room temperature ionic conductivity was measured to be only 0.08 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0064] Example 3
[0065] Li 6.35 Al 0.1 LqCy 1.55 Ta 0.45 O 12.05 The powder of the components was sintered at 1280°C for 45 min, ground through a 60-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten, and then subjected to XRD testing. The 2θ test range of XRD was 10-60°, and the X-ray scanning speed was 3° / min.
[0066] XRD test results are as follows Figure 3 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =13310,I B =14534,I C =13310,I D =12672, background peak intensity I BG <400, so the strongest peak-to-peak strength is I B / I BG >20, the crystallinity also meets the requirements. A / I B =0.92, I C / I D =1.05, meeting 0.85≤I A / I B ≤0.95 and the strongest peak corresponds to 2θ=33.961° in the range of 34.0±0.5°. Therefore, according to this test result, it can be determined that the room temperature ionic conductivity of this component material under the sintering conditions can reach the requirement of more than 0.6mS / cm.
[0067] To verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare a dense block. The room temperature ionic conductivity was tested using an electrochemical workstation, and the accurate room temperature ionic conductivity was measured to be 0.69 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0068] Example 4
[0069] The same composition as in Example 3 was added to 6.35 Al 0.1 LqCy 1.55 Ta 0.45 O 12.05 The powder was sintered at 950°C for 12 h, and an XRD test was performed according to the XRD test method of Example 3. The XRD test results are shown in FIG. Figure 4 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =9889,I B =7386,I C =9889,I D =6915, background peak intensity I BG <300, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.34, I C / I D =1.43, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio of ≤0.90, that is, they are not in the corresponding optimal value region, indicating that the room temperature ionic conductivity of the component material under the sintering condition is low and does not meet the requirement of 0.6 mS / cm or above. This example shows that the sintering condition of 950°C sintering for 12 hours cannot make the component material have a high room temperature ionic conductivity.
[0070] In order to verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare dense blocks, and their room temperature ionic conductivity was tested using an electrochemical workstation. The accurate room temperature ionic conductivity was measured to be only 0.1 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0071] Example 5
[0072] Li6.45 Ga 0.25 La3Zr2O 12.1 The powder of the components was sintered at 1050°C for 3h, ground through a 200-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten, and then subjected to XRD testing. The 2θ test range of XRD was 10-60°, and the X-ray scanning speed was 2° / min.
[0073] XRD test results are as follows Figure 5 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =14120,I B =13742,I C =14120,I D =15871, background peak intensity I BG <450, so the strongest peak-to-peak strength is I D / I BG >20, the crystallinity also meets the requirements. A / I B =1.03,I C / I D =0.89, which meets 0.75≤I C / I D ≤0.90 and the strongest peak corresponds to 2θ=30.802° in the range of 31.0±0.5°. Therefore, according to this test result, it can be determined that the room temperature ionic conductivity of this component material under the sintering conditions can reach the requirement of more than 0.8mS / cm.
[0074] To verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare a dense block. The room temperature ionic conductivity was tested using an electrochemical workstation, and the accurate room temperature ionic conductivity was measured to be 1.13 mS / cm, which is consistent with the above identification conclusion of this example.
[0075] Example 6
[0076] The same composition as in Example 5 was added 6.45 Ga 0.25 La3Zr2O 12.1 The powder was sintered at 850°C for 8 hours and XRD test was performed according to the XRD test method of Example 5. The XRD test results are shown in Figure 6It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =13921,I C =13921,I B =8102,I D =10325, background peak intensity I BG <450, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.72, I C / I D =1.35, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio of ≤0.90, that is, they are not in the corresponding optimal value region, indicating that the room temperature ionic conductivity of the component material under the sintering condition is low and does not meet the requirement of 0.6 mS / cm or above. This example shows that the sintering condition of 850° C. sintering for 8 hours cannot make the component material have a high room temperature ionic conductivity.
[0077] In order to verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare dense blocks, and their room temperature ionic conductivity was tested using an electrochemical workstation. The accurate room temperature ionic conductivity was measured to be only 0.26 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0078] Example 7
[0079] Li 6.5 LqCy 1.7 W 0.3 O 12.05 The powder of the components was sintered at 1260°C for 2h, ground through a 100-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten, and then subjected to XRD testing. The 2θ test range of XRD was 10-60°, and the X-ray scanning speed was 4° / min.
[0080] XRD test results are as follows Figure 7 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A=11219,I B =13152,I C =11219,I D =11105, background peak intensity I BG <450, so the strongest peak-to-peak strength is I B / I BG >20, the crystallinity also meets the requirements. A / I B =0.85, I C / I D =1.01, meeting 0.85≤I A / I B ≤0.95 and the strongest peak corresponds to 2θ=33.942° in the range of 34.0±0.5°. Therefore, according to this test result, it can be determined that the room temperature ionic conductivity of this component material under the sintering conditions can reach the requirement of more than 0.6mS / cm.
[0081] To verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare a dense block. The room temperature ionic conductivity was tested using an electrochemical workstation, and the accurate room temperature ionic conductivity was measured to be 0.68 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0082] Example 8
[0083] The same composition as in Example 7 was added 6.5 LqCy 1.7 W 0.3 O 12.05 The powder was sintered at 950°C for 4 h and XRD test was performed according to the XRD test method of Example 7. The XRD test results are shown in Figure 8 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =9913,I B =7103,I C =9913,I D =6514, background peak intensity I BG <350, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.40,I C / I D =1.52, does not satisfy 0.85≤I A / I B≤0.95 or 0.75≤I C / I D The ratio of ≤0.90, that is, they are not in the corresponding optimal value region, indicating that the room temperature ionic conductivity of the component material under the sintering condition is low and does not meet the requirement of 0.6 mS / cm or above. This example shows that the sintering condition of 950° C. sintering for 4 hours cannot make the component material have a high room temperature ionic conductivity.
[0084] In order to verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare dense blocks, and their room temperature ionic conductivity was tested using an electrochemical workstation. The accurate room temperature ionic conductivity was measured to be only 0.12 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0085] Example 9
[0086] Li 6.6 Fe 0.2 La3Zr2O 12.1 The powder of the components was sintered at 1100°C for 2h, ground through a 60-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten, and then subjected to XRD testing. The 2θ test range of XRD was 10-60°, and the X-ray scanning speed was 4° / min.
[0087] XRD test results are as follows Fig. 9 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =12467,I B =12303,I C =12467,I D =14721, background peak intensity I BG <450, so the strongest peak-to-peak strength is I D / I BG >20, the crystallinity also meets the requirements. A / I B =1.01,I C / I D =0.85, which meets 0.75≤I C / I D ≤0.90 and the strongest peak corresponds to 2θ=30.812° in the range of 31.0±0.5°. Therefore, according to this test result, it can be determined that the room temperature ionic conductivity of this component material under the sintering conditions can reach the requirement of more than 0.8mS / cm.
[0088] To verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare a dense block. The room temperature ionic conductivity was tested using an electrochemical workstation, and the accurate room temperature ionic conductivity was measured to be 1.04 mS / cm. The test result of the room temperature ionic conductivity is consistent with the above identification conclusion of this embodiment.
[0089] Example 10
[0090] The same composition as in Example 9 was added 6.6 Fe 0.2 La3Zr2O 12.1 The powder was sintered at 900°C for 4 h and XRD test was performed according to the XRD test method of Example 9. The XRD test results are shown in Fig.10 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =11897,I B =7903,I C =11897,I D =10763, background peak intensity I BG <450, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.51,I C / I D =1.11, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio of ≤0.90, that is, they are not in the corresponding optimal value region, indicating that the room temperature ionic conductivity of the component material under the sintering condition is low and does not meet the requirement of 0.6 mS / cm or above. This example shows that the sintering condition of 900°C sintering for 4 hours cannot make the component material have a high room temperature ionic conductivity.
[0091] In order to verify the accuracy of the above identification conclusion, materials with the same components were sintered under the same conditions to prepare dense blocks, and their room temperature ionic conductivity was tested using an electrochemical workstation. The accurate room temperature ionic conductivity was measured to be only 0.38 mS / cm, which is consistent with the above identification conclusion of this embodiment.
[0092] The present invention also describes a method for identifying components of a solid electrolyte material, wherein the solid electrolyte material is a lithium garnet solid electrolyte material, and specifically comprises the following steps:
[0093] The solid electrolyte material to be tested is made into a powder material suitable for XRD testing;
[0094] Perform XRD detection to obtain XRD diffraction peak results;
[0095] Compare the XRD diffraction peak results with the standard PDF card. If other diffraction peaks other than those on the standard PDF card appear, it is determined that the phase structure of the solid electrolyte material under test does not meet the standard, otherwise it meets the standard.
[0096] For the tested solid electrolyte material with a phase structure that meets the standard, if the ratio of the strongest peak intensity of its diffraction peak to the background peak intensity is greater than a preset multiple, it is determined that the crystallinity of the tested solid electrolyte material meets the standard, otherwise it is considered not to meet the standard;
[0097] For the tested solid electrolyte material with qualified crystallinity, the peak intensities of the highest peaks at 2θ=16.8±0.5° and 31.0±0.5° of the tested solid electrolyte material after deducting the background intensity are defined as I C and I D , when 0.75≤I C / I D ≤0.90 and 2θ=31.0±0.5° is the strongest peak, when the spatial point group structure of the solid electrolyte material being tested is No.220I-43d, its components contain Ga or Fe doping.
[0098] The identification method of the solid electrolyte material of the present invention is further described below in conjunction with the accompanying drawings and examples.
[0099] Embodiment 11
[0100] The powder of the solid electrolyte material to be tested was sintered at 1250℃ for 1h, ground through a 100-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten it for XRD testing. The 2θ test range of XRD is 10-60°, and the X-ray scanning speed is 4° / min.
[0101] XRD test results are as follows Figure 1 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =12912,I B =13785,I C =12912,ID =12565, background peak intensity I BG <400, so the strongest peak-to-peak strength is I B / I BG >20,I A / I B =0.94, I C / I D =1.03, which meets 0.85≤I A / I B ≤0.95 and the strongest peak corresponds to 2θ=33.977° in the range of 34.0±0.5°, and the crystallinity also meets the requirements.
[0102] The spatial point group structure obtained by software comparison should be No.230Ia-3d. Since its spatial point group structure is not No.220I-43d, it is impossible to determine whether the component is doped with Ga or Fe. Obtaining the spatial point group structure by existing software is a conventional technical means and will not be described in detail here.
[0103] Example 12
[0104] The powder of the solid electrolyte material to be tested was sintered at 1000°C for 6 hours, and an XRD test was performed according to the XRD test method of Example 11. The XRD test results are shown in FIG. Figure 2 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =10368,I B =7685,I C =10368,I D =7011, background peak intensity I BG <300, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.35,I C / I D =1.48, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio relationship is ≤0.90, that is, they are not in the corresponding optimal value region, indicating that it is impossible to determine whether the component is doped with Ga or Fe.
[0105] Example 13
[0106] The powder of the solid electrolyte material to be tested was sintered at 1280℃ for 45min, ground through a 60-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten it for XRD testing. The 2θ test range of XRD is 10-60°, and the X-ray scanning speed is 3° / min.
[0107] XRD test results are as follows Figure 3 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =13310,I B =14534,I C =13310,I D =12672, background peak intensity I BG <400, so the strongest peak-to-peak strength is I B / I BG >20, the crystallinity also meets the requirements. A / I B =0.92, I C / I D =1.05, meeting 0.85≤I A / I B ≤0.95 and the strongest peak corresponds to 2θ=33.961° in the range of 34.0±0.5°.
[0108] Through software comparison, its space point group structure is obtained as No.230Ia-3d. It can be seen that its space point group structure is not No.220I-43d, so it is impossible to determine whether the component is doped with Ga or Fe.
[0109] Embodiment 14
[0110] The powder of the solid electrolyte material to be tested was sintered at 950°C for 12 hours, and an XRD test was performed according to the XRD test method of Example 13. The XRD test results are shown in FIG. Figure 4 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =9889,I B =7386,I C =9889,I D =6915, background peak intensity I BG <300, so the strongest peak-to-peak strength is I A / I BG>20, the crystallinity also meets the requirements. A / I B =1.34, I C / I D =1.43, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio relationship is ≤0.90, that is, they are not in the corresponding optimal value region, indicating that it is impossible to determine whether the component is doped with Ga or Fe.
[0111] Embodiment 15
[0112] The powder of the solid electrolyte material to be tested was sintered at 1050℃ for 3h, ground through a 200-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten it for XRD testing. The 2θ test range of XRD is 10-60°, and the X-ray scanning speed is 2° / min.
[0113] XRD test results are as follows Figure 5 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =14120,I B =13742,I C =14120,I D =15871, background peak intensity I BG <450, so the strongest peak-to-peak strength is I D / I BG >20, the crystallinity also meets the requirements. A / I B =1.03,I C / I D =0.89, which meets 0.75≤I C / I D ≤0.90 and the strongest peak corresponds to 2θ=30.802° in the range of 31.0±0.5°.
[0114] The spatial point group structure obtained by software comparison is No.220I-43d, which indicates that Ga or Fe is doped in the component.
[0115] To verify the accuracy of the above identification conclusion, the material was tested for composition using an X-ray fluorescence spectrometer (XRF), and the results showed that the mass ratio of La2O3:ZrO2:Ga2O3 was 58.74:29.84:3.11, and the mass ratios of the remaining metal oxides were all lower than 0.7, so it can be seen that the material composition contains Ga element, which is consistent with the above identification conclusion of this embodiment.
[0116] Example 16
[0117] The powder of the solid electrolyte material to be tested was sintered at 850°C for 8 hours, and an XRD test was performed according to the XRD test method of Example 15. The XRD test results are shown in FIG. Figure 6 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =13921,I B =8102,I C =13921,I D =10325, background peak intensity I BG <450, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.72, I C / I D =1.35, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio relationship is ≤0.90, that is, they are not in the corresponding optimal value region, indicating that it is impossible to determine whether the component is doped with Ga or Fe.
[0118] Embodiment 17
[0119] The powder of the solid electrolyte material to be tested was sintered at 1260℃ for 2h, ground through a 100-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten it for XRD testing. The 2θ test range of XRD is 10-60°, and the X-ray scanning speed is 4° / min.
[0120] XRD test results are as follows Figure 7It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =11219,I B =13152,I C =11219,I D =11105, background peak intensity I BG <450, so the strongest peak-to-peak strength is I B / I BG >20, the crystallinity also meets the requirements. A / I B =0.85, I C / I D =1.01, meeting 0.85≤I A / I B ≤0.95 and the strongest peak corresponds to 2θ=33.942° in the range of 34.0±0.5°.
[0121] Through software comparison, it is obtained that its space point group structure should be No.230Ia-3d. Since its space point group structure is not No.220I-43d, it is impossible to determine whether the component is doped with Ga or Fe.
[0122] Embodiment 18
[0123] The powder of the solid electrolyte material to be tested was sintered at 950°C for 4 hours, and an XRD test was performed according to the XRD test method of Example 17. The XRD test results are as follows: Figure 8 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =9913,I B =7103,I C =9913,I D =6514, background peak intensity I BG <350, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.40,I C / I D =1.52, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio relationship is ≤0.90, that is, they are not in the corresponding optimal value region, indicating that it is impossible to determine whether the component is doped with Ga or Fe.
[0124] Embodiment 19
[0125] The powder of the solid electrolyte material to be tested was sintered at 1100℃ for 2h, ground through a 60-mesh sieve, and the sieved powder was placed on a standard sample table to fill and flatten it for XRD testing. The 2θ test range of XRD is 10-60°, and the X-ray scanning speed is 4° / min.
[0126] XRD test results are as follows Fig. 9 It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS 80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =12467,I B =12303,I C =12467,I D =14721, background peak intensity I BG <450, so the strongest peak-to-peak strength is I D / I BG >20, the crystallinity also meets the requirements. A / I B =1.01,I C / I D =0.85, which meets 0.75≤I C / I D ≤0.90 and the strongest peak corresponds to 2θ=30.812° in the range of 31.0±0.5°. The spatial point group structure obtained by software comparison should be No.220I-43d, and Ga or Fe is doped in the component.
[0127] To verify the accuracy of the above identification conclusion, the material was tested for composition using an X-ray fluorescence spectrometer (XRF), and the results showed that the mass ratio of La2O3:ZrO2:Fe2O3 was 56.95:29.11:1.97, and the mass ratios of the remaining metal oxides were all lower than 0.7, so it can be seen that the material composition contains Fe element, which is consistent with the above identification conclusion of this embodiment.
[0128] Embodiment 20
[0129] The powder of the solid electrolyte material to be tested was sintered at 900°C for 4 hours, and an XRD test was performed according to the XRD test method of Example 9. The XRD test results are shown in FIG. Fig.10It is shown that there are no other diffraction peaks by comparing with the standard PDF card JCPDS80-0457, and its phase structure meets the requirements. The peak intensities of the highest peaks at 2θ=16.8±0.5°, 34.0±0.5°, and 31.0±0.5° after deducting the background intensity are I A =11897,I B =7903,I C =11897,I D =10763, background peak intensity I BG <450, so the strongest peak-to-peak strength is I A / I BG >20, the crystallinity also meets the requirements. A / I B =1.51,I C / I D =1.11, does not satisfy 0.85≤I A / I B ≤0.95 or 0.75≤I C / I D The ratio relationship is ≤0.90, that is, they are not in the corresponding optimal value region, indicating that it is impossible to determine whether the component is doped with Ga or Fe.
[0130] The above description is only a preferred embodiment of the present invention and does not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A method for identifying a solid electrolyte material, wherein the solid electrolyte material is a lithium garnet solid electrolyte material, characterized in that: The following steps are involved: The solid electrolyte material to be tested is made into a powder material suitable for XRD testing; Perform XRD detection to obtain XRD diffraction peak results; Compare the XRD diffraction peak results with the standard PDF card. If other diffraction peaks other than those on the standard PDF card appear, it is determined that the phase structure of the solid electrolyte material under test does not meet the standard, otherwise it meets the standard. For the tested solid electrolyte material with a phase structure that meets the standard, if the ratio of the strongest peak intensity of its diffraction peak to the background peak intensity is greater than a preset multiple, it is determined that the crystallinity of the tested solid electrolyte material meets the standard, otherwise it is considered not to meet the standard; For the tested solid electrolyte materials that meet the crystallinity standards, the room temperature ionic conductivity of the tested solid electrolyte materials is identified based on the ratio of the peak intensities of the highest peaks at different diffraction peak positions after deducting the background intensity and the peak position of the strongest peak; In the process of identifying the room temperature ionic conductivity performance of the solid electrolyte material to be tested, the peak intensities of the highest peaks at the diffraction peak positions 2θ=16.8±0.5° and 34.0±0.5° of the solid electrolyte material to be tested after deducting the background intensity are defined as I A and I B , when 0.85≤I A / I B ≤0.95 and 2θ= 34.0±0.5° is the strongest peak, the room temperature ionic conductivity of the solid electrolyte material under test exceeds 0.6 mS / cm; or, the peak intensities of the highest peaks at 2θ=16.8±0.5° and 31.0±0.5° of the solid electrolyte material under test after deducting the background intensity are defined as I C and I D , when 0.75≤I C / I D When ≤0.90 and 2θ= 31.0±0.5° is the strongest peak, the room temperature ionic conductivity of the solid electrolyte material being tested exceeds 0.8mS / cm.
2. The method for identifying a solid electrolyte material according to claim 1, wherein: The chemical formula of the solid electrolyte material to be tested is Li 7-3x-y+z A x LqCy 2-y B y O 12+z / 2 , wherein A is a trivalent metal element, B is a pentavalent metal element, 0≤x≤0.4, 0≤y≤0.8, 0≤z≤0.2; or, The chemical formula of the solid electrolyte material to be tested is Li 7-3x-2w+z A x LqCy 2-w C w O 12+z / 2 , wherein A is a trivalent metal element, C is a hexavalent metal element, 0≤x≤0.4, 0≤w≤0.7, 0≤z≤0.
2.
3. The method for identifying a solid electrolyte material according to claim 1, wherein: The process of making the solid electrolyte material to be tested into a powder material suitable for XRD testing includes: The solid electrolyte material to be tested is ground and sieved to make a powder material suitable for XRD testing.
4. The method for identifying a solid electrolyte material according to claim 3, wherein: The sieving is through a 60-200 mesh sieve.
5. The method for identifying a solid electrolyte material according to claim 1, wherein: The process of performing XRD detection comprises: The powder material suitable for XRD test made of the solid electrolyte material to be tested is filled and flattened on the standard sample table for XRD detection.
6. The method for identifying a solid electrolyte material according to claim 5, wherein: The detection angle range of the XRD detection is 10-60°.
7. The method for identifying a solid electrolyte material according to any one of claims 1 to 6, wherein: The card number of the standard PDF card is JCPDS 80-0457.
8. The method for identifying a solid electrolyte material according to any one of claims 1 to 6, wherein: The preset multiple is 20.
9. A method for identifying components of a solid electrolyte material, wherein the solid electrolyte material is a lithium garnet solid electrolyte material, characterized in that: The following steps are involved: The solid electrolyte material to be tested is made into a powder material suitable for XRD testing; Perform XRD detection to obtain XRD diffraction peak results; Compare the XRD diffraction peak results with the standard PDF card. If other diffraction peaks other than those on the standard PDF card appear, it is determined that the phase structure of the solid electrolyte material under test does not meet the standard, otherwise it meets the standard. For the tested solid electrolyte material with a phase structure that meets the standard, if the ratio of the strongest peak intensity of its diffraction peak to the background peak intensity is greater than a preset multiple, it is determined that the crystallinity of the tested solid electrolyte material meets the standard, otherwise it is considered not to meet the standard; For the tested solid electrolyte material with qualified crystallinity, the peak intensities of the highest peaks at 2θ=16.8±0.5° and 31.0±0.5° of the tested solid electrolyte material after deducting the background intensity are defined as I C and I D , when 0.75≤I C / I D ≤0.90 and 2θ= 31.0±0.5° is the strongest peak, and the spatial point group structure of the solid electrolyte material being tested is No.220I-43d, then its components contain Ga or Fe doping.
Citation Information
Patent Citations
Method for judging lithium ion battery material performance
CN109884100A
Sulfide solid electrolyte material, battery, and producing method for sulfide solid electrolyte material
US20150357673A1