Release agent for plastics

By coating organic polysiloxane emulsion on the plastic, combining anionic surfactant and polyoxyethylene alkyl ether and other components, the coating unevenness and crack problems in the prior art are solved, and the stability and safety of plastics are provided. Use mold release agent, suitable for food container packaging.

CN113853287BActive Publication Date: 2024-11-26SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080037028.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-24
Filing Date
2020-04-29
Publication Date
2024-11-26
Estimated Expiration
2040-04-29

AI Technical Summary

Technical Problem

The existing mold release agent for plastics is prone to uneven wetting, oil floating and plastic bonding problems during the coating process, and contains environmentally harmful substances, making it difficult to ensure dilution stability, mechanical stability and no cracks.

Method used

An emulsion composed of organopolysiloxane, anionic surfactant, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid esters and water is used, with an average particle size of less than 200 nm, and is emulsified by specific combination ratios and emulsification. Process to prepare a mold release agent for plastics with excellent dilution stability and mechanical stability.

Benefits of technology

It achieves uniform wetting of plastic surfaces, avoids bonding and cracking problems, and is composed of approved safe materials, suitable for food container packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004929845810000011
    Figure FDA0004929845810000011
  • Figure FDA0004929845810000012
    Figure FDA0004929845810000012
  • Figure FDA0004929845810000021
    Figure FDA0004929845810000021
Patent Text Reader

Abstract

The present invention is a mold release agent for plastics, characterized in that it contains the following (A) to (E) components and has an average particle size of 200 nm or less. Thus, a mold release agent for plastics is provided, which is an emulsion of an organopolysiloxane and has excellent dilution stability and mechanical stability, good wettability, and is not prone to cracking in plastics. 100 parts by mass of the (A) organopolysiloxane has a viscosity of 100 to 100,000 mm / s at 25°C. 2 / s; 0.1 to 15.0 parts by mass of (B) one or more anionic surfactants; 1.0 to 30.0 parts by mass of (C) polyoxyethylene alkyl ether; 0.5 to 15.0 parts by mass of (D) polyoxyethylene sorbitan fatty acid ester; 50 to 100,000 parts by mass of (E) water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a mold release agent for plastics, which is an emulsion composition of organic polysiloxane. Background Art

[0002] From the perspective of freshness or hygiene, food is sold in a protected form using plastic trays, sheets, films, etc. Depending on the type of food or storage temperature, various plastics such as PET, PP, and PS are used for food container packaging.

[0003] In the manufacturing process of plastics for food packaging, they are formed into sheets or films and then wound into rolls. Usually, a release agent is applied to the surface of the sheet or film when it is wound on a roll to prevent the sheets or films from sticking to each other.

[0004] In addition, molded products such as boxes, trays, and cups obtained by molding sheets or films are stored stacked up. If a release agent is applied to them, they can be removed smoothly one by one without sticking.

[0005] From the viewpoint of mold release and lubricity, the viscosity of the mold release agent for synthetic resin used in food container packaging is preferably 100 to 100,000 mm 2 When the organopolysiloxane emulsion composition is applied to plastic as a mold release agent, the organopolysiloxane is diluted with water to a concentration of 0.1 to 5.0%, and applied by rotary dampening, gravure or spraying.

[0006] In coating methods that involve strong stirring such as spin wetting, the emulsion itself may be destroyed, resulting in gelation or oil floating, etc. If the emulsion is applied to plastic in a state where gelation or oil floating occurs, uneven wetting will occur, causing problems such as adhesion between plastics or uneven appearance.

[0007] In addition, if an emulsion of an organopolysiloxane containing a large amount of a nonionic surfactant is applied to a plastic, the following problem may occur: cracks are generated due to the impregnation of the nonionic surfactant into the plastic, and cracks are generated in the molded body. Such cracks are easily generated in plastics, especially in OPS or PS.

[0008] Therefore, there is a need for an organopolysiloxane emulsion-type mold release agent that is excellent in dilution stability, mechanical stability, and storage stability, has good wettability, and does not cause cracks in plastics.

[0009] In Japan, the Japan Hygienic Olefin And Styrene Plastics Association has stipulated the raw materials that can be used in plastics for containers and packaging that come into direct contact with food (positive list system), and has recommended the use of raw materials whose safety has been confirmed in the use of containers and packaging that come into direct contact with food.

[0010] Therefore, an organopolysiloxane emulsion is desired as a plastic release agent for food container packaging, which uses a raw material listed in the positive list of the Japan Polyolefin Sanitation Council and can solve the above-mentioned objective technical problems.

[0011] In order to solve the above-mentioned problems, various methods have been studied so far.

[0012] Patent Document 1 is an organopolysiloxane emulsion release agent composition having excellent wettability and good transparency. The average particle diameters in the examples are all larger than 200 nm, so the dilution stability or mechanical stability may be poor. In addition, sodium polyoxyethylene nonylphenyl ether sulfate is used as an anionic surfactant in the examples, but it is suspected to be an environmentally hazardous substance, so it is not recommended to use it as a plastic release agent for food container packaging.

[0013] Patent document 2 is a silicone release agent composition with less whitening of the film. The composition of Patent document 2 contains propylene glycol. In addition, polyoxyethylene lauryl ether is used alone as a nonionic emulsifier in the embodiment, but when the nonionic emulsifier is used alone, the average particle size may not become finer and the stability may be poor. In addition, in polyoxyethylene lauryl ether, polyoxyethylene (polyoxyethylene) chains of 1 to 6 may cause cracks in synthetic resins, especially PS or OPS, so when the emulsion of the embodiment of Patent document 2 is used as a release agent for PS or OPS, cracks may also occur.

[0014] Patent Document 3 is an emulsion having a narrow particle size distribution and excellent stability. Phenoxyethanol is blended during emulsification. The average particle size of the examples is large, being 1 μm or more. It is expected that the dilution stability and mechanical stability are low.

[0015] Patent Document 4 discloses an alkyl-aralkyl co-modified silicone emulsion mold release agent for aluminum die casting. The mold release property of alkyl-aralkyl co-modified silicone for plastics is lower than that of dimethyl polysiloxane, and is not suitable as a mold release agent for plastics.

[0016] Patent Document 5 is a silicone water-dispersible release agent composition suitable for use in vulcanization molding of acrylic rubber, which uses sorbitan higher alkyl esters and other nonionic surfactants. It claims that when an anionic surfactant is blended into a silicone emulsion, the negative value of the zeta potential of the emulsion becomes larger, the electron repulsion between the emulsion particles becomes stronger, and it is difficult to aggregate, and the mechanical stability is improved. However, Patent Document 5 does not contain anionic surfactants, and it is expected that the mechanical stability is low.

[0017] Patent Document 6 is an emulsion obtained by emulsifying an organopolysiloxane with a polyoxyethylene alkyl ether having an HLB of 10 or more. Similar to Patent Document 5, no anionic surfactant is added, and it is expected that the mechanical stability is low.

[0018] Patent Document 7 discloses an organosilicon emulsion composition comprising an organopolysiloxane, a polyoxyethylene alkyl ether having an alkyl chain with carbon atoms of 8 to 11, and an anionic surfactant. When the emulsion containing the polyoxyethylene alkyl ether having carbon atoms of 8 to 11 is applied to plastic, cracks may occur.

[0019] Patent Document 8 is a silicone emulsion composition obtained by emulsifying an organopolysiloxane with a polyoxyethylene alkyl ether and a sucrose fatty acid ester. In the examples, polyoxyethylene (3) decyl ether is used as the polyoxyethylene alkyl ether, but polyoxyethylene alkyl ethers having an alkyl group with 10 or less carbon atoms may cause cracks in the plastic.

[0020] Patent Document 9 is a silicone emulsion obtained by emulsifying organopolysiloxane with polyoxyethylene hexyldecyl ether or polyoxyethylene isostearyl ether. The average particle size in the examples is relatively large at about 400 nm, and dilution stability or mechanical stability may be poor.

[0021] Patent document 10 is an emulsion obtained by emulsifying an organopolysiloxane with an anionic surfactant and a polyol. Generally speaking, the function of reducing surface tension of anionic surfactants or polyols is lower than that of nonionic surfactants such as polyoxyethylene alkyl ethers. Since the surface tension (25° C.) of the emulsion of Patent document 10 after dilution 50 times with water is high at 45 dyne / cm or more, and it does not contain an anionic surfactant, when applied on plastic, the wettability may be poor and uneven coating (crawling) may occur.

[0022] Prior art literature

[0023] Patent Literature

[0024] Patent Document 1: Japanese Patent No. 3106079

[0025] Patent Document 2: Japanese Patent Application Publication No. 2005-281409

[0026] Patent Document 3: Japanese Patent Application Publication No. 2000-169705

[0027] Patent Document 4: Japanese Patent No. 4722542

[0028] Patent Document 5: Japanese Patent Application Laid-Open No. 8-283771

[0029] Patent Document 6: Japanese Patent No. 3638087

[0030] Patent Document 7: Japanese Patent Application Publication No. 2004-331784

[0031] Patent Document 8: Japanese Patent Application Publication No. 2004-035820

[0032] Patent Document 9: Japanese Patent No. 4828054

[0033] Patent Document 10: Japanese Patent No. 3835646 Summary of the invention

[0034] Technical Problems to be Solved by the Invention

[0035] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a mold release agent for plastics which is an emulsion of an organopolysiloxane and which has excellent dilution stability and mechanical stability, good wettability, and is less likely to cause cracks in plastics.

[0036] Technical means to solve technical problems

[0037] In order to achieve the above technical problem, the present invention provides a plastic release agent, characterized in that it contains the following (A) to (E) components and has an average particle size of 200 nm or less:

[0038] 100 parts by mass of (A) an organopolysiloxane represented by the following general formula (1) and having a viscosity at 25° C. of 100 to 100,000 mm 2 / s,

[0039] [Chemical formula 1]

[0040]

[0041] In formula (1), R 1are optionally the same or different, and are any one of a hydroxyl group, a hydrogen atom, a linear unsubstituted alkyl group having 1 to 32 carbon atoms, and a phenyl group, L is an integer from 60 to 1500, and the content of each of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane in the organopolysiloxane (A) is less than 3%;

[0042] 0.1 to 15.0 parts by mass of (B) anionic surfactant, which is one or more selected from alkyl sulfonates, alkylbenzene sulfonates, α-olefin sulfonates, polyoxyethylene alkyl ether sulfates, alkyl ether sulfates, polyoxyethylene alkyl ether acetates, alkyl acetates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, alkyl sulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, methyltaurine, alanine esters and salts thereof;

[0043] 1.0 to 30.0 parts by mass of (C) polyoxyethylene alkyl ether represented by the following general formula (2):

[0044] C m H 2m+1 (OCH2CH2) n OH (2)

[0045] m is an integer of 12 to 20, and n is an integer of 4 to 50, wherein when m is 12 to 15, n is an integer of 8 to 50, and when m is 16 to 20, n is an integer of 4 to 50;

[0046] 0.5 to 15.0 parts by mass of (D) polyoxyethylene sorbitan fatty acid ester represented by the following general formula (3):

[0047] [Chemical formula 2]

[0048]

[0049] R 2 is an alkyl group having 12 to 18 carbon atoms, and the total of a+b+c is 20;

[0050] 50 to 100,000 parts by mass of (E) water.

[0051] According to the mold release agent for plastic of the present invention, it is possible to provide a mold release agent for plastic which is an emulsion of an organopolysiloxane and which has excellent dilution stability and mechanical stability, good wettability, and is unlikely to cause cracks in plastics.

[0052] The plastic release agent of the present invention preferably further contains 5.0 parts by mass or less of (F) a sorbitan fatty acid ester represented by the following general formula (4) based on 100 parts by mass of the (A) organopolysiloxane.

[0053] [Chemical formula 3]

[0054]

[0055] R 3 It is an alkyl group having 12 to 22 carbon atoms.

[0056] By blending the above-mentioned sorbitan fatty acid ester, stress cracks can be further reduced in the plastic. In addition, the stability of the plastic release agent can be improved, the foaming property can be reduced, and the handling can be facilitated.

[0057] The content of the (F) sorbitan fatty acid ester is preferably 0.1 to 5.0 parts by mass.

[0058] When the content of (F) sorbitan fatty acid ester is within this range, cracks are less likely to occur when the mold release agent for plastics of the present invention is applied.

[0059] Furthermore, it is preferred that the content of the (B) anionic surfactant is 0.1 to 10.0 parts by mass.

[0060] When the content of the anionic surfactant (B) is within this range, the mechanical stability and releasability of the mold release agent for plastics of the present invention tend to be higher.

[0061] Furthermore, it is preferred that the average particle size of the plastic release agent is 100 nm or less.

[0062] Such a mold release agent for plastics tends to have good dilution stability and mechanical stability, and oil floating is less likely to occur during dilution or stirring.

[0063] Furthermore, it is preferred that the pH value of the plastic release agent at 25° C. is 4.0 to 10.0.

[0064] This is because, in the case of such a mold release agent for plastics, even if stored at high temperatures, the structure of the component (A) changes and the influence on the mold release properties of the plastic is small.

[0065] The mold release agent for plastics can be particularly suitably used for plastics for food container packaging.

[0066] This is because the plastic release agent of the present invention does not contain environmentally harmful substances such as nonylphenol and octylphenol, and the composition of the plastic release agent of the present invention can be composed only of raw materials approved by the "Voluntary Standards Related to Food Packaging Made of Synthetic Resins Such as Polyolefins", and such a plastic release agent is suitable as a release agent for food trays or egg packaging boxes.

[0067] Effects of the Invention

[0068] As described above, according to the present invention, it is possible to provide a plastic release agent which has good dilution stability, mechanical stability, and storage stability due to the small particle size of the emulsion, is excellent in wettability to plastics, and is less likely to cause stress cracks in plastics. In addition, the plastic release agent of the present invention can be composed of raw materials listed in the positive list provided by the Japan Polyolefin Sanitation Association, and is suitable for use in food container packaging. DETAILED DESCRIPTION

[0069] As described above, there is a need for an organopolysiloxane emulsion-type mold release agent that is excellent in dilution stability, mechanical stability, and storage stability, has good wettability, and does not cause cracks in plastics.

[0070] The inventors of the present application have conducted intensive studies to achieve the above-mentioned purpose and have found that by emulsifying a cellulose ester having a viscosity of 100 to 100,000 mm at 25° C. with an anionic surfactant, a polyoxyethylene alkyl ether, a polyoxyethylene sorbitan fatty acid ester and, if necessary, a sorbitan fatty acid ester, 2 / s of organopolysiloxane, an emulsion-type plastic release agent with an average particle size of 200nm or less can be prepared, and the obtained release agent has excellent dilution stability, mechanical stability, and storage stability, good wettability to plastics, and is not prone to stress cracking, thereby completing the present invention. In addition, the plastic release agent of the present invention can be composed of raw materials listed in the positive list of the Japan Polyolefin Sanitation Agreement, and can also be safely used in containers and packaging that are in direct contact with food.

[0071] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.

[0072] [Mold release agent for plastics]

[0073] The mold release agent for plastics of the present invention is a mold release agent for plastics characterized by containing the following components (A) to (E) and having an average particle size of 200 nm or less:

[0074] 100 parts by mass of (A) an organopolysiloxane represented by the following general formula (1) and having a viscosity at 25° C. of 100 to 100,000 mm 2 / s,

[0075] [Chemical formula 4]

[0076]

[0077] In formula (1), R 1are optionally the same or different, and are any one of a hydroxyl group, a hydrogen atom, a linear unsubstituted alkyl group having 1 to 32 carbon atoms, and a phenyl group, L is an integer from 60 to 1500, and the content of each of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane in the organopolysiloxane (A) is less than 3%;

[0078] 0.1 to 15.0 parts by mass of (B) anionic surfactant, which is one or more selected from alkyl sulfonates, alkylbenzene sulfonates, α-olefin sulfonates, polyoxyethylene alkyl ether sulfates, alkyl ether sulfates, polyoxyethylene alkyl ether acetates, alkyl acetates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, alkyl sulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, methyltaurine, alanine esters and salts thereof;

[0079] 1.0 to 30.0 parts by mass of (C) polyoxyethylene alkyl ether represented by the following general formula (2):

[0080] C m H 2m+1 (OCH2CH2) n OH (2)

[0081] m is an integer of 12 to 20, and n is an integer of 4 to 50, wherein when m is 12 to 15, n is an integer of 8 to 50, and when m is 16 to 20, n is an integer of 4 to 50;

[0082] 0.5 to 15.0 parts by mass of (D) polyoxyethylene sorbitan fatty acid ester represented by the following general formula (3):

[0083] [Chemical formula 5]

[0084]

[0085] R 2 is an alkyl group having 12 to 18 carbon atoms, and the sum of a+b+c is 20;

[0086] 50 to 100,000 parts by mass of (E) water.

[0087] [(A) Organopolysiloxane]

[0088] 100 parts by mass of (A) an organopolysiloxane represented by the following general formula (1) and having a viscosity at 25° C. of 100 to 100,000 mm 2 / s.

[0089] [Chemical formula 6]

[0090]

[0091] In formula (1), R1 They are optionally the same or different and are any one of a hydroxyl group, a hydrogen atom, a linear unsubstituted alkyl group having 1 to 32 carbon atoms, and a phenyl group, and L is an integer from 60 to 1500. In addition, the content of each of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane in the organopolysiloxane (A) is less than 3%.

[0092] In the above formula (1), R 1 It is optionally the same or different, and is any one of a straight-chain unsubstituted alkyl group, a phenyl group, a hydroxyl group and a hydrogen atom having 1 to 32 carbon atoms. L is an integer from 60 to 1500, preferably from 150 to 1200. As straight-chain unsubstituted alkyl groups having 1 to 32 carbon atoms, methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, n-decyl, n-dodecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, eicosyl and other alkyl groups can be cited. Preferably, a straight-chain unsubstituted alkyl group or a phenyl group having 1 to 20 carbon atoms is used, and from the perspective of versatility, a methyl group or a phenyl group is more preferred. In addition, from the perspective of mold release, it is preferred that at least 50 mol% of the organic groups bonded to the silicon atom in one molecule are methyl groups.

[0093] If the organopolysiloxane (A) contains a large amount of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane, it may become difficult to emulsify, or the average particle size may become larger, or the storage stability, dilution stability and mechanical stability may decrease. The contents of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane in the organopolysiloxane (A) are respectively less than 3%. Preferably, they are respectively less than 1%, and more preferably, they are respectively less than 0.1%. In addition, the lower limit of each content is not limited, and can be set to 0.001%, for example.

[0094] The viscosity of the organopolysiloxane of the component (A) at 25°C is 100 to 100,000 mm 2 / s. If the viscosity is less than 100mm 2 / s, the obtained composition cannot show sufficient mold release properties. In addition, the minimum viscosity of dimethyl polysiloxane, methyl hydrogen polysiloxane and methyl phenyl polysiloxane registered in the positive list of the Japan Polyolefin Hygiene Association is 100 mm 2 On the other hand, if the viscosity of the organopolysiloxane of component (A) is greater than 100,000 mm 2 / s, when applied to a film, the surface may become sticky. Preferably, it is 200 to 50,000 mm 2 / s, more preferably 300 to 10,000 mm 2 / s.

[0095] The organopolysiloxane of the component (A) may have a viscosity at 25° C. within the above range, and may be used alone or in combination of two or more.

[0096] [(B) Anionic surfactant]

[0097] 0.1 to 15.0 parts by mass of (B) anionic surfactant, which is one or more selected from alkyl sulfonates, alkylbenzene sulfonates, α-olefin sulfonates, polyoxyethylene alkyl ether sulfates, alkyl ether sulfates, polyoxyethylene alkyl ether acetates, alkyl acetates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, alkyl sulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, methyltaurine, alanine esters and salts thereof.

[0098] The anionic surfactants of the following structures among the above-mentioned anionic surfactants are anionic surfactants listed in the positive list of the Japan Polyolefin Sanitation Association. When the plastic release agent of the present invention is used for plastics for food container packaging, it is more preferable to select an anionic surfactant of the following structure. The alkyl group of the alkyl sulfonate has 10 to 20 carbon atoms, and the salt is sodium, potassium, or ammonium. The number of carbon atoms is preferably 10 to 15. If the number of carbon atoms is within the range of 10 to 15, the emulsion as the plastic release agent of the present invention is easy to be reduced in particle size and has good storage stability. The alkyl group of the alkylbenzene sulfonate has 9 to 20 carbon atoms, and the salt is sodium, potassium, or ammonium. The number of carbon atoms is preferably 9 to 15. If the number of carbon atoms is within the range of 9 to 15, the plastic release agent of the present invention is easy to be reduced in particle size and has good storage stability. The alkyl group of the alkyl ether sulfate has 12 to 16 carbon atoms, and the salt is a sodium salt. The alkyl group of the alkyl sulfosuccinate has 4 to 16 carbon atoms. The carbon number of the alkyl group of the polyoxyethylene alkyl ether sulfate is 12 to 20, and the salt is sodium and ammonium. The carbon number is preferably 12 to 16. If the carbon number is within the range of 12 to 16, the plastic release agent of the present invention is easy to reduce the particle size and has good storage stability. The carbon number of the alkyl group of the polyoxyethylene alkyl ether phosphate is 12 to 13, and the carbon number of the polyoxyethylene group is 4 to 10. The carbon number of the alkyl group of the alkyl acetate is 8 to 22, and the salt is sodium, potassium, or ammonium.

[0099] The anionic surfactant as the emulsifier component (B) is 0.1 to 15.0 parts by mass relative to 100 parts by mass of the organopolysiloxane as the component (A). It is preferably 0.1 to 10.0 parts by mass, and more preferably 0.1 to 8.0 parts by mass. If it is less than 0.1 parts by mass, the mechanical stability of the plastic release agent of the present invention may be reduced. On the other hand, if it is more than 15.0 parts by mass, the demoulding property may be reduced.

[0100] [(C) Polyoxyethylene alkyl ether]

[0101] 1.0 to 30.0 parts by mass of (C) polyoxyethylene alkyl ether represented by the following general formula (2).

[0102] C m H 2m+1 (OCH2CH2) n OH (2)

[0103] m is an integer of 12 to 20, and n is an integer of 4 to 50, wherein when m is 12 to 15, n is an integer of 8 to 50, and when m is 16 to 20, n is an integer of 4 to 50.

[0104] The alkyl group m of the polyoxyethylene alkyl ether (C) of the above formula (2) is an integer of 12 to 20, preferably an integer of 13 to 18, and more preferably an integer of 13 to 16. If m is less than 12, cracks may occur in the plastic coated with the plastic release agent of the present invention. On the other hand, if it is greater than 20, the particle size of the plastic release agent of the present invention is not easy to become fine, and the storage stability, dilution stability and mechanical stability may be reduced. In addition, either a branched alkyl group or a straight-chain alkyl group can be used, as long as the selection is based on the ease of emulsification of the organopolysiloxane of component (A) or the degree to which cracks are not easily generated when applied to the plastic.

[0105] The number n of the polyoxyethylene alkyl ether of the component (C) of the above formula (2) is an integer of 4 to 50. It is preferably 4 to 30, and more preferably 4 to 25. If n is less than 4, cracks may occur in the plastic coated with the plastic release agent of the present invention. On the other hand, if n is greater than 50, the polyoxyethylene alkyl ether of the above formula (2) becomes solid and becomes difficult to handle.

[0106] In addition, when the alkyl group is shorter and the polyoxyethylene chain is shorter, cracks are more likely to occur in the plastic. Therefore, when using polyoxyethylene alkyl ethers with shorter alkyl groups, polyoxyethylene alkyl ethers with shorter polyoxyethylene chains should be avoided. Specifically, when m is 12 to 15, n is preferably an integer of 8 to 50; when m is 16 to 20, n is preferably an integer of 4 to 50.

[0107] The polyoxyethylene alkyl ether of component (C) may be used alone or in combination of two or more. The HLB of the polyoxyethylene alkyl ether of component (C) can be set to 8 to 18, preferably 10 to 17, and more preferably 13 to 16. When storage stability, mechanical stability, and dilution stability cannot be obtained, a polyoxyethylene alkyl ether having a higher HLB of 15 to 18 and a polyoxyethylene alkyl ether having a lower HLB of 8 to 12 are used in combination so that the HLB becomes 13 to 16, thereby improving the storage stability, mechanical stability, and dilution stability. On the other hand, when a large amount of polyoxyethylene alkyl ether of component (C) having an HLB of 8 to 12 is contained, the release agent for plastics of the present invention may cause cracks in the plastic, so it is preferred that the blending amount of component (C) of such a structure is small.

[0108] The blending amount of the polyoxyethylene alkyl ether of the component (C) is 1.0 to 30.0 parts by mass. It is preferably 2.0 to 25.0 parts by mass, and more preferably 3.0 to 21.0 parts by mass. If it is less than 1.0 parts by mass, the storage stability, dilution stability, and mechanical stability of the plastic release agent of the present invention may be reduced, and the wettability to the plastic may be reduced. On the other hand, if it is more than 30.0 parts by mass, cracks may occur when the plastic release agent of the present invention is applied to the plastic.

[0109] Examples of the polyoxyethylene alkyl ether of the component (C) include the following polyoxyethylene alkyl ethers, but the polyoxyethylene alkyl ethers are not limited to these polyoxyethylene alkyl ethers.

[0110] Polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene hexyldecyl ether, polyoxyethylene isostearyl ether, polyoxyethylene octyldodecyl ether.

[0111] [(D) Polyoxyethylene sorbitan fatty acid ester]

[0112] 0.5 to 15.0 parts by mass of (D) polyoxyethylene sorbitan fatty acid ester represented by the following general formula (3).

[0113] [Chemical formula 7]

[0114]

[0115] R 2 It is an alkyl group having 12 to 18 carbon atoms, and the total of a+b+c is 20.

[0116] R 2It is an alkyl group having 12 to 18 carbon atoms, and the total of a+b+c is 20. Among them, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monooleate, and polyoxyethylene sorbitan monostearate having 12, 16, and 18 carbon atoms are approved as food additives and are therefore suitable for use in the plastic release agent for food container packaging of the present invention.

[0117] The polyoxyethylene sorbitan fatty acid ester as the component (D) has a relatively high emulsifying power for the organopolysiloxane as the component (A), and is not prone to cracking when applied to plastic. In addition, by using the polyoxyethylene alkyl ether as the component (C) together with the polyoxyethylene sorbitan fatty acid ester as the component (D) and the sorbitan fatty acid ester as the component (F) described below, the stability of the emulsion obtained by emulsifying the organopolysiloxane as the component (A) can be improved.

[0118] The amount of polyoxyethylene sorbitan fatty acid ester as component (D) is 0.5 to 15.0 parts by mass. Preferably, it is 0.5 to 10.0 parts by mass, and more preferably, it is 2.0 to 10.0 parts by mass. If component (D) is not blended or the amount of component (D) is less than 0.5 parts by mass, the stability of the emulsion obtained by emulsifying the organopolysiloxane as component (A) may decrease. On the other hand, if it is more than 15.0 parts by mass, cracks may occur when the plastic release agent of the present invention is applied to the plastic.

[0119] [(E) Water]

[0120] 50 to 100,000 parts by mass of (E) water.

[0121] The amount of water added as the (E) component is 50 to 100,000 parts by mass. Preferably, it is 500 to 20,000 parts by mass, and more preferably, it is 2,000 to 10,000 parts by mass. If the (E) water is less than 50 parts by mass, stickiness, uneven coating, and cracks may occur when the plastic release agent of the present invention is applied to the plastic. On the other hand, if the (E) water is more than 100,000 parts by mass, the mechanical stability may decrease, and oil floating may occur after dilution and stirring.

[0122] [(F) Sorbitan fatty acid ester]

[0123] The mold release agent for plastics of the present invention preferably further contains 5.0 parts by mass or less of (F) a sorbitan fatty acid ester represented by the following general formula (4) based on 100 parts by mass of the (A) organopolysiloxane.

[0124] [Chemical formula 8]

[0125]

[0126] R 3 It is an alkyl group having 12 to 22 carbon atoms.

[0127] R 3 is an alkyl group having 12 to 22 carbon atoms. From the viewpoint of emulsification, it is preferably 12 to 20, and more preferably 12 to 18. 3 If the carbon number of the alkyl group is 12 or more, no cracks will occur when applied to the synthetic resin. 3 If the carbon number of the alkyl group is 22 or less, the applied synthetic resin will not whiten. Sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monooleate, sorbitan monopalmitate, and sorbitan monostearate are approved for use as food additives and are compounds approved by the positive list of the voluntary standards related to food containers and packaging of the Japan Polyolefin Sanitation Association, and are most suitable for the use of the present invention.

[0128] The blending amount of the sorbitan fatty acid ester as the component (F) can be set to 0.1 to 5.0 parts by mass. It is preferably 0.1 to 3.0 parts by mass, and more preferably 0.2 to 3.0 parts by mass. If the sorbitan fatty acid ester as the component (F) is 5.0 parts by mass or less, cracks are less likely to occur when applying the plastic release agent of the present invention.

[0129] As described above, in order to improve the storage stability, mechanical stability, and dilution stability of the plastic release agent of the present invention, it is effective to use a high HLB and a low HLB polyoxyethylene alkyl ether as the component (C). However, a plastic release agent containing a large amount of polyoxyethylene alkyl ether as the component (C) with an HLB of 8 to 12 may cause stress cracks in the plastic. The HLB of sorbitan fatty acid ester as the component (F) is generally low at 3.0 to 10.0, but it is less likely to cause stress cracks in the plastic than the component (C) with the same HLB. Moreover, by combining the components (D) and (F) to make the HLB of the plastic release agent 13 to 16, the stability of the plastic release agent is further improved. In addition, by blending the component (F), the foaming property may be reduced and the handling may become easier.

[0130] The total amount of the nonionic surfactant components (C), (D) and (F) can be set to 2.5 to 50.0 parts by mass relative to 100 parts by mass of the component (A). It is preferably 2.5 to 35.0 parts by mass, and more preferably 3.0 to 30.0 parts by mass. If it is 2.5 parts by mass or more, the stability of the plastic release agent of the present invention will not decrease, and it is not easy to produce light and dark separation or oil floating. In addition, when applied to plastic, uneven coating is not easy to occur. On the other hand, if it is 50.0 parts by mass or less, stress cracks are not easy to occur in the plastic when the plastic release agent is applied.

[0131] [Preparation of composition]

[0132] An example of a specific method for preparing the mold release agent for plastics of the present invention is mainly as follows.

[0133] (A) organopolysiloxane, (B) anionic surfactant, (C) polyoxyethylene alkyl ether, (D) polyoxyethylene sorbitan fatty acid ester, (F) sorbitan fatty acid ester as required, and a portion of (E) water are stirred for emulsification, and then diluted with the remaining (E) water. When component (A) is not easily emulsified, it can be easily emulsified by the following method: after adding a portion of each of components (A) to (D) and component (F) and a portion of component (E) and stirring, the remaining components (A) to (D) and component (F) are added and further stirred. Especially when the viscosity of component (A) is less than 1,000 mm 2 / s, the component (A) may not be easily emulsified. In such a case, emulsification can be easily performed by adding the components (A) to (D) and the component (F) in portions. A specific example of the emulsified formulation is as follows.

[0134] (A) organopolysiloxane, (B) anionic surfactant, (C) polyoxyethylene alkyl ether, (D) polyoxyethylene sorbitan fatty acid ester, and (F) sorbitan fatty acid ester as required, and part of (E) water are blended in COMBI MIX (PRIMIX Corporation), and emulsified using a homomixer (a stirrer utilizing the rotation of the rotor in the stator) at 2,000 rpm or a disperser (a stirrer utilizing the rotation of the toothed blades) at 2,000 rpm and an anchor mixer at 20 rpm. After the whole is emulsified, stirring is performed for 15 to 180 minutes using a disperser at 2,000 rpm and an anchor mixer at 30 rpm until the particle size reaches a predetermined value, and then the remaining (E) water is added and diluted using a homomixer at 2,000 to 3,000 rpm to prepare the plastic release agent of the present invention.

[0135] The temperature during emulsification is preferably 0 to 80°C, more preferably 10 to 60°C. When the temperature is 10°C to 80°C, emulsification tends to be easier and the prepared emulsion tends to be more stable. During emulsification, the pressure may be not only normal pressure but also reduced pressure or increased pressure. When emulsification is performed under reduced pressure or increased pressure, bubbles are less likely to be mixed in, and emulsification can be performed effectively. When reduced pressure is set, the pressure is preferably higher than the vapor pressure of the raw material so as not to volatilize the raw material. In addition, the emulsification time is not particularly specified, as long as it is set to the time to reach the target particle size, and is generally preferably set to 30 to 360 minutes.

[0136] The emulsifier used during emulsification is not particularly limited as long as it can stir the raw materials or the emulsified composition. Examples of the emulsifier include: a colloid mill (IKA, PUC, NISSEI, IWAKI CO., LTD.) having a stirring portion consisting of a rotor and a stator, a high shear mixer (Silverson, PRIMIX Corporation), a homogenizer (PRIMIX Corporation), a vacuum emulsifier (PRIMIX Corporation), a COMBI MIX (PRIMIX Corporation) which is a three-axis dispersion kneading machine composed of a homogenizer, a homogenizer and an anchor mixer, a twin-axis mixer having a co-rotating screw or a counter-rotating screw, such as HAAKE Mini Lab II (Thermo scientific), MC15, MC5 (Rheo Lab), etc.

[0137] In the plastic release agent of the present invention, in addition to the surfactant, water-soluble polymers such as polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, hydroxymethyl cellulose, polyvinyl pyrrolidone, alginate, xanthan gum, acrylic acid polymer, etc., which are protective colloids or thickeners, can be blended according to the purpose of the present invention. Furthermore, antibacterial agents such as oxazoline compounds and aromatic carboxylates, or preservatives, fragrances, antioxidants, rust inhibitors, dyes, fillers, curing catalysts, organic powders, inorganic powders, etc. can also be blended.

[0138] The average particle size of the plastic release agent of the present invention is 200 nm or less. Preferably, it is 150 nm or less, and more preferably, it is 100 nm or less. If the average particle size is greater than 200 nm, the dilution stability and mechanical stability may decrease, and oil floating may occur during dilution or stirring. In addition, when stored for a long time, separation of thick and thin particles may also occur. In addition, the lower limit of the average particle size is not particularly limited, and for example, it can be set to 10 nm. The measurement can be performed using LA920 or LA960 manufactured by HORIBA, Ltd., or N4 PLUS manufactured by Beckman Coulter, and the average particle size measured using LA960 is shown in this specification.

[0139] The pH value of the plastic release agent of the present invention is preferably 4.0 to 10.0 at 25° C., preferably 4.5 to 9.0, and more preferably 4.5 to 8.0. When the pH value is within the range of 4.0 to 10.0, the structural change of the component (A) during storage at high temperatures will have less influence on the release properties of the plastic.

[0140] The emulsion obtained in the above manner is extremely useful as a release agent for plastic sheets for food packaging. For example, the plastic release agent of the present invention containing 0.1 to 2.0% by weight of the component (A) can be applied by spin wetting, gravure or spraying. The amount of application is usually 0.01 to 1.0 g / m 2 , especially suitable for 0.02~0.2g / m 2 If 0.01g / m 2 If the mold release rate is 1.0 g / m 2 The following are preferred from the viewpoints of transparency and stickiness.

[0141] Examples of plastics for food containers and packaging include polyethylene, polypropylene, polymethylpentene, polybutene, ethylene-tetracyclododecene, ethylene-2-norbornene, polystyrene, AS resin, ABS resin, polyphenylene ether, polyacrylonitrile, polymethacrylic acid-styrene, methacrylic resin, nylon, polyethylene terephthalate, polycarbonate, polyvinyl alcohol, polyacetal, polybutylene terephthalate, polycyclohexylenedimethylene terephthalate), polyethylene naphthalate, and vinyl chloride.

[0142] According to the present invention, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester and, if necessary, sorbitan fatty acid ester are blended in a specific ratio and the organopolysiloxane is emulsified, thereby providing a plastic release agent having excellent releasability, good dilution stability and mechanical stability, and less prone to stress cracking.

[0143] Example

[0144] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples. In the following examples, the viscosity is a value measured at 25° C. using a BM-type or BH-type rotational viscometer or an Ostwald viscometer.

[0145] [Example 1]

[0146] [Chemical formula 9]

[0147]

[0148] 30 parts by mass (90 g) of the organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm) represented by the above formula (A) component [1] were stirred at 500 rpm using a HOMO DISPER MODEL 2.5 (manufactured by PRIMIX Corporation). 2 / s), 0.2 parts by mass (0.6 g) of the (B) component [1] EMAL 270J (manufactured by Kao Corporation, a 70% aqueous solution of polyoxyethylene alkyl ether sodium sulfate), 6.0 parts by mass (18 g) of the (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of the (D) component [1] NONION LT-221 (manufactured by NOF CORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (manufactured by NOF CORPORATION, sorbitan monolaurate) and 1.5 parts by mass (4.5 g) of water as the component (E)-1 were emulsified as a whole, stirred at 1,500 rpm for 20 minutes, and then 60.15 parts by mass (180.45 g) of water as the component (E)-2 was added, and diluted with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) at 1,500 rpm for 3 minutes. Then, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 1.

[0149] [Example 2]

[0150] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of the (B) component [1] EMAL 270J (manufactured by Kao Corporation, a 70% aqueous solution of polyoxyethylene alkyl ether sodium sulfate), 6.0 parts by mass (18 g) of the (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of the (D) component [1] NONION LT-221 (manufactured by NOF CORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (manufactured by NOF CORPORATION, sorbitan monolaurate) and 1.0 mass part (3.0 g) of water as the (E)-1 component were emulsified as a whole, and then stirred at 1,500 rpm for 20 minutes, and then 59.55 mass parts (178.65 g) of water as the (E)-2 component was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation), and then 0.1 mass part (0.3 g) of sodium benzoate and 0.05 mass part (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 2.

[0151] [Example 3]

[0152] [Chemical formula 10]

[0153]

[0154] 30 parts by mass (90 g) of the organopolysiloxane (1b) (L2 of about 200 and viscosity of 1,000 mm) represented by the above formula (A) component [2] were stirred at 500 rpm using HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation). 2 / s), 1.3 parts by mass (3.9 g) of (B) component [1] EMAL 270J (manufactured by Kao Corporation, 70% aqueous solution of sodium polyoxyethylene alkyl ether sulfate), 6.0 parts by mass (18 g) of (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of (D) component [1] NONION LT-221 (manufactured by NOF CORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of (F) component NONION LP-20R (manufactured by NOF CORPORATION, sorbitan monolaurate) and 1.0 parts by mass (3.0 g) of water as component (E)-1 were all emulsified and then treated with HOMO DISPER II was stirred at 1,500 rpm for 20 minutes, and then 59.55 parts by mass (178.65 g) of water as the (E)-2 component was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes with HOMO MIXER MARK II MODEL 2.5 (manufactured by PRIMIX Corporation). Then, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARK II MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 3.

[0155] [Example 4]

[0156] 30 parts by mass (90 g) of the component (A) [2] organopolysiloxane (1b) (L2 of about 200 and a viscosity of 1,000 mm 2 / s), 1.3 parts by mass (3.9 g) of the (B) component [1] EMAL 270J (manufactured by Kao Corporation, a 70% aqueous solution of sodium polyoxyethylene alkyl ether sulfate), 1.0 parts by mass (3.0 g) of the (B) component [2] Newcol 291M (manufactured by NIPPON NYUKAZAI CO., LTD., a 70% aqueous solution of sodium dioctyl sulfosuccinate), 1.25 parts by mass (3.75 g) of the (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of the (D) component [2] RHEODOL TW-O120V (manufactured by Kao Corporation, polyoxyethylene sorbitan monooleate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (NOF CORPORATION, sorbitan monolaurate) and 1.5 parts by mass (4.5 g) of water as the component (E)-1 were emulsified as a whole, and then stirred at 1,500 rpm for 20 minutes with HOMO DISPER II, and then 62.8 parts by mass (188.4 g) of water as the component (E)-2 was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes with HOMOMIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation), and then 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 4.

[0157] [Example 5]

[0158] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of (B) component [1] EMAL 270J (manufactured by Kao Corporation, 70% aqueous solution of sodium polyoxyethylene alkyl ether sulfate), 6.0 parts by mass (18 g) of (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., 80% aqueous solution of polyoxyethylene alkyl ether), 2.0 parts by mass (6.0 g) of (D) component [2] RHEODOLTW-O120V (manufactured by Kao Corporation, polyoxyethylene sorbitan monooleate), and 1.0 parts by mass (3.0 g) of water as component (E)-1 were emulsified as a whole, stirred at 1,500 rpm for 20 minutes, and then 59.55 parts by mass (178.65 g) of water as component (E)-2 were added, and the mixture was stirred at 1,500 rpm for 20 minutes. Then, HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) was stirred at 1,500 rpm for 3 minutes to dilute, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 5.

[0159] [Example 6]

[0160] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of the (B) component [1] EMAL 270J (manufactured by Kao Corporation, a 70% aqueous solution of polyoxyethylene alkyl ether sodium sulfate), 6.0 parts by mass (18 g) of the (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of the (D) component [2] RHEODOLTW-O120V (manufactured by Kao Corporation, polyoxyethylene sorbitan monooleate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (NOF CORPORATION, sorbitan monolaurate) and 1.0 mass part (3.0 g) of water as the (E)-1 component were emulsified as a whole, and then stirred at 1,500 rpm for 20 minutes, and then 59.55 mass parts (178.65 g) of water as the (E)-2 component was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation), and then 0.1 mass part (0.3 g) of sodium benzoate and 0.05 mass part (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 6.

[0161] [Comparative Example 1]

[0162] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of (B) component [1] EMAL 270J (manufactured by Kao Corporation, a 70% aqueous solution of sodium polyoxyethylene alkyl ether sulfate), 8.5 parts by mass (25.5 g) of (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether), 1.5 parts by mass (4.5 g) of water as component (E)-1, the whole was emulsified, stirred at 1,500 rpm for 20 minutes, and then 58.55 parts by mass (175.65 g) of water as component (E)-2 was added, and HOMO MIXER MARKII MODEL 2.5 (PRIMIX After dilution with stirring at 1,500 rpm for 3 minutes, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare emulsified composition 7.

[0163] [Comparative Example 2]

[0164] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of the component (B) [1] EMAL 270J (manufactured by Kao Corporation, 70% aqueous solution of sodium polyoxyethylene alkyl ether sulfate), 4.8 parts by mass (14.4 g) of the surfactant [2] EMULGEN 104P (2b) (manufactured by Kao Corporation, polyoxyethylene (4) lauryl ether), 1.6 parts by mass (4.8 g) of the component (D) [2] RHEODOL TW-O120V (manufactured by Kao Corporation, polyoxyethylene sorbitan monooleate), 0.4 parts by mass (1.2 g) of the component (F) NONION LP-20R (manufactured by NOFCORPORATION, sorbitan monolaurate) and 2.0 parts by mass (6.0 g) of water as the component (E)-1 were emulsified as a whole, and then stirred at 1,500 rpm for 20 minutes. Then, 59.75 parts by mass (179.25 g) of water as the component (E)-2 was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes using HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation). Then, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute using HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 8.

[0165] [Comparative Example 3]

[0166] 30 parts by mass (90 g) of component [3] organopolysiloxane (1c) (L1 is about 550, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane are each contained in an amount of 3.3%, and the viscosity is 7,000 mm 2 / s), 1.3 parts by mass (3.9 g) of the (B) component [1] EMAL 270J (manufactured by Kao Corporation, a 70% aqueous solution of polyoxyethylene alkyl ether sodium sulfate), 6.0 parts by mass (18.0 g) of the (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of the (D) component [1] NONION LT-221 (manufactured by NOFCORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (NOF CORPORATION, sorbitan monolaurate) and 2.0 parts by mass (6.0 g) of water as the component (E)-1 were emulsified as a whole, stirred at 1,500 rpm for 15 minutes, and then 58.55 parts by mass (175.65 g) of water as the component (E)-2 was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation), and then 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 9.

[0167] [Comparative Example 4]

[0168] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 6.0 parts by mass (18 g) of the (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of the (D) component [1] NONION LT-221 (manufactured by NOFCORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (manufactured by NOF CORPORATION, sorbitan monolaurate), and 1.5 parts by mass (4.5 g) of water as the (E)-1 component were emulsified as a whole, stirred at 1,500 rpm for 20 minutes, and then 60.35 parts by mass (181.05 g) of water as the (E)-2 component were added, and the mixture was stirred at 1,500 rpm for 20 minutes. Then, HOMO MIXER MARKII MODEL 2.5 (PRIMIX After dilution with stirring at 1,500 rpm for 3 minutes, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 10.

[0169] [Comparative Example 5]

[0170] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of component (B) [1] EMAL 270J (manufactured by Kao Corporation, 70% aqueous solution of sodium polyoxyethylene alkyl ether sulfate), 2.0 parts by mass (6.0 g) of surfactant [3] polyoxyethylene alkyl ether (2d) (C m H 2m+1 (OCH2CH2) n OH, m is 10, n is 3), 4.3 parts by mass (12.9 g) of a 65% aqueous solution (2e) of a surfactant [4] polyoxyethylene alkyl ether (C m H 2m+1 (OCH2CH2) nOH, m is 10, n is 40), 1.6 parts by mass (4.8 g) of the component (D) [1] NONION LT-221 (manufactured by NOF CORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of the component (F) NONION LP-20R (manufactured by NOF CORPORATION, sorbitan monolaurate) and 1.0 parts by mass (3.0 g) of water as the component (E)-1 were emulsified as a whole, stirred at 1,500 rpm for 20 minutes, and then 59.25 parts by mass (177.75 g) of water as the component (E)-2 were added, and the mixture was stirred at 1,500 rpm for 20 minutes. Then, HOMO MIXER MARKII MODEL 2.5 (PRIMIX After dilution with stirring at 1,500 rpm for 3 minutes, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 11.

[0171] [Comparative Example 6]

[0172] An aqueous solution obtained by dissolving 1 part (3 g) of component (B) [3]EMAL2FG in 9 parts (27 g) of water as component (E)-1 was added to a mixture of 29.914 parts (89.742 g) of octamethylcyclotetrasiloxane and 0.086 parts (0.258 g) of hexamethyldisiloxane, and stirred at 500 rpm using HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation). After the mixture was emulsified, the high-speed stirring was increased to 5,000 rpm for 15 minutes, and then 49.35 parts (148.05 g) of water as component (E)-2 was added and diluted by stirring at 1,500 rpm for 3 minutes using HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation). 2 The emulsion was emulsified twice at a pressure of 50°C for 20 hours, then cooled at about 15°C for 10 hours, and neutralized by adding 2 parts by mass (6 g) of a 10% sodium carbonate aqueous solution to obtain an emulsion of dimethylpolysiloxane. An equal amount of isopropanol was added to 100 parts by mass of the emulsion to extract dimethylpolysiloxane, and the extracted oil was washed with water and dried at 105°C. The viscosity of the dimethylpolysiloxane obtained at 25°C was about 10,000 mm 2 / s. In addition, the emulsion contains 1.9% of octamethylcyclotetrasiloxane, 0.8% of decamethylcyclopentasiloxane, and 0.15% of dodecamethylcyclohexasiloxane. 8.5 parts by mass (25.5 g) of the component (C) [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether) and 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added to 91.35 parts by mass (274.05 g) of the emulsion after emulsion polymerization, and mixed at 100 rpm for 30 minutes using an anchor-type stirring rod to prepare an emulsified composition 12.

[0173] [Comparative Example 7]

[0174] An aqueous solution obtained by dissolving 1 part (3 g) of component (B) [3]EMAL2FG in 9 parts (27 g) of water as component (E)-1 was added to a mixture of 29.914 parts (89.742 g) of octamethylcyclotetrasiloxane and 0.086 parts (0.258 g) of hexamethyldisiloxane, and stirred at 500 rpm using HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation). After the mixture was emulsified, the high-speed stirring was increased to 5,000 rpm for 15 minutes, and then 54.85 parts (164.55 g) of water as component (E)-2 was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes using HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation). 2 The emulsion was emulsified twice at a pressure of 50°C for 20 hours, then cooled at about 15°C for 10 hours, and neutralized by adding 2 parts by mass (6 g) of a 10% sodium carbonate aqueous solution to obtain an emulsion of dimethylpolysiloxane. An equal amount of isopropanol was added to 100 parts by mass of the emulsion to extract dimethylpolysiloxane, and the extracted oil was washed with water and dried at 105°C. The viscosity of the dimethylpolysiloxane obtained at 25°C was about 10,000 mm 2 / s. In addition, the emulsion contains 1.9% of octamethylcyclotetrasiloxane, 0.8% of decamethylcyclopentasiloxane, and 0.15% of dodecamethylcyclohexasiloxane. 3 parts by mass (9 g) of glycerol, 0.1 parts by mass (0.3 g) of sodium benzoate, and 0.05 parts by mass (0.15 g) of citric acid were added to 96.95 parts by mass (290.85 g) of the emulsion after emulsion polymerization, and mixed at 100 rpm for 30 minutes using an anchor-type stirring rod to prepare an emulsified composition 13.

[0175] [Comparative Example 8]

[0176] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of the (B) component [1] EMAL 270J (manufactured by Kao Corporation, a 70% aqueous solution of polyoxyethylene alkyl ether sodium sulfate), 12.0 parts by mass (36 g) of the (C) component [1] LEOCOL TDN90-80 (2a) (manufactured by Lion Specialty Chemicals Co., Ltd., an 80% aqueous solution of polyoxyethylene alkyl ether), 1.6 parts by mass (4.8 g) of the (D) component [1] NONION LT-221 (manufactured by NOF CORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (manufactured by NOF CORPORATION, sorbitan monolaurate) and 1.0 mass part (3.0 g) of water as the (E)-1 component were emulsified as a whole, and then stirred at 1,500 rpm for 20 minutes, and then 53.55 mass parts (160.65 g) of water as the (E)-2 component was added, and the mixture was diluted by stirring at 1,500 rpm for 3 minutes with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation), and then 0.1 mass part (0.3 g) of sodium benzoate and 0.05 mass part (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXER MARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 14.

[0177] [Comparative Example 9]

[0178] 30 parts by mass (90 g) of the component (A) [1] organopolysiloxane (1a) (L1 of about 550 and viscosity of 10,000 mm 2 / s), 1.3 parts by mass (3.9 g) of component (B) [1] EMAL 270J (manufactured by Kao Corporation, 70% aqueous solution of sodium polyoxyethylene alkyl ether sulfate), 4.8 parts by mass (14.4 g) of surfactant [5] polyoxyethylene alkyl ether (2f) (C m H 2m+1 (OCH2CH2) n OH, m is 22, n is 20), 1.6 parts by mass (4.8 g) of the (D) component [1] NONION LT-221 (manufactured by NOF CORPORATION, polyoxyethylene sorbitan monolaurate), 0.4 parts by mass (1.2 g) of the (F) component NONION LP-20R (manufactured by NOF CORPORATION, sorbitan monolaurate) and 2.5 parts by mass (7.5 g) of water as the (E)-1 component were emulsified as a whole, stirred at 1,500 rpm for 20 minutes, and then 59.25 parts by mass (177.75 g) of water as the (E)-2 component was added, and the mixture was stirred at 1,500 rpm for 20 minutes. Then, ... After dilution with stirring at 1,500 rpm for 3 minutes, 0.1 parts by mass (0.3 g) of sodium benzoate and 0.05 parts by mass (0.15 g) of citric acid were added, and the mixture was further stirred at 1,500 rpm for 1 minute with HOMO MIXERMARKII MODEL 2.5 (manufactured by PRIMIX Corporation) to prepare an emulsified composition 15.

[0179] The average particle size, pH value, centrifugal separation stability, water dilution stability, mechanical stability, wettability to plastic (PET), and stress cracking in plastic (OPS) were evaluated for the above examples and comparative examples. The results of these evaluations are shown in Tables 1 to 3.

[0180] Average particle size:

[0181] The values ​​were measured by diluting emulsified compositions 1 to 15 approximately 10 times with water and using HORIBA LA960.

[0182] pH value:

[0183] The values ​​obtained by measuring emulsified compositions 1 to 15 at 25°C using a pH meter (LAQUA manufactured by HORIBA, Ltd.).

[0184] Centrifugal separation stability:

[0185] Emulsified compositions 1 to 15 were placed in a dedicated tube of about 15 mL and rotated at 3,000 rpm for 15 minutes using a centrifuge H-19FM (manufactured by KOKUSAN Co. Ltd.). Then, 1.0 g of the non-volatile components in the upper layer and 1.0 g of the non-volatile components in the lower layer in the tube were measured (105° C.×3 hours).

[0186] The values ​​of upper layer non-volatile component / lower layer non-volatile component = 0.95 to 1.05 were considered acceptable. In other cases, light-dark separation may occur during storage over time.

[0187] Water dilution stability:

[0188] 2 g of each of the emulsified compositions 1 to 15 was mixed with 98 g of water to prepare plastic release agents 1. The entire amount was placed in a 200 mL beaker and allowed to stand for 1 day, and the surface of the plastic release agent 1 was observed.

[0189] ○: No separation of light and dark colors occurs, and the plastic release agent is dispersed.

[0190] There are no oil spots or interference films on the surface, or there is an interference film of about 10% to 30% on the surface.

[0191] △: No separation of light and dark colors occurs, and the plastic release agent is dispersed.

[0192] There are no oil spots or interference films on the surface, or there is an interference film of about 30% to 60% on the surface.

[0193] ×: The plastic release agent is unevenly dispersed.

[0194] Alternatively, interference films or oily spots of 60% or more are generated on the surface.

[0195] ○ and △ were marked as passing.

[0196] Mechanical stability:

[0197] 10 g of each of the emulsion compositions 1 to 15 was mixed with 90 g of water to prepare plastic release agents 2. The plastic release agents 2 were placed in a 200 mL beaker and stirred at 3,000 rpm for 10 minutes using HOMO MIXER MARKII, then left to stand for 1 day and the liquid level was observed.

[0198] ○: No separation of light and dark colors occurs, and the plastic release agent is dispersed.

[0199] There are no oil spots or interference films on the surface, or there is an interference film of about 10% to 30% on the surface.

[0200] △: No separation of light and dark colors occurs, and the plastic release agent is dispersed.

[0201] There are no oil spots or interference films on the surface, or there is an interference film of about 30% to 60% on the surface.

[0202] ×: The plastic release agent is unevenly dispersed.

[0203] Alternatively, interference films or oily spots of 60% or more are generated on the surface.

[0204] ○ and △ were marked as passing.

[0205] Wettability:

[0206] The plastic release agent 2 was applied onto a PET film using Wire Bar No. 3 (manufactured by RD Specialties, USA), and the coating unevenness was observed with the naked eye.

[0207] ○: Overall wetting

[0208] △: Uneven coating occurs in some areas

[0209] ×: Uneven coating occurs immediately after coating.

[0210] ○ and △ were marked as passing.

[0211] Crack resistance:

[0212] The above-mentioned plastic release agent 1 was applied to an OPS sheet using gauze. The OPS sheet was wound around a cylinder having a diameter of 37 mm, and the occurrence of cracks was visually checked.

[0213] ○: No cracks occurred within 75 seconds after winding on the drum

[0214] ×: Cracks occur within 75 seconds after winding on the drum

[0215] ○ was recorded as passing.

[0216] (Component (A) and comparative organopolysiloxane)

[0217] Component (A) [1]: organopolysiloxane (1a)

[0218] (L1 is about 550, viscosity is 10,000mm 2 / s)

[0219] Component (A) [2]: organopolysiloxane (1b)

[0220] (L2 is about 200, viscosity is 1,000mm2 / s)

[0221] The content of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane in the above-mentioned components (A) [1] and [2] is less than 0.1%.

[0222] Ingredient [3]: Organopolysiloxane (1c)

[0223] (L1 is about 550, the content of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane is 3.3%, and the viscosity is 7,000 mm 2 / s)

[0224] The organopolysiloxane (1c) is obtained by blending octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane into the organopolysiloxane (1a) of the component (A) so that each of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane is 3.3%.

[0225] Ingredient [4]: ​​Organopolysiloxane (1d)

[0226] (L1 is about 550)

[0227] The organopolysiloxane (1d) is prepared by emulsion polymerization, and contains 6.3% of octamethylcyclotetrasiloxane, 2.7% of decamethylcyclopentasiloxane, and 0.5% of dodecamethylcyclohexasiloxane in 100 parts by mass of the organopolysiloxane (1d).

[0228] (Component (B))

[0229] Component (B) [1]: EMAL 270J (manufactured by Kao Corporation)

[0230] 70% aqueous solution of sodium polyoxyethylene (2) alkyl ether sulfate

[0231] Component (B) [2]: Newcol 291M (manufactured by NIPPON NYUKAZAI CO., LTD.)

[0232] 70% aqueous solution of dioctyl sodium sulfosuccinate

[0233] Component (B) [3]: EMAL 2FG (manufactured by Kao Corporation)

[0234] Sodium lauryl sulfate

[0235] (Component (C) and comparative surfactant)

[0236] Component (C) [1]: LEOCOL TDN90-80 (manufactured by Lion Specialty Chemicals Co., Ltd., 80% aqueous solution of polyoxyethylene alkyl ether) (2a)

[0237] (C m H 2m+1 (OCH2CH2) n 80% aqueous solution of OH, m is 13, n is 9)

[0238] Surfactant [2]: EMULGEN 104P (manufactured by Kao Corporation, polyoxyethylene alkyl ether) (2b)

[0239] (C m H 2m+1 (OCH2CH2) n OH, m is 12, n is 4)

[0240] Surfactant[3]: Polyoxyethylene alkyl ether (2d)

[0241] (C m H 2m+1 (OCH2CH2) n OH, m is 10, n is 3)

[0242] Surfactant [4]: ​​65% aqueous solution of polyoxyethylene alkyl ether (2e)

[0243] (C m H 2m+1 (OCH2CH2) n OH, m is 10, n is 40)

[0244] Surfactant[5]: Polyoxyethylene alkyl ether (2f)

[0245] (C m H 2m+1 (OCH2CH2) n OH, m is 22, n is 20)

[0246] (ingredient (D))

[0247] Component (D) [1]: NONION LT-221 ((manufactured by NOF CORPORATION)

[0248] Polyoxyethylene sorbitan monolaurate

[0249] Component (D) [2]: RHEODOL TW-O120V (manufactured by Kao Corporation)

[0250] Polyoxyethylene sorbitan monooleate

[0251] (Ingredient (E))

[0252] Ingredient (E)-1, Ingredient (E)-2: Water

[0253] (ingredient (F))

[0254] Ingredient (F): NONION LP-20R (manufactured by NOF CORPORATION) Sorbitan monolaurate

[0255] [Table 1]

[0256]

[0257] [Table 2]

[0258]

[0259] [Table 3]

[0260]

[0261] In Comparative Examples 6 and 7, 1.0 parts by mass of a 10% aqueous solution of lauryl sulfuric acid was reacted with 2 parts by mass of a 10% aqueous solution of sodium carbonate, and the amount of sodium lauryl sulfate in the final emulsified composition was 1.1 parts by mass.

[0262] As can be seen from Table 1, the mold release agent for plastics of the present invention is an emulsion of organopolysiloxane which is excellent in dilution stability and mechanical stability, has good wettability, and is less likely to cause cracks in plastics.

[0263] On the other hand, Comparative Examples 1 and 6, which did not contain either the component (D) or the component (F) of the present invention, were inferior in mechanical stability and crack resistance.

[0264] In addition, it is considered that since the average particle size of the release agent in Comparative Examples 2, 6, and 7 was larger than 200 nm, the mechanical stability was reduced.

[0265] Unlike the component (C) of the present invention, C m H 2m+1 (OCH2CH2) n In Comparative Example 2 in which m in OH is 12 and n is 4, cracks are easily generated.

[0266] In addition, C in the component (C) of the present invention is used m H 2m+1 (OCH2CH2) n Comparative Example 5 of the surfactant [3] in which both m and n in OH are below the lower limit also easily causes cracks.

[0267] Furthermore, unlike the component (C) of the present invention, C m H 2m+1 (OCH2CH2) n In Comparative Example 9 in which n in OH was 20 and m was 22, the mechanical stability was reduced.

[0268] In Comparative Example 3, in which the contents of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane were each greater than 3%, the mechanical stability was reduced.

[0269] In Comparative Example 4 which did not contain the component (B) of the present invention, the mechanical stability was reduced.

[0270] In Comparative Example 7 which did not contain the components (C), (D) and (F) of the present invention, no nonionic surfactant was used, resulting in uneven coating and poor wettability.

[0271] In Comparative Example 8, in which the component (C) was contained in an amount exceeding the upper limit of the blending amount range of the component (A) of the present invention, cracks were likely to occur.

[0272] The above embodiments are merely examples, and any technical solution having substantially the same structure and having the same function and effect as the technical concept described in the claims of the present invention is included in the protection scope of the present invention.

Claims

1. A plastic release agent, characterized in that: It contains the following (A) to (E) components, wherein the average particle size of the plastic release agent is 100 nm or less and the pH value at 25° C. is 4.5 to 8.0: 100 parts by mass of (A) an organopolysiloxane represented by the following general formula (1) and having a viscosity at 25° C. of 100 to 100,000 mm 2 / s, In formula (1), R 1 are optionally the same or different, and are any one of a hydroxyl group, a hydrogen atom, a linear unsubstituted alkyl group having 1 to 32 carbon atoms, and a phenyl group, L is an integer from 60 to 1500, and the content of each of octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane in the organopolysiloxane (A) is less than 3%; 0.1 to 15.0 parts by mass of (B) anionic surfactant, which is one or more selected from alkyl sulfonates, alkylbenzene sulfonates, α-olefin sulfonates, polyoxyethylene alkyl ether sulfates, alkyl ether sulfates, polyoxyethylene alkyl ether acetates, alkyl acetates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, alkyl sulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, methyltaurine, alanine esters and salts thereof; 1.0 to 30.0 parts by mass of (C) polyoxyethylene alkyl ether represented by the following general formula (2): C m H 2m+1 (OCH2CH2) n OH(2) m is an integer of 12 to 20, and n is an integer of 4 to 50, wherein when m is 12 to 15, n is an integer of 8 to 50, and when m is 16 to 20, n is an integer of 4 to 50; 0.5 to 15.0 parts by mass of (D) polyoxyethylene sorbitan fatty acid ester represented by the following general formula (3): R 2 is an alkyl group having 12 to 18 carbon atoms, and the sum of a+b+c is 20; 50 to 100,000 parts by mass of (E) water.

2. The plastic release agent according to claim 1, characterized in that (F) a sorbitan fatty acid ester represented by the following general formula (4) in an amount of 5.0 parts by mass or less based on 100 parts by mass of the (A) organopolysiloxane, R 3 It is an alkyl group having 12 to 22 carbon atoms.

3. The plastic release agent according to claim 2, characterized in that: The content of the (F) sorbitan fatty acid ester is 0.1 to 5.0 parts by mass.

4. The plastic release agent according to claim 1, characterized in that: The content of the (B) anionic surfactant is 0.1 to 10.0 parts by mass.

5. The plastic release agent according to claim 2, characterized in that: The content of the (B) anionic surfactant is 0.1 to 10.0 parts by mass.

6. The plastic release agent according to claim 3, characterized in that: The content of the (B) anionic surfactant is 0.1 to 10.0 parts by mass.

7. The plastic release agent according to any one of claims 1 to 6, characterized in that The plastic release agent is used for plastics used for food container packaging.