A reversible thermosensitive color-changing microcapsule and preparation method thereof
By using bisphenol-type epoxy resin and epoxy-based POSS as microcapsule wall materials, combining hiding dyes and color developers, reversible thermally sensitive color-distorted microcapsules are prepared and applied to UV light-curing adhesives, the existing solutions are solved The lack of reversible thermally sensitive UV curing adhesives in the technology has achieved adhesives with high color development sensitivity and improved mechanical properties.
Patent Information
- Application Number
- CN202111317260.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-11-09
AI Technical Summary
The prior art lacks reversible thermally discolored UV curing adhesives, and the color-developing substances of reversible thermally discolored materials are easily disturbed by external environment, affecting the color-developing properties, and their applications are limited in the fields of ink and textiles.
Using bisphenol-type epoxy resin and epoxy-based POSS as microcapsule wall materials, combined with hiding dyes and color developers, reversible thermally discolored microcapsules are prepared by improving the ratio of sensitizers and applied to UV In photocuring adhesives, the mechanical properties and color rendering sensitivity of the adhesive are improved.
Reversible thermally sensitive color-changing UV light curing adhesive at a color change temperature of 80-90℃ has been achieved, with high color development sensitivity and improved shear strength, filling the market gap and suitable for a wider range of application fields.
Smart Images

Figure BDA0003343944280000111 
Figure BDA0003343944280000121
Abstract
Description
Technical Field
[0001] The invention belongs to the field of thermochromic materials, and specifically relates to a reversible thermochromic microcapsule and a preparation method thereof, and a UV light-curing adhesive controlled by the reversible thermochromic microcapsule. Background Art
[0002] Thermochromic materials are intelligent materials that can show different colors due to temperature changes. Thermochromic materials are widely used in industry, medical treatment, anti-counterfeiting and other fields, and have broad market prospects. Thermochromic materials are divided into reversible thermochromic materials and irreversible thermochromic materials. There are three main categories of reversible thermochromic materials, namely inorganic, organic and liquid crystal thermochromic materials. Among them, organic reversible thermochromic materials are often composed of electron donors, electron acceptors, regulators, sensitizers and other solvents. Leuco dyes are substances that can develop color by combining with protons, such as lactone compounds. In the color-changing system, they act as electron-donating parts and determine the color change. The color displayed varies with different substituents, but the conjugated system in its molecules is interrupted, and it needs to react with the developer under certain conditions to develop color. The developer is an acid-releasing compound that reversibly releases protons, that is, an electron-withdrawing compound, which determines the depth of color. The temperature regulator mainly affects the temperature of thermochromism. When it melts, the color developer and the leuco dye separate, hindering the formation of the conjugated system. At this time, the system is colorless. For example, the leuco dye is a color-changing system of crystal violet lactone and the color developer bisphenol A. In a certain medium, when the temperature drops to a certain level, bisphenol A releases protons, that is, gains electrons, crystal violet lactone opens the ring, the molecule rearranges, the conjugated double bonds penetrate and combine with bisphenol A ions, thus showing color.
[0003] Since the color-developing substance itself has certain physical and chemical properties, it is easy to be interfered by other substances in the system and affect the color-developing properties when added to other chemical systems. At the same time, the color-developing substance may also react chemically with the components in the system, making the system as a whole ineffective. In order to solve the problem of mutual interference between the color-developing substance and the external environment, the application of thermosensitive microcapsule technology was born. The shell-core structure is adopted to wrap the color-developing substance with a more stable material, isolate the color-developing substance from the external environment, and is not affected by other substances and does not affect other substances. Thermosensitive microcapsules are micro-containers with polymer wall shells that can encapsulate and protect the color-developing substance in its capsule core. The capsule wall of the thermosensitive microcapsule is usually composed of a seamless, solid film, and the capsule core is the encapsulated color-developing substance. The particle size of the thermosensitive microcapsule is generally in the range of 5-200μm, or in the millimeter range, and the thickness of the capsule wall is generally in the range of 0.2-2μm.
[0004] Patent document 201611248508.9 discloses a thermochromic microcapsule UV light-curing ink, including 22-60 parts of epoxy acrylate, 15-25 parts of color-developing microcapsules, 15-25 parts of polyester acrylate, 10-15 parts of dipropylene glycol diacrylate, 5-10 parts of trimethylolpropane triacrylate, 5-10 parts of 4-hydroxybutyl acrylate, 0.5-3 parts of benzoin dimethyl ether, 1-5 parts of dispersant, 1-5 parts of hollow glass microspheres, and 1-3 parts of UV ink varnish. The preparation method of the color-developing microcapsule core material includes: taking 5-10 parts of thermosensitive pigment, 12-22 parts of color developer, and 13-18 parts of sensitizer, mixing and stirring for 1-2 hours to obtain the core material. ① Take 10L of water, heat it to 50℃, add 250g of Arabic resin and 250g of gelatin, stir at a speed of 5000r / min until dissolved, and obtain a mixed resin solution; ② Take 98 parts of the mixed resin solution in step ①, add core material and 2 parts of nano-silicon dioxide, add 6g / L acetic acid aqueous solution at 300r / min, adjust pH=4, stir at 5000r / min for 15-30min, prepare O / W type emulsion with a mixing emulsifier, let stand, and cool to 3℃; ③ Heat to 50℃ at 300r / min, adjust pH=9 with 10g / L sodium hydroxide solution, keep warm for 40min, let stand, cool to room temperature, centrifuge, and dry to obtain color microcapsules. In the technical scheme, Arabic resin and gelatin are used as wall materials of color microcapsules. Since the cross-linking density of the resin is small, the color-developing substance can only be wrapped when the capsule wall is thick, and when the capsule wall is thick, it will affect the color appearance.
[0005] At present, reversible thermochromic materials are mostly used in the fields of ink, textiles, etc., and there is no reversible thermochromic UV curing adhesive on the market. In order to fill this gap, the present invention provides a reversible thermochromic UV light curing adhesive, the adhesive is color-controlled by reversible thermochromic microcapsules, and the mechanical properties of the UV curing adhesive containing the microcapsules can be improved by improving the raw materials of the capsule wall. In addition, by improving the sensitizer raw materials and ratio of the thermochromic microcapsules, an adhesive with higher color sensitivity can be prepared. Summary of the invention
[0006] One object of the present invention is to provide a reversible thermochromic microcapsule and a preparation method thereof. Another object of the present invention is to provide a reversible thermochromic UV light-curing adhesive comprising the reversible thermochromic microcapsule and a preparation method thereof.
[0007] In a first aspect, the present invention provides a reversible thermosensitive color-changing microcapsule, characterized in that the microcapsule is prepared by coating a core material with a wall material, the wall material comprises a bisphenol epoxy resin, and the core material consists of a leuco dye, a developer and a sensitizer.
[0008] Preferably, the wall material comprises bisphenol epoxy resin and epoxy cage silsesquioxane, and the mass ratio of bisphenol epoxy resin to epoxy cage silsesquioxane is 1:(0.1-0.2).
[0009] The bisphenol epoxy resin is one or a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydrogenated bisphenol A epoxy resin, and the epoxy equivalent of the epoxy resin is 155-190.
[0010] In a preferred embodiment of the present invention, the epoxy POSS is one or a combination of two or more of octa(2,3-glycidoxypropyl)T8-POSS (CAS#164017-77-0), deca(2,3-glycidoxypropyl)T10-POSS (CAS#690993-04-5). Most preferably, the epoxy POSS is deca(2,3-glycidoxypropyl)T10-POSS.
[0011] Preferably, the reversible thermochromic microcapsules include the following raw materials in parts by weight: 10-35 parts of wall material, 30-65 parts of wall material solvent, 2-7 parts of leuco dye, 2-7 parts of developer, 2-7 parts of sensitizer, 0.02-0.15 parts of emulsifier, and 2-10 parts of curing agent.
[0012] The wall material solvent includes any one of n-hexane, n-pentane, ethyl acetate, methanol and isobutanol.
[0013] The leuco dye is a fluoran with a lactone ring structure, including any one of crystal violet lactone, 4-(dimethyl)-2,3-diethylaminofluoran, 6-(diethylamino)-1,3-dimethylfluoran, 2-(dibenzylamino)-3-(dimethyl)fluoran, 1,3-dimethyl-6-ethylfluoran, 2-(1,3-diethylamino)-3-ethyl-6-dimethylfluoran, and 3-isoamyl-6-phenylamino-7-methylfluoran, or a combination of two or more thereof.
[0014] The developer comprises one or a combination of two or more of bisphenol A, 2,4-diphenylsulfone phenol, 4,4-dihydroxydiphenyl sulfone, 2,2-di(6-hydroxyphenyl)pentane, 4-methoxyphenol, and small molecule carboxylic acids.
[0015] The sensitizer includes one or a combination of two or more paraffin waxes, modified waxes, microcrystalline waxes and polymer waxes of different brands. The polymer wax is polyethylene wax, polypropylene wax and polytetrafluoroethylene wax. The modified wax is maleated wax and fumarated wax. The acidification grafting rate is 1-3%.
[0016] The maleated wax and fumarated wax used in the present invention can be purchased through commercial channels or prepared by oneself. For example, the preparation method of the maleated wax used in the embodiment of the present invention is as follows: 10 parts of paraffin wax and 1 part of maleic anhydride are added to a four-necked flask, an inert gas is passed through, 0.5 parts of BPO as an initiator is slowly added, and the reaction is carried out for 30 minutes to obtain a product, and the maleic anhydride grafting rate is 2%.
[0017] Preferably, the sensitizer is a combination of modified wax and polymer wax or a combination of microcrystalline wax and polymer wax, and the mass fraction of the polymer wax is 5-20%.
[0018] In the most preferred embodiment of the present invention, the sensitizer is a combination of modified wax and polytetrafluoroethylene wax, or a combination of microcrystalline wax and polytetrafluoroethylene wax, and the mass fraction of polytetrafluoroethylene wax in the sensitizer is 10-20%.
[0019] The emulsifier includes one or a combination of two or more of betaine, gum arabic, Tween-60, Span-30, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate.
[0020] The curing agent is one or a combination of two or more of a phenol curing agent, an acid anhydride curing agent and an amine curing agent.
[0021] In a second aspect, the present invention provides a method for preparing reversible thermochromic microcapsules, the method comprising the following steps:
[0022] (1) Weighing the epoxy resin and / or epoxy POSS as wall material components according to their mass fractions, adding the wall material solvent, and stirring to completely dissolve them to obtain a solution A;
[0023] (2) Weighing the leuco dye, developer and sensitizer according to their mass fractions, heating to a temperature above the melting point of the sensitizer, stirring the system evenly, and maintaining the heating temperature to obtain solution B;
[0024] (3) Mixing solution A and solution B while maintaining the heating temperature, stirring evenly, to obtain solution C;
[0025] (4) Weighing an emulsifier by mass and dissolving it in water, adding solution C to the emulsifier solution, and dispersing at a high speed of 1500-2000 r / min for 1-2 hours to obtain emulsion D;
[0026] (5) Weighing a curing agent by mass and dissolving it in water to obtain a solution E, and adding the solution E dropwise to the emulsion D under high-speed shear dispersion at 1500-2000 r / min, keeping the system temperature higher than the melting point of the sensitizer and reacting for 5-6 hours to obtain an emulsion product F;
[0027] (6) The emulsion product F is filtered, and the obtained solid G is repeatedly washed with a wall material solvent and dried to obtain reversible thermosensitive color-changing microcapsules.
[0028] In a third aspect, the present invention provides a reversible thermochromic UV light-curing adhesive, characterized in that the UV light-curing adhesive comprises the following raw materials in parts by mass: 50-80 parts of liquid acrylic resin, 20-40 parts of acrylic monomer, 0.5-3 parts of free radical photoinitiator, 5-10 parts of filler, and 5-10 parts of the above-mentioned reversible thermochromic microcapsules.
[0029] In a fourth aspect, the present invention provides a method for preparing a reversible thermochromic UV light-curing adhesive, which is as follows: 50-80 parts of liquid acrylic resin, 20-40 parts of acrylic monomer, 0.5-3 parts of free radical photoinitiator, and 5-10 parts of filler are added into a stirring kettle, and uniformly dispersed at a speed of 500-1000r / min for 1-2 hours at room temperature and -0.1MPa conditions, then 5-10 parts of reversible thermochromic microcapsules are added, and then uniformly dispersed at a speed of 1000-1500r / min for 0.5-1 hour, and the temperature is kept not higher than 40°C during the dispersion process, and the reversible thermochromic UV light-curing adhesive is obtained by discharging the material.
[0030] The liquid acrylic resin is selected from one or a combination of two or more of silicone-modified polyacrylate, polyurethane acrylate and epoxy acrylate.
[0031] The acrylic acid monomer is selected from one or a combination of two or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, 2-hydroxypropyl methacrylate and 2-hydroxypropyl acrylate;
[0032] The free radical photoinitiator is selected from methyl benzoylformate, 2,2-dimethoxy-phenylacetophenone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, and 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone, or a combination of two or more thereof.
[0033] The filler is selected from one or a combination of two or more of fumed silica, alumina, aluminum powder, titanium dioxide, quartz powder, and mica powder.
[0034] The reversible thermochromic UV light-curing adhesive provided by the present invention has the following advantages: 1. At present, the color change temperature of most reversible thermochromic adhesives on the market is about 40°C, and color change will occur during the curing process of the adhesive. In order to fill the market gap and meet the needs of some users, the present invention provides a reversible thermochromic adhesive with a color change temperature of 80-90°C; 2. The adhesive prepared by the present invention has good color sensitivity; 3. By adding epoxy POSS to the microcapsule wall material, the shear strength of the adhesive is improved. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only some embodiments of the present invention, not all. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Preparation of reversible thermochromic microcapsules
[0037] Preparation Example 1
[0038] S1: Weigh 5 g of bisphenol A epoxy resin (epoxy equivalent weight 195), dissolve it in 10 g of n-hexane, and stir evenly until it is completely dissolved to obtain solution A;
[0039] S2: Weigh 1 g of crystal violet lactone, 1 g of 2,4-diphenylsulfonylphenol and 5 g of paraffin, and heat in a 95°C water bath with magnetic stirring for 0.5 h until the system is completely mixed to obtain solution B;
[0040] S3: Keep heating in a water bath at 95°C, mix solution A and solution B, and stir magnetically for 0.5 h to obtain solution C;
[0041] S4: Measure 150 mL of a 10% betaine solution, preheat it to 95°C, add solution C thereto, keep heating in a water bath at 95°C, and high-speed shear dispersion at a speed of 2000 r / min for 1 h to obtain emulsion D;
[0042] S5: Weigh 2.0 g of aliphatic amine curing agent (active hydrogen equivalent 68), dissolve it in distilled water at a mass ratio of 1:4 to obtain solution E, add solution E dropwise to emulsion D under high-speed shear dispersion at 2000 r / min, keep the reaction at 95°C for 6 h, and obtain emulsion product F;
[0043] S6: filtering the emulsion product F, and repeatedly washing the obtained solid G with n-hexane, and drying to obtain reversible thermosensitive color-changing microcapsules.
[0044] Preparation Example 2
[0045] S1: Weigh 5 g of bisphenol F epoxy resin (epoxy equivalent weight 160), dissolve it in 10 g of isobutyl alcohol, and stir evenly until it is completely dissolved to obtain solution A;
[0046] S2: Weigh 1 g of 6-(diethylamino)-1,3-dimethylfluoran, 1 g of 4,4-dihydroxydiphenyl sulfone and 6 g of microcrystalline wax, and heat them in a water bath at 80°C with magnetic stirring for 0.5 h until the system is completely and evenly mixed to obtain solution B;
[0047] S3: Keep heating in a water bath at 80°C, mix solution A and solution B, and keep magnetic stirring for 0.5h to obtain solution C;
[0048] S4: Measure 150 mL of 10% Tween-60 solution, preheat to 80°C, add solution C thereto, keep heating at 80°C in a water bath, and high-speed shear dispersion at a speed of 2000 r / min for 1 h to obtain emulsion D;
[0049] S5: Weigh 2.5 g of a polyetheramine curing agent (active hydrogen equivalent 75) and dissolve it in distilled water at a mass ratio of 1:4 to obtain a solution E. Add the solution E dropwise to the emulsion D under high-speed shear dispersion at 2000 r / min, and keep the reaction at 80° C. for 6 h to obtain an emulsion product F.
[0050] S6: filtering the emulsion product F, and repeatedly washing the obtained solid G with isobutyl alcohol, and drying to obtain reversible thermosensitive color-changing microcapsules.
[0051] Preparation Example 3
[0052] The preparation method is the same as that of Preparation Example 1, except for step S1, which is as follows: 4.5 g of bisphenol A epoxy resin (epoxy equivalent 195) and 0.5 g of octa(2,3-glycidoxypropyl) T8-POSS are weighed, dissolved in 10 g of n-hexane, and stirred evenly until completely dissolved to obtain solution A.
[0053] Preparation Example 4
[0054] The preparation method is the same as that in Preparation Example 1, except for step S1, which is as follows: 4.5 g of bisphenol A epoxy resin (epoxy equivalent 195) and 0.5 g of deca(2,3-glycidoxypropyl) T10-POSS are weighed, dissolved in 10 g of n-hexane, and stirred evenly until completely dissolved to obtain solution A.
[0055] Preparation of reversible thermochromic UV light-curing adhesive
[0056] Example 1
[0057] 60 parts of polyurethane acrylic resin, 15 parts of n-butyl acrylate, 10 parts of 2-ethylhexyl methacrylate, 0.5 parts of 2,2-dimethoxy-phenylacetophenone, 1 part of 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, and 5 parts of fumed silica were added to a stirring kettle. Under the conditions of 25°C and -0.1MPa, the mixture was uniformly dispersed at a speed of 1000r / min for 1h, and then 8.5 parts of the reversible thermochromic microcapsules obtained in Preparation Example 1 were added. The temperature was maintained at 25°C and the pressure was -0.1MPa. The mixture was uniformly dispersed at a speed of 1500r / min for 0.5h. The temperature was maintained at no more than 40°C during the dispersion process. The reversible thermochromic UV light-curing adhesive was obtained by discharging the material.
[0058] Example 2
[0059] 65 parts of epoxy acrylic resin, 10 parts of 2-ethylhexyl acrylate, 10 parts of 2-hydroxypropyl methacrylate, 1 part of 1-hydroxycyclohexyl phenyl ketone, 1 part of ethyl 2,4,6-trimethylbenzoylphenylphosphonate and 5 parts of titanium dioxide were added into a stirring kettle. Under the conditions of 25°C and -0.1MPa, the mixture was uniformly dispersed at a speed of 1000r / min for 1h. Then 7 parts of the reversible thermochromic microcapsules obtained in Preparation Example 2 were added. The temperature was maintained at 25°C and the pressure was -0.1MPa. The mixture was uniformly dispersed at a speed of 1500r / min for 0.5h. The temperature was maintained at no more than 40°C during the dispersion process. The reversible thermochromic UV light-curing adhesive was obtained by discharging the material.
[0060] Example 3
[0061] The raw materials and preparation method are the same as those in Example 1, except that the reversible thermochromic microcapsules obtained in Preparation Example 1 are replaced by the reversible thermochromic microcapsules obtained in Preparation Example 3, and the added amount remains unchanged.
[0062] Example 4
[0063] The raw materials and the preparation method are the same as those in Example 1, except that the reversible thermochromic microcapsules obtained in Preparation Example 1 are replaced by the reversible thermochromic microcapsules obtained in Preparation Example 4, and the added amount remains unchanged.
[0064] Effect Example 1 Performance Testing of Reversible Thermochromic UV Light Curing Adhesive
[0065] ①Adhesive discoloration performance
[0066] The reversible thermochromic UV light-curing adhesive prepared in Examples 1 to 4 was placed in a heating device. As the temperature of the heating device increased, the temperature and color change time when the adhesive changed color were recorded; the heating was stopped, and as the temperature dropped, the color restoration temperature and color restoration time were recorded. The results are shown in the following table:
[0067] Table 1
[0068] Color change temperature / ℃ Color change time / s Color recoloring temperature / ℃ Recolorization time / s Example 1 53 40 45 57 Example 2 74 40 60 60 Example 3 54 41 47 58 Example 4 56 40 47 61
[0069] It can be seen from the data in the above table that the time for the reversible thermochromic UV light-curing adhesive prepared in Example 1 to change from white to bluish purple is 40s, and the time for bluish purple to lighten to white is 57s. The time for the reversible thermochromic UV light-curing adhesive prepared in Example 2 to change from white to orange-red is 40s, and the time for orange-red to lighten to white is 60s. The adhesives prepared in Example 3 and Example 4 are respectively based on Example 1, in which 10% by weight of epoxy POSS is added to the wall material of the thermochromic microcapsule, but compared with Example 1, there is no significant difference in the color change time and color recoloring time of the prepared adhesive. It shows that adding epoxy POSS to the wall material of the thermochromic microcapsule has no effect on the thermal induction efficiency of the microcapsules, and will not cause significant changes in the color change and color recoloring time.
[0070] ②Adhesive shear strength
[0071] According to the national standard GB / T7124-2008, with glass as the substrate, the reversible thermochromic UV light-curing adhesive prepared in Example 1 to Example 4 was coated on the glass substrate with a thickness of 0.2 mm, UV light-cured, and the shear strength of the adhesive was tested. Test results: The shear strength of the adhesive prepared in Example 1 was 16.8362 MPa, the shear strength of the adhesive prepared in Example 2 was 17.1004 MPa, the shear strength of the adhesive prepared in Example 3 was 19.4890 MPa, and the shear strength of the adhesive prepared in Example 4 was 20.0107 MPa. From the test data, it can be seen that when the wall material of the reversible thermochromic microcapsule contains eight (2,3-glycidoxypropyl) T8-POSS or ten (2,3-glycidoxypropyl) T10-POSS, the shear strength of the adhesive prepared by using the microcapsule is better. This is because epoxy POSS is a material between silicon dioxide (SiO2) and silicone resin (R2SiO), and its structure contains Si-O bonds. Adding it to the adhesive can enhance the mechanical shear strength of the adhesive. Among them, ten (2,3-glycidoxypropyl) T10-POSS has a better effect, because the structure of T10 epoxy POSS is denser than that of T8 epoxy POSS, and after co-curing with the adhesive resin, the density of the adhesive will also increase, so that the mechanical properties are improved.
[0072] Based on the above test results, the inventors unexpectedly found that the temperature sensitivity of the final prepared adhesive can be significantly changed by changing the ratio of the sensitizer and the sensitizer raw materials. For example, when the sensitizer is only paraffin wax or microcrystalline wax, the color change time of the adhesive is basically between 40-41s, and the color recoloring time is between 50-62s. When a certain proportion of polymer wax is added to paraffin wax or microcrystalline wax, the color change time will be reduced to 31-35s, and the color recoloring time will be shortened to between 36-42s. The specific results are shown in the following experiments:
[0073] Group A: The wall material of the thermochromic microcapsule is 4.5g bisphenol A epoxy resin (epoxy equivalent 195) and 0.5g ten (2,3-glycidoxypropyl) T10-POSS, the core material is 1g crystal violet lactone, 1g 2,4-diphenylsulfone phenol, the sensitizer is 4g paraffin + 1g polyethylene wax, the preparation method of the microcapsule is the same as that of Preparation Example 1, and the raw materials and method for preparing the reversible thermochromic adhesive are the same as those in Example 1.
[0074] Group B: The wall material of the thermochromic microcapsule is 4.5g bisphenol A epoxy resin (epoxy equivalent 195) and 0.5g ten (2,3-glycidoxypropyl) T10-POSS, the core material is 1g crystal violet lactone, 1g 2,4-diphenylsulfone phenol, the sensitizer is 4g paraffin + 1g polypropylene wax, the preparation method of the microcapsule is the same as that of Preparation Example 1, and the raw materials and method for preparing the reversible thermochromic adhesive are the same as those in Example 1.
[0075] Group C: The wall material of the thermochromic microcapsule is 4.5g bisphenol A epoxy resin (epoxy equivalent 195) and 0.5g ten (2,3-glycidoxypropyl) T10-POSS, the core material is 1g crystal violet lactone, 1g 2,4-diphenylsulfone phenol, the sensitizer is 4g paraffin + 1g polytetrafluoroethylene wax, the preparation method of the microcapsule is the same as that of Preparation Example 1, and the raw materials and method for preparing the reversible thermochromic adhesive are the same as those in Example 1.
[0076] Group D: The wall material of the thermochromic microcapsule is 4.5g bisphenol A epoxy resin (epoxy equivalent 195) and 0.5g ten (2,3-glycidoxypropyl) T10-POSS, the core material is 1g crystal violet lactone, 1g 2,4-diphenylsulfone phenol, the sensitizer is 4.5g paraffin + 0.5g polytetrafluoroethylene wax, the preparation method of the microcapsule is the same as that of Preparation Example 1, and the raw materials and method for preparing the reversible thermochromic adhesive are the same as those in Example 1.
[0077] Group E: The wall material of the thermochromic microcapsule is 4.5g bisphenol A epoxy resin (epoxy equivalent 195) and 0.5g ten (2,3-glycidoxypropyl) T10-POSS, the core material is 1g crystal violet lactone, 1g 2,4-diphenylsulfone phenol, the sensitizer is 5g maleated wax (grafting rate 2%), the preparation method of the microcapsule is the same as that of Preparation Example 1, and the raw materials and method for preparing the reversible thermochromic adhesive are the same as those in Example 1.
[0078] Group F: The wall material of the thermochromic microcapsule is 4.5g bisphenol A epoxy resin (epoxy equivalent 195) and 0.5g ten (2,3-glycidoxypropyl) T10-POSS, the core material is 1g crystal violet lactone, 1g 2,4-diphenylsulfone phenol, the sensitizer is 4g maleated wax (grafting rate 2%) + 1g polytetrafluoroethylene wax, the preparation method of the microcapsule is the same as that of Preparation Example 1, and the raw materials and method for preparing the reversible thermochromic adhesive are the same as those in Example 1.
[0079] The reversible thermochromic UV light-curing adhesive prepared by the AF group was placed in a heating device. As the temperature of the heating device increased, the temperature and color change time when the adhesive changed color were recorded; the heating was stopped, and as the temperature dropped, the color restoration temperature and color restoration time were recorded. The results are shown in the following table:
[0080] Table 2
[0081]
[0082]
[0083] From the data in the table above, it can be seen that, as in the data of group AC, when 20% polymer wax by mass is added to the sensitizer paraffin, the color change temperature and the color recoloring temperature are higher than those using paraffin alone, and the color change time and the color recoloring time are shorter than before. The inventor analyzed the reasons and believed that after adding polymer wax to paraffin, the melting point of the mixture will increase, so the color change temperature and the color recoloring temperature are higher than those of paraffin, but the color change time and the color recoloring time are shortened. This is mainly because the mixture contains polymer wax powder with a particle size of 10-50 microns. Polymer wax is more sensitive to temperature. When the temperature rises to the melting point, the color change response is more timely and the color change time is shorter. The color recoloring is also the same principle, which makes the prepared adhesive more sensitive to color change. The inventor conducted the same test on the sensitizer microcrystalline wax, and the results were consistent with those of paraffin.
[0084] And from the data of group AC in the above table, it can be seen that the combination of paraffin wax and polytetrafluoroethylene wax has a better effect, indicating that compared with polyethylene wax and polypropylene wax, polytetrafluoroethylene wax has better temperature sensitivity. At the same time, as shown in the data of group CD, when the mass fraction of polytetrafluoroethylene wax in the sensitizer is 20%, the effect is better than 10%, indicating that the higher the mass fraction of polymer wax in the sensitizer, the better the temperature sensitivity of the sensitizer. However, considering that the purchase cost of polymer wax is relatively high, the most preferred polymer wax of the present invention accounts for less than 20%.
[0085] In the adhesive prepared by group E, the sensitizer of the reversible color-changing microcapsules is modified wax (maleic acid wax). Compared with the group in which the sensitizer is paraffin, the color change time and the color recolorization time did not change, but the color change temperature and the color recolorization temperature increased.
[0086] Group F is a sensitizer with modified wax (maleic acid wax) and 20% polytetrafluoroethylene wax added. The color change temperature and the color recolor temperature are increased, but the color change time and the color recolor time are reduced. This shows that the combination of maleic acid wax and polytetrafluoroethylene wax is the best sensitizer choice.
[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A reversible thermochromic microcapsule, characterized in that: The microcapsule is prepared by coating a core material with a wall material, wherein the wall material is a combination of a bisphenol epoxy resin and an epoxy-based POSS, and the core material is composed of a leuco dye, a developer and a sensitizer; the bisphenol epoxy resin is one or a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydrogenated bisphenol A epoxy resin, and the epoxy equivalent of the epoxy resin is 155-190; the epoxy-based POSS is ten (2,3-glycidoxypropyl) T10-POSS, and the mass ratio of the bisphenol epoxy resin to the epoxy-based POSS is 1:(0.1-0.2).
2. The reversible thermochromic microcapsule according to claim 1, characterized in that: The reversible thermochromic microcapsule comprises the following raw materials in parts by weight: 10-35 parts of wall material, 30-65 parts of wall material solvent, 2-7 parts of leuco dye, 2-7 parts of developer, 2-7 parts of sensitizer, 0.02-0.15 parts of emulsifier, and 2-10 parts of curing agent; The leuco dye is a fluoran with a lactone ring structure, including any one of crystal violet lactone, 4-(dimethyl)-2,3-diethylaminofluoran, 6-(diethylamino)-1,3-dimethylfluoran, 2-(dibenzylamino)-3-(dimethyl)fluoran, 1,3-dimethyl-6-ethylfluoran, 2-(1,3-diethylamino)-3-ethyl-6-dimethylfluoran, and 3-isopentyl-6-phenylamino-7-methylfluoran, or a combination of two or more thereof; the developer includes one of bisphenol A, 2,4-diphenylsulfonephenol, 4,4-dihydroxydiphenylsulfone, 2,2-di(6-hydroxyphenyl)pentane, 4-methoxyphenol, and a small molecule carboxylic acid, or a combination of two or more thereof; the sensitizer is a combination of modified wax and polytetrafluoroethylene wax, or a combination of microcrystalline wax and polytetrafluoroethylene wax, and the mass fraction of the polytetrafluoroethylene wax is 10-20%.
3. A method for preparing the reversible thermochromic microcapsule according to claim 2, comprising the following steps: (1) Weighing the wall material components epoxy resin and epoxy POSS according to their mass fractions, adding the wall material solvent, and stirring to completely dissolve them to obtain solution A; (2) Weighing the leuco dye, developer and sensitizer according to their mass fractions, heating to a temperature above the melting point of the sensitizer, stirring the system evenly, and maintaining the heating temperature to obtain solution B; (3) Mixing solution A and solution B while maintaining the heating temperature, stirring evenly, to obtain solution C; (4) Weighing an emulsifier by mass and dissolving it in water, adding solution C to the emulsifier solution, and dispersing at a high speed of 1500-2000 r / min for 1-2 hours to obtain emulsion D; (5) Weighing a curing agent by mass and dissolving it in water to obtain a solution E, and adding the solution E dropwise to the emulsion D under high-speed shear dispersion at 1500-2000 r / min, keeping the system temperature higher than the melting point of the sensitizer and reacting for 5-6 hours to obtain an emulsion product F; (6) The emulsion product F is filtered, and the obtained solid G is repeatedly washed with a wall material solvent and dried to obtain reversible thermosensitive color-changing microcapsules.
4. A reversible thermochromic UV light-curing adhesive, characterized in that: The UV light-curing adhesive comprises the following raw materials in parts by mass: 50-80 parts of liquid acrylic resin, 20-40 parts of acrylic monomer, 0.5-3 parts of free radical photoinitiator, 5-10 parts of filler, and 5-10 parts of the reversible thermochromic microcapsule according to claim 1.
5. The reversible thermochromic UV light-curing adhesive according to claim 4, characterized in that: The liquid acrylic resin is selected from one or more of silicone modified polyacrylate, polyurethane acrylate, epoxy acrylate; the acrylic monomer is selected from one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxypropyl acrylate; The photoinitiator is selected from methyl benzoylformate, 2,2-dimethoxy-phenylacetophenone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, and 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone, or a combination of two or more thereof.
6. A method for preparing a reversible thermochromic UV light-curing adhesive as described in claim 4, wherein the method is as follows: 50-80 parts of liquid acrylic resin, 20-40 parts of acrylic monomer, 0.5-3 parts of free radical photoinitiator, and 5-10 parts of filler are added into a stirring kettle, and uniformly dispersed at a speed of 500-1000r / min for 1-2 hours at room temperature and -0.1MPa, and then 5-10 parts of reversible thermochromic microcapsules are added, and then uniformly dispersed at a speed of 1000-1500r / min for 0.5-1 hour, and the temperature is kept not higher than 40°C during the dispersion process, and the reversible thermochromic UV light-curing adhesive is obtained by discharging the material.