Low-weight rare earth magnet and manufacturing method

By forming a low-heavy rare earth diffusion source film with specific grain boundary distribution on the NdFeB magnet, the problems of high cost and insufficient coercivity of traditional NdFeB magnets are solved, and the coercivity improvement under low-heavy rare earth conditions is achieved and cost reduction.

CN113871122BActive Publication Date: 2024-11-15YANTAI DONGXING MAGNETIC MATERIALS INC
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202111121038.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-24
Publication Date
2024-11-15
Estimated Expiration
2041-09-24

AI Technical Summary

Technical Problem

Traditional neodymium iron boron magnets have high cost problems in improving coercivity, mainly due to their dependence on heavy rare earths, and the existing technology is difficult to maintain performance while reducing the heavy rare earth content, especially the coercive force enhancement is limited.

Method used

By forming a thin film of low-heavy rare earth diffusion source with a specific grain boundary distribution on the neodymium iron boron magnet and performing diffusion and aging treatment, a neodymium iron boron magnet with a specific grain boundary phase structure is formed to reduce the heavy rare earth content and increase coercive force.

Benefits of technology

The coercive force of magnets is significantly improved under the low content of heavy rare earths, while greatly reducing the production cost of magnets. The process is simple and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113871122B_ABST
    Figure CN113871122B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of neodymium iron boron magnets, and in particular to a low-heavy rare earth magnet and a manufacturing method thereof. The low-heavy rare earth magnet is prepared from a neodymium iron boron magnet main alloy and a low-heavy rare earth diffusion source, wherein the chemical formula of the low-heavy rare earth diffusion source is R x H y M 1‑x‑y , wherein R refers to at least one of Nd, Pr, Ce, La, Ho, and Gd, H refers to at least one of Tb and Dy, and M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and the structure distribution of the low-heavy rare earth diffusion source is a uniform distribution of RH phase and RHM phase inlaid. The low-heavy rare earth diffusion source is coated on the surface of the main alloy of the NdFeB magnet, and diffusion and tempering treatment are performed to obtain a low-heavy rare earth magnet, and the magnet grain boundary structure includes a main phase, an R shell, a transition metal shell, and a triangular region. The benefit of the present invention is that the coercive force is greatly improved by regulating the magnet composition and the low-heavy diffusion source structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of neodymium iron boron magnets, and in particular to a low-weight rare earth magnet and a manufacturing method thereof. Background Art

[0002] NdFeB sintered permanent magnets are widely used in high-tech fields such as electronic information, medical equipment, new energy vehicles, household appliances, robots, etc. In the past few decades, NdFeB permanent magnets have developed rapidly, and the residual magnetic properties have basically reached the theoretical limit. However, the coercive force is still far from the theoretical value. Therefore, improving the coercive force of magnets is a major research hotspot.

[0003] Since the traditional manufacturing process consumes a large amount of Tb or Dy heavy rare earth metals, the cost increase is increasing. The heavy rare earth content can be greatly reduced through grain boundary diffusion technology, but with the current soaring price of heavy rare earth Tb, the cost is still very high. Therefore, it is still important to continue to reduce the content of heavy rare earths. Due to the diffusion mechanism, that is, the diffusion hardening of the Nd2Fe14B main phase containing heavy rare earth elements, a large number of core-shell structures are formed to increase the coercive force. Therefore, the research on magnets and diffusion sources has become the focus.

[0004] The most significant effect of improving coercivity is through the diffusion of heavy rare earths, but the abundance of heavy rare earths is low and the price is expensive. Therefore, more and more researchers are preparing heavy rare earth alloys as diffusion sources for diffusion to achieve the same performance of NdFeB magnets. There are many applications for patents related to special grain boundaries. For example, patent CN 106024253 A coats the surface of the magnet with heavy rare earths Tb, Dy or Ho to make the magnet contain M2 boride phase, with a core-shell structure of HR enriched layer and (R,HR)-Fe(Co)-M1 phase covering the main phase; patent CN 108305772 A mainly uses the diffusion source as hydride powder of R1-R2-M type alloy. The melting point of R1-R2-M type alloy is 400-800℃, and it is not combined with a specifically designed magnet to form a magnet with a specific phase structure. After diffusion, the Hcj performance increases significantly. Patent CN 111524674 A proposes that the magnet contains a grain boundary epitaxial layer, that is, a two-grain grain boundary phase R X Ho y Cu Z The X1-characterized magnet has greatly increased performance after diffusion. The above technologies use magnets to form specific phases or use low-cost diffusion sources to reduce the production cost of magnets, but lack a NdFeB magnet and manufacturing method that combines a magnet with a specific manufacturing method and a diffusion source with a specific grain boundary structure to improve performance and greatly reduce the content of heavy rare earth. Summary of the invention

[0005] The present invention proposes a low-heavy rare earth magnet and a manufacturing method. A diffusion source film with a specific grain boundary distribution is formed on a NdFeB magnet of a specific composition, and a NdFeB magnet with a specific grain boundary phase structure distribution is formed through diffusion and aging treatment. The coercive force of the magnet can be greatly increased and the production cost of the magnet can be greatly reduced under the condition of low heavy rare earth content.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] A low-heavy rare earth magnet is prepared from a neodymium iron boron magnet main alloy and a diffusion source, wherein the diffusion source is a low-heavy rare earth diffusion source, and the chemical formula of the low-heavy rare earth diffusion source is R x H y M 1-x-y , wherein R refers to at least one of Nd, Pr, Ce, La, Ho, and Gd, H refers to at least one of Tb and Dy, and M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn. x and y are weight percentages, wherein 10% < x ≤ 50%, and 40% < y ≤ 70%. The structural distribution of the low-heavy rare earth diffusion source is a uniform distribution of RH phase and RHM phase inlaid.

[0008] The low-heavy rare earth diffusion source is coated on the surface of the main alloy of the NdFeB magnet, and diffusion and tempering treatment are performed to obtain the low-heavy rare earth magnet, wherein the grain boundary structure of the low-heavy rare earth magnet includes a main phase, an R shell, a transition metal shell and a triangular region, wherein the R shell, R refers to at least one of Nd, Pr, Ce, La, Ho and Gd, and the transition metal shell, the transition metal refers to at least one of Cu, Al and Ga, and the triangular region has the following characteristics:

[0009] Sum or triangle area point scan 1: Nd a Fe b R c M d , wherein R refers to at least one of Pr, Ce, La, Ho, and Gd, M refers to at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and a, b, c, and d are weight percentages, wherein 30% ≤ a ≤ 70%, 5% ≤ b ≤ 40%, 5% ≤ c ≤ 35%, and 0% ≤ d ≤ 15%;

[0010] Sum or triangle area point scan 2: Nd e Fe f R g H h K i M j, wherein R refers to at least one of Pr, Ce, and La, H refers to one of Dy and Tb, K refers to one of Ho and Gd, M refers to at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and e, f, g, h, i, and j are weight percentages, wherein 25% ≤ e ≤ 65%, 5% ≤ f ≤ 35%, 5% ≤ g ≤ 30%, 5% ≤ h ≤ 30%, 5% ≤ i ≤ 10%, and 0% ≤ j ≤ 10%;

[0011] Sum or triangle area point scan 3: Nd k Fe l R m D n M o , wherein R refers to at least one of Pr, Ce, La, Ho, and Gd, D refers to at least one of Al, Cu, and Ga, M refers to at least one of Ti, Co, Mg, Zn, and Sn, and k, l, m, n, and o are weight percentages, wherein 30% ≤ k ≤ 70%, 5% ≤ l ≤ 35%, 5% ≤ m ≤ 35%, 5% ≤ n ≤ 25%, and 0% ≤ o ≤ 10%.

[0012] Preferably, the NdFeB main alloy is prepared by mixing NdFeB alloy raw material, low melting point powder and other additives, the NdFeB alloy raw material contains rare earth R with a weight percentage of 28%≤R≤30%, R refers to a mixture of at least two of Nd, Pr, Ce, La, Tb, and Dy, B with a weight percentage of 0.8%≤B≤1.2%, Gd with a weight percentage of 0%≤Gd≤5%, Ho with a weight percentage of 0%≤Ho≤5%, and M with a percentage of 0%≤M≤3%, wherein M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe, the low melting point powder contains NdCu, NdAl, and CeGa, and the weight percentage of each component is 0%≤NdCu≤3%, 0%≤NdAl≤3%, and 0%≤NdGa≤3%.

[0013] Preferably, the low-heavy rare earth magnet has a thickness of 0.3-6 mm.

[0014] The present invention also proposes a method for manufacturing the above-mentioned low-weight rare earth magnet, comprising the following steps:

[0015] S1, smelting and rapidly solidifying the prepared NdFeB alloy raw material to obtain NdFeB alloy flakes, and mechanically crushing the NdFeB alloy flakes into 150-400 μm scaly NdFeB alloy flakes;

[0016] S2, mechanically mixing and stirring the flaky NdFeB alloy flakes, low melting point powder, and lubricant, and then placing them in a hydrogen treatment furnace for hydrogen absorption and dehydrogenation treatment, and preparing NdFeB powder by air jet milling;

[0017] S3, pressing the above powder into a shape, and sintering to obtain the required NdFeB magnet main body alloy.

[0018] S4, machining the sintered NdFeB magnet main alloy into a desired shape, and then forming a thin film of a low-heavy rare earth diffusion source on a surface of the NdFeB magnet main alloy perpendicular or parallel to the C-axis direction by coating;

[0019] S5. Perform diffusion, aging and tempering treatments to obtain low-heavy rare earth magnets.

[0020] Preferably, the NdFeB alloy raw material composition described in step S1 contains rare earth R in a weight percentage of 28%≤R≤30%, where R refers to a mixture of at least two of Nd, Pr, Ce, La, Tb, and Dy, the weight percentage of B is 0.8%≤B≤1.2%, the weight percentage of Gd is 0%≤Gd≤5%, the weight percentage of Ho is 0%≤Ho≤5%, and the percentage of M is 0%≤M≤3%, where M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe. The low-melting-point powder contains NdCu, NdAl, and CeGa, and the weight percentage of each component is 0%≤NdCu≤3%, 0%≤NdAl≤3%, and 0%≤NdGa≤3%.

[0021] Preferably, the low-heavy rare earth diffusion source is prepared by atomization powder making, amorphous belt spinning powder making or ingot casting.

[0022] Preferably, the low-heavy rare earth diffusion source needs to undergo hydrogen absorption and dehydrogenation treatments, with the dehydrogenation temperature being 400-600°C.

[0023] Preferably, the particle size of the low melting point powder in step S2 is 200nm-4μm, and the particle size of the NdFeB powder is 3-5μm.

[0024] Preferably, the sintering temperature of the sintering process in step S3 is 980-1060° C., and the sintering time is 6-15 hours.

[0025] Preferably, in step S5, the diffusion temperature is 850-930°C, the diffusion time is 6-30h, the aging temperature is 420-680°C, the heating rate is 1-5°C / min, the cooling rate is 5-20°C / min, and the aging time is 3-10h.

[0026] The beneficial effects of adopting the above further scheme are:

[0027] 1. By designing the grain boundary as a low melting point magnet and forming a diffusion source with a special grain boundary structure on the magnet, diffusion and aging treatment are performed to obtain a neodymium iron boron magnet with a low heavy rare earth content and a specific grain boundary structure. By regulating the magnet composition and diffusion source structure, the coercive force is greatly improved.

[0028] 2. The low-heavy rare earth magnet of the present invention contains NdCu, NdAl and NdGa with low melting point, which is beneficial to increase the diffusion coefficient of the magnet grain boundary, thereby improving the diffusion efficiency of the diffusion source.

[0029] 4. The crystal phase structure distribution of the diffusion source is a mosaic distribution of RH phase and RHM phase, which enables the low melting point phase and the heavy rare earth phase to quickly enter the magnet at the same time. While greatly improving the diffusion coefficient, it can well form a shell layer with magnetic isolation effect, and well achieve the effect of improving coercive force.

[0030] 5. The diffused low-heavy rare earth magnet has a characteristic phase, the Fe mass content of the characteristic phase is less than 30%, it has non-ferromagnetic properties, and can have a good magnetic isolation effect;

[0031] 6. The present invention is capable of significantly reducing the heavy rare earth content in magnets, can significantly reduce the cost of magnets, has a simple process, and can achieve mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments of the present invention. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 : Scanning electron microscope photograph of the magnet microstructure after diffusion of heavy rare earth alloy. DETAILED DESCRIPTION

[0034] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0035] It should also be noted that the term “and or” refers to inclusion rather than exclusivity, so that it includes not only the listed elements but also some elements that are necessary for the elements, methods, processes, articles and equipment that are not explicitly listed.

[0036] The present invention is further described in detail below in conjunction with the accompanying drawings.

[0037] A low-heavy rare earth magnet is prepared from a neodymium iron boron magnet main alloy and a diffusion source, wherein the diffusion source is a low-heavy rare earth diffusion source, and the chemical formula of the low-heavy rare earth diffusion source is Rx H y M 1-x-y , wherein R refers to at least one of Nd, Pr, Ce, La, Ho, and Gd, H refers to at least one of Tb and Dy, and M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn. x and y are weight percentages, wherein 10% < x ≤ 50%, 40% < y ≤ 70%, and the structural distribution of the low-heavy rare earth diffusion source is a uniform distribution of RH phase and RHM phase inlaid.

[0038] The raw material composition of the NdFeB alloy contains rare earth R in a weight percentage of 28%≤R≤30%, where R refers to a mixture of at least two of Nd, Pr, Ce, La, Tb, and Dy, B in a weight percentage of 0.8%≤B≤1.2%, Gd in a weight percentage of 0%≤Gd≤5%, Ho in a weight percentage of 0%≤Ho≤5%, and M in a weight percentage of 0%≤M≤3%, where M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe. The low-melting-point powder contains NdCu in a weight percentage of 0-3%, NdAl in a weight percentage of 0-3%, and NdGa in a weight percentage of 0-3%.

[0039] With reference to the above-mentioned composition ratio, the embodiments are as follows:

[0040] 1. Composition of NdFeB magnet materials:

[0041] The component numbers are divided into 1-22, wherein the components with different composition ratios are formed by mixing low melting point alloy powders of NdCu, NdAl, or NdGa in different proportions, and the unit is weight percentage, i.e., wt%. As shown in Table 1 below:

[0042] Table 1

[0043]

[0044] The blank means that the element is not contained. The composition is designed into the above 22 kinds of formulations. The preparation method of the NdFeB magnet material numbered 1-22 is as follows:

[0045] (1) Smelting the components except for adding low melting point powder to prepare NdFeB magnet quick solidification flakes, and then mechanically crushing them into scaly NdFeB magnet flakes with a particle size range of 150-400 μm;

[0046] (2) mixing NdCu, NdAl, and NdGa low melting point powders with a particle size range of 200 nm to 4 μm in corresponding alloy proportions and adding the mixture to the flaky NdFeB magnet sheets;

[0047] (3) mixing the flaky NdFeB magnet flakes, low melting point powder, and lubricant, mechanically stirring, and then placing in a hydrogen treatment furnace for hydrogen absorption and dehydrogenation treatment, wherein the dehydrogenation temperature is 400-600° C., and jet milling to obtain alloy powder, preferably jet milling to obtain a particle size of 3-5 μm with a D50;

[0048] (4) The alloy powder after air flow milling is oriented and molded and cold isostatically pressed to form a blank.

[0049] (5) The blank is subjected to vacuum sintering, argon gas is introduced for rapid cooling, and then primary tempering and secondary aging are performed, and the magnet performance is tested by digging out the column. The specific process is shown in Table 2 below;

[0050] Table 2

[0051]

[0052] (6) The blank is machined and cut into samples of corresponding sizes. The diffusion source slurry is coated on both sides of the sample perpendicular to the C axis. The weight gain of metal Dy is 1.0%, the Dy content in the Dy alloy is 1.0%, and the weight gain is weight percentage, i.e., wt%.

[0053] The main alloy of NdFeB magnet is subjected to the optimization process test to achieve the best performance and then the diffusion test is carried out. The coercive force increase of Dy alloy after diffusion can reach 8-9.5kOe. The production cost of the magnet is greatly reduced by using low Dy content.

[0054] The diffused Dy alloy is taken as an example, and the diffused metal Dy is taken as a comparative example.

[0055] The embodiment is the diffusion of Dy alloy and its specific process, as shown in Table 3 below:

[0056] Table 3

[0057]

[0058] Comparative Example Diffusion Metal Dy and Its Specific Process, as Shown in Table 4

[0059] Table 4

[0060]

[0061] Based on the above data, NdCu, NdAl, or NdGa low-melting-point powders are first added to the grain boundaries in the spinning strip to make NdFeB magnets with low-melting-point grain boundary channels suitable for magnet diffusion, which is beneficial to the diffusion, especially the diffusion of heavy rare earth dysprosium alloy diffusion sources. After diffusion, △Hcj>7.5kOe, and the coercive force is significantly increased.

[0062] The embodiments and comparative examples are specifically analyzed as follows:

[0063] In Example 1, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.2 kGS, and Hcj increased by 10.21 kOe. In Comparative Example 1, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.19 kGS, and Hcj increased by 8.21 kOe. The coercive force increased significantly, but the Hcj of diffused PrDyCu increased more significantly, and the advantage was more obvious.

[0064] In Example 2, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.24kGS, and Hcj increased by 8.78kOe. In Comparative Example 2, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.23kGS, and Hcj increased by 6.78kOe. The coercive force increased significantly, but the Hcj of diffused PrDyCu increased more significantly, and the advantage was more obvious.

[0065] In Example 3, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.22kGS, and Hcj increased by 7.58kOe. In Comparative Example 3, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.20kGS, and Hcj increased by 5.08kOe. The coercive force increased significantly, but the Hcj of diffused PrDyCu increased more significantly, and the advantage was more obvious.

[0066] In Example 4, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.24kGS, and Hcj increased by 7.52kOe. In Comparative Example 4, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.23kGS, and Hcj increased by 5.02kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0067] In Example 5, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing NdDyCu, Br decreased by 0.25 kGS, and Hcj increased by 9.51 kOe. In Comparative Example 5, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.23 kGS, and Hcj increased by 7.51 kOe. The coercive force increased significantly, but the increase in Hcj of diffused NdDyCu was greater, and the advantage was more obvious.

[0068] In Example 6, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing NdDyCu, Br decreased by 0.23kGS, and Hcj increased by 8.31kOe. In Comparative Example 6, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.21kGS, and Hcj increased by 6.81kOe. The coercive force increased significantly, but the increase in Hcj of diffused NdDyCu was greater, and the advantage was more obvious.

[0069] In Example 7, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing NdDyCu, Br decreased by 0.22kGS, and Hcj increased by 8.82kOe. In Comparative Example 7, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.21kGS, and Hcj increased by 7.32kOe. The coercive force increased significantly, but the increase in Hcj of diffused NdDyCu was greater, and the advantage was more obvious.

[0070] In Example 8, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.21 kGS, and Hcj increased by 9.35 kOe. In Comparative Example 8, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.19 kGS, and Hcj increased by 7.85 kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0071] In Example 9, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.24kGS, and Hcj increased by 9.35kOe. In Comparative Example 9, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.22kGS, and Hcj increased by 7.35kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0072] In Example 10, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.22 kGS, and Hcj increased by 9.88 kOe. In Comparative Example 10, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.21 kGS, and Hcj increased by 7.88 kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0073] In Example 11, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.21 kGS, and Hcj increased by 7.74 kOe. In Comparative Example 11, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.2 kGS, and Hcj increased by 4.74 kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0074] In Example 12, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.22kGS, and Hcj increased by 7.6kOe. In Comparative Example 12, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.2kGS, and Hcj increased by 5.1kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0075] In Example 13, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCuGa, Br decreased by 0.25kGS, and Hcj increased by 7.6kOe. In Comparative Example 13, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.23kGS, and Hcj increased by 5.6kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCuGa was greater, and the advantage was more obvious.

[0076] In Example 14, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCuGa, Br decreased by 0.22kGS, and Hcj increased by 8.25kOe. In Comparative Example 14, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.21kGS, and Hcj increased by 6.75kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCuGa was greater, and the advantage was more obvious.

[0077] In Example 15, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCuGa, Br decreased by 0.25kGS, and Hcj increased by 8.98kOe. In Comparative Example 15, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.23kGS, and Hcj increased by 7.48kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCuGa was greater, and the advantage was more obvious.

[0078] In Example 16, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCuAl, Br decreased by 0.23kGS, and Hcj increased by 8.94kOe. In Comparative Example 16, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.22kGS, and Hcj increased by 7.44kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCuAl was greater, and the advantage was more obvious.

[0079] In Example 17, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCuAl, Br decreased by 0.2 kGS, and Hcj increased by 8.07 kOe. In Comparative Example 17, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.2 kGS, and Hcj increased by 6.57 kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCuAl was greater, and the advantage was more obvious.

[0080] In Example 18, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCuAl, Br decreased by 0.26 kGS, and Hcj increased by 8.6 kOe. In Comparative Example 18, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.25 kGS, and Hcj increased by 7.1 kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCuAl was greater, and the advantage was more obvious.

[0081] In Example 19, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.25kGS, and Hcj increased by 8.5kOe. In Comparative Example 19, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.24kGS, and Hcj increased by 6kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0082] In Example 20, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.2 kGS, and Hcj increased by 7.5 kOe. In Comparative Example 20, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.2 kGS, and Hcj increased by 6 kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0083] In Example 21, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.25kGS, and Hcj increased by 9.5kOe. In Comparative Example 21, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.24kGS, and Hcj increased by 7kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0084] In Example 22, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, after diffusing PrDyCu, Br decreased by 0.2 kGS, and Hcj increased by 7.5 kOe. In Comparative Example 22, compared with before diffusion, after diffusing metal Dy, Br decreased by 0.2 kGS, and Hcj increased by 5 kOe. The coercive force increased significantly, but the increase in Hcj of diffused PrDyCu was greater, and the advantage was more obvious.

[0085] The performance of the above heavy rare earth alloy diffusion source after diffusion is significantly better than that of pure heavy rare earth after diffusion. Therefore, we will measure the microstructure of the magnet after diffusion of heavy rare earth alloy. The ZISS electron microscope is mainly used for SEM testing, and the Oxford EDS is used for the composition of sample magnet elements. Definition: rare earth shell, i.e. R shell, refers to the continuity around the grain exceeding 60%, and transition metal shell refers to the continuity around the grain exceeding 40%. In addition, points a, b, and c are sampling points at different positions, but in the small triangle area with a size of less than 1μm, it is characterized by a 6:14 phase-type Cu-rich, that is, the chemical formula of the point scan is weight percentage, i.e. wt%:Fe 30-51 (NdPr )45-60 Cu 2-15 Ga 0-5 Co 0-5 or Fe 30-51 (NdPr )45-60 Dy 2-15 Cu 2-15 Ga 0-5 Co 0-5 The other three points are SEM, 3 sampling points, see Figure 1 The R shell and transition metal shell are formed by diffusing the diffusion source, and the statistical analysis of the three points a, b, and c is as follows (the subscript of the chemical formula is weight percentage, i.e., wt%):

[0086] Example 1: After the magnet is diffused with PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 50-70 Fe 10-30 Pr 10-20 Cu 0-5 Triangle area point scan 2: Nd 50-55 Fe10-30 Pr 5-15 Dy 5-15 Cu 0-5 Triangle area point scan 3: Nd 50-70 Fe 10-35 Pr 10-20 Cu 10-20 Co 0-5

[0087] Example 2: After the magnet is diffused with PrDyCu, it has a rare earth shell of Pr, Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 50-65 Fe 10-30 Pr 10-25 Cu 0-5 Ga 0-5 Al 0-3 Triangle area point scan 2: Nd 50-55 Fe 10-30 Pr 5-15 Dy 5-15 Cu 0-5 Triangle area point scan 3: Nd 50-70 Fe 10-35 Pr 10-20 Cu 10-15 Co 0-5

[0088] Example 3: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Al, forming a triangular area point scan 1: Nd 45-65 Fe 10-35 Pr 10-25 Cu 0-5 Ga 0-5 Al 3-5 Triangle area point scan 2: Nd 45-55 Fe 10- 30 Pr 5-20 Dy 5-10 Cu 0-5 Triangle area point scan 3: Nd 50-65 Fe 10-35 Pr 10-20 Cu 10-15 Co 0-5 Al 0-5

[0089] Example 4: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Al, forming a triangular area point scan 1: Nd 45-60 Fe 10-35 Pr 10-20 Cu 3-8 Ga 0-5 Al3-5 Triangle area point scan 2: Nd 45-55 Fe 10- 30 Pr 5-20 Dy 5-10 Cu 2-5 Al 2-10 Triangle area point scan 3: Nd 45-65 Fe 10-30 Pr 10-20 Cu 10-25 Co 0-5 Al 0-5

[0090] Example 5: After the magnet is diffused into NdDyCu, the magnet has Nd, Dy rare earth shell and transition metal shell Cu, forming a triangle area point scan 1: Nd 50-65 Pr 10-15 Fe 10-30 Cu 2-6 Go 0-5 Triangle area point scan 2: Nd 45-60 Pr 5-15 Dy 5-15 Fe 5-30 Triangle area point scan 3: Nd 45-60 Pr 10-20 Fe 5-30 Cu 10-20 Co 0-5

[0091] Example 6: After the magnet is diffused into NdDyCu, the magnet has Nd, Dy rare earth shell and transition metal shell Cu, forming a triangle area point scan 1: Nd 45-60 Pr 10-20 Fe 10-30 Cu 2-5 Ga 0-5 Triangle area point scan 2: Nd 45-60 Pr 5-12 Dy 5-20 Fe 5-25 Triangle area point scan 3: Nd 50-60 Pr 10-15 Fe 5-25 Cu 5-25 Co 0-5

[0092] Example 7: After the magnet is diffused into NdDyCu, the magnet has a rare earth shell of Nd and Dy and a transition metal shell of Cu and Al, forming a triangular area point scan 1: Nd 50-65 Pr 10-15 Fe 10-40 Cu 5-10 Al 0-5 Triangle area point scan 2: Nd50-60 Pr 5-15 Dy 5- 25 Fe 5-30 Al 2-10 Triangle area point scan 3: Nd 50-60 Pr 10-15 Fe 5-25 Cu 5-15 Co 0-5 Al 0-5

[0093] Example 8: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 40-65 Pr 20-35 Fe 10-25 Cu 5-10 Triangle area point scan 2: Nd 25-40 Pr 10-25 Dy 15-20 Fe 10- 30 Co 0-5 Cu 0-5 Triangle area point scan 3: Nd 35-45 Pr 15-35 Fe 5-25 Cu 10-25 Co 0-5

[0094] Example 9: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 40-60 Pr 20-30 Fe 10-30 Cu 3-8 Triangle area point scan 2: Nd 35-45 Pr 10-25 Dy 5-25 Fe 10- 30 Co 0-5 Cu 0-5 Triangle area point scan 3: Nd 35-50 Pr 15-30 Fe 5-25 Cu 5-20 Co 0-5

[0095] Example 10: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 40-60 Pr 20-35 Fe 10-30 Cu 0-5 Triangle area point scan 2: Nd25-40 Pr 10-25 Dy 5-15 Fe 10- 30 Co 0-5 Cu 0-5 Triangle area point scan 3: Nd 35-45 Pr 15-35 Fe 5-30 Cu 5-20 Co 0-5

[0096] Example 11: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 50-65 Fe 10-25 Pr 10-20 Cu 0-5 Ga 0-5 Al 0-5 Triangle area point scan 2: Nd 45-55 Fe 10- 30 Pr 5-20 Dy 5-20 Cu 0-5 Triangle area point scan 3: Nd 45-70 Fe 10-30 Pr 10-25 Cu 10-25 Co 0-5 Ga 0-5

[0097] Example 12: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 50-65 Fe 10-30 Pr 10-25 Cu 0-5 Ga 2-7 Al 3-7 Triangle area point scan 2: Nd 45-55 Fe 10- 30 Pr 5-20 Dy 5-10 Cu 0-5 Ga 0-5 Triangle area point scan 3: Nd 50-65 Fe 10-35 Pr 5-20 Cu 10-20 Co 0-5 Al 0-5

[0098] Example 13: After the magnet is diffused into PrDyCuGa, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Ga, forming a triangular area point scan 1: Nd 45-55 Pr 20-25 Fe 15-30 Ga 2-10 Cu 3-5 Triangle area point scan 2: Nd 30-45 Pr 25- 30 Dy 5-20 Fe 5-25 Cu 0-5 Triangle area point scan 3: Nd 35-45 Pr 20-35 Fe 10-35 Cu 5-15 Ga 5-10 Co 2-5

[0099] Example 14: After the magnet is diffused into PrDyCuGa, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Ga, forming a triangular region point scanning phase 1: Nd 40-55 Pr 20-30 Fe 15-30 Ga 2-10 Cu 3-5 Triangle area point scan 2: Nd 30- 40 Pr 25-30 Dy 5-15 Fe 5-25 Cu 0-5 Triangle area point scan 3: Nd 30-50 Pr 25-30 Fe 10-30 Cu 5-10 Ga 5-10 Co 2-5

[0100] Example 15: After the magnet is diffused into PrDyCuGa, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Ga, forming a triangular area point scan 1: Nd 40-55 Pr 20-30 Fe 15-25 Ga 5-10 Cu 3-10 Triangle area point scan 2: Nd 30-40 Pr 15- 30 Dy 5-20 Fe 5-25 Cu 0-5 Triangle area point scan 3: Nd 30-45 Pr 25-35 Fe 10-30 Cu5-10 Ga 5-10 Co 2-5

[0101] Example 16: After the magnet is diffused into PrDyCuAl, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Al, forming a triangular area point scan 1: Nd 45-65 Fe 10-35 Pr 5-15 Cu 5-15 Al 5-10 Triangle area point scan 2: Nd 45-65 Fe 5- 30 Pr 5-20 Dy 5-10 Cu 5-10 Al 2-10 Triangle area point scan 3: Nd 50-65 Fe 10-20 Pr 10-15 Cu 10-25 Al 0-5

[0102] Example 17: After the magnet is diffused into PrDyCuAl, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Al, forming a triangular area point scan 1: Nd 45-55 Fe 10-30 Pr 5-20 Cu 5-10 Al 2-5 Triangle area point scan 2: Nd 45-60 Fe 5- 25 Pr 5-25 Dy 5-15 Cu 5-10 Al 3-5 Triangle area point scan 3: Nd 45-60 Fe 10-20 Pr 10-20 Cu 10-20 Ga 0-5 Al 0-5

[0103] Example 18: After the magnet is diffused into PrDyCuAl, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu and Al, forming a triangular area point scan 1: Nd 50-65 Fe 10-30 Pr 5-20 Cu 5-10 Al 2-5 Triangle area point scan 2: Nd 45-65 Fe 5- 30 Pr 5-20 Dy 5-15Cu 5-10 Al 5-10 Triangle area point scan 3: Nd 45-60 Fe 10-25 Pr 10-20 Cu 10-20 Ga 0-5 Al 0-5

[0104] Example 19: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 45-55 Fe 5-30 Pr 20-35 Cu 0-5 Triangle area point scan 2: Nd 45-55 Fe 5-10 Pr 10-30 Dy 5- 20 Cu 0-5 Triangle area point scan 3: Nd 35-55 Fe 5-30 Pr 10-35 Cu 5-10 Ga 0-5 Co 0-5

[0105] Example 20: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 35-50 Fe 15-40 Pr 15-30 Cu 0-10 Ga 0-3 Al 0-3 Triangle area point scan 2: Nd 40-60 Fe 3- 30 Pr 10-20 Dy 5-25 Triangle area point scan 3: Nd 40-55 Fe 5-35 Pr 15-30 Cu 5-25 Ga 0-5 Co 0-5

[0106] Example 21: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 30-45 Fe 10-30 Pr 20-25 Cu 5-10 Ga 0-5 Co 0-5 Ti 0-5Triangle area point scan 2: Nd 30- 40 Fe 5-25 Pr 10-15 Dy 10-30 Ho 5-10 Triangle area point scan 3: Nd 35-45 Fe 5-30 Pr 15-30 Cu 5-25 Ga 0-3 Co 0-5

[0107] Example 22: After the magnet is diffused into PrDyCu, the magnet has a rare earth shell of Pr and Dy and a transition metal shell of Cu, forming a triangular area point scan 1: Nd 30-40 Fe 20-30 Pr 20-30 Cu 0-10 Ga 0-5 Triangle area point scan 2: Nd 45-55 Fe 10-20 Pr 20- 30 Dy 5-20 Triangle area point scan 3: Nd 40-55 Fe 10-25 Pr 15-35 Cu 5-20 Ga 0-10 Co 0-5

[0108] By referring to the above embodiments, experiments were conducted with other raw materials and conditions listed in this specification, and the low-weight rare earth magnets of the present invention were also prepared.

[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A low-heavy rare earth magnet, prepared from a neodymium iron boron magnet main alloy and a diffusion source, characterized in that: The diffusion source is a low-heavy rare earth diffusion source, and the chemical formula of the low-heavy rare earth diffusion source is R x H y M 1-x-y , wherein R refers to at least one of Nd, Pr, Ce, La, Ho, and Gd, H refers to at least one of Tb and Dy, and M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and x and y are weight percentages, wherein 10% < x ≤ 50%, and 40% < y ≤ 70%, and the structure distribution of the low-heavy rare earth diffusion source is a uniform distribution of RH phase and RHM phase inlaid; The low-heavy rare earth diffusion source is coated on the surface of the main alloy of the NdFeB magnet, and diffusion and tempering treatment are performed to obtain the low-heavy rare earth magnet, wherein the grain boundary structure of the low-heavy rare earth magnet includes a main phase, an R shell, a transition metal shell and a triangular region, wherein the R shell, R refers to at least one of Nd, Pr, Ce, La, Ho and Gd, and the transition metal shell, the transition metal refers to at least one of Cu, Al and Ga, and the triangular region has the following characteristics: Sum or triangle area point scan 1: Nd a Fe b R c M d , wherein R refers to at least one of Pr, Ce, La, Ho, and Gd, M refers to at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and a, b, c, and d are weight percentages, wherein 30%≤a≤70%, 5%≤b≤40%, 5%≤c≤35%, and 0%≤d≤15%; Sum or triangle area point scan 2: Nd e Fe f R g H h K i M j , wherein R refers to at least one of Pr, Ce, and La, H refers to one of Dy and Tb, K refers to one of Ho and Gd, M refers to at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and e, f, g, h, i, and j are weight percentages, wherein 25%≤e≤65%, 5%≤f≤35%, 5%≤g≤30%, 5%≤h≤30%, 5%≤i≤10%, and 0%≤j≤10%; Sum or triangle area point scan 3: Nd k Fe l R m D n M o , wherein R refers to at least one of Pr, Ce, La, Ho, and Gd, D refers to at least one of Al, Cu, and Ga, M refers to at least one of Ti, Co, Mg, Zn, and Sn, and k, l, m, n, and o are weight percentages, wherein 30% ≤ k ≤ 70%, 5% ≤ l ≤ 35%, 5% ≤ m ≤ 35%, 5% ≤ n ≤ 25%, and 0% ≤ o ≤ 10%; The NdFeB main alloy is prepared by mixing NdFeB alloy raw materials, low melting point powders and other additives. The NdFeB alloy raw materials contain rare earth R with a weight percentage of 28%≤R≤30%, R refers to a mixture of at least two of Nd, Pr, Ce, La, Tb, and Dy, B with a weight percentage of 0.8%≤B≤1.2%, Gd with a weight percentage of 0%≤Gd≤5%, Ho with a weight percentage of 0%≤Ho≤5%, and M with a percentage of 0%≤M≤3%, wherein M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe. The low melting point powder contains NdCu, NdAl, and NdGa, and the weight percentage of each component is 0%≤NdCu≤3%, 0%≤NdAl≤3%, and 0%≤NdGa≤3%.

2. The low-weight rare earth magnet according to claim 1, characterized in that: The thickness of the low-heavy rare earth magnet is 0.3-6 mm.

3. A method for manufacturing a low-weight rare earth magnet according to claim 1, characterized in that: The steps include: S1, smelting and rapidly solidifying the prepared NdFeB alloy raw material to obtain NdFeB alloy flakes, and mechanically crushing the NdFeB alloy flakes into 150-400 μm scaly NdFeB alloy flakes; S2, mechanically mixing and stirring the flaky NdFeB alloy flakes, low melting point powder, and lubricant, and then placing them in a hydrogen treatment furnace for hydrogen absorption and dehydrogenation treatment, and preparing NdFeB powder by air jet milling; S3, pressing the above powder into a shape, and sintering to obtain the desired NdFeB magnet main alloy; S4, machining the sintered NdFeB magnet main body alloy into a desired shape, and then forming a low-heavy rare earth diffusion source film on a surface of the NdFeB magnet main body perpendicular or parallel to the C-axis direction by coating; S5. Perform diffusion and aging treatment to obtain low-heavy rare earth magnets.

4. The method for producing a low-weight rare earth magnet according to claim 3, characterized in that: The raw material composition of the NdFeB alloy described in step S1 contains rare earth R in a weight percentage of 28%≤R≤30%, where R refers to a mixture of at least two of Nd, Pr, Ce, La, Tb, and Dy, the weight percentage of B is 0.8%≤B≤1.2%, the weight percentage of Gd is 0%≤Gd≤5%, the weight percentage of Ho is 0%≤Ho≤5%, and the percentage of M is 0%≤M≤3%, where M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe. The low-melting-point powder contains NdCu, NdAl, and NdGa, and the weight percentage of each component is 0%≤NdCu≤3%, 0%≤NdAl≤3%, and 0%≤NdGa≤3%.

5. The method for manufacturing a low-weight rare earth magnet according to claim 3, characterized in that: The preparation method of the low-heavy rare earth diffusion source is atomization powder making, amorphous belt spinning powder making or ingot casting.

6. The method for manufacturing a low-weight rare earth magnet according to claim 3, characterized in that: In step S2, the hydrogen absorption and dehydrogenation treatment is performed at a dehydrogenation temperature of 400-600°C.

7. The method for manufacturing a low-weight rare earth magnet according to claim 3, characterized in that: The particle size of the low melting point powder in step S2 is 200 nm-4 μm, and the particle size of the NdFeB powder is 3-5 μm.

8. The method for manufacturing a low-weight rare earth magnet according to claim 3, characterized in that: The sintering temperature of the sintering process described in step S3 is 980-1060° C., and the sintering time is 6-15 hours.

9. The method for manufacturing a low-weight rare earth magnet according to claim 3, characterized in that: The diffusion temperature in step S5 is 850-930°C, the diffusion time is 6-30h, the aging temperature is 420-680°C, the heating rate is 1-5°C / min, the cooling rate is 5-20°C / min, and the aging time is 3-10h.

Citation Information

Cited By

  • Rare earth permanent magnets, methods and uses

    CN120809407A

  • Rare earth permanent magnets, methods and applications

    CN120809407B