Low-cost rare earth magnets and manufacturing methods
A low-cost NdFeB magnet is produced using a Ce-containing alloy with a low melting point diffusion source, addressing high production costs and performance issues by enhancing coercive force and temperature resistance.
Patent Information
- Application Number
- CN202111121731.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-09-24
AI Technical Summary
Existing NdFeB magnets face high production costs due to the use of heavy rare earth metals like Tb and Dy, and when Ce replaces Nd or PrNd, coercive force performance decreases, along with poor high temperature resistance.
A low-cost NdFeB magnet is manufactured using a neodymium iron boron alloy with a low melting point diffusion source, comprising CeCu, CeAl, and CeGa, coated with a diffusion source containing Ho, Gd, and other elements, and subjected to diffusion and aging processes to enhance coercive force and high temperature resistance.
The method significantly reduces heavy rare earth content, increasing coercive force by over 8kOe, enhances high temperature resistance, and lowers production costs while maintaining performance, allowing for mass production.
Smart Images

Figure BDA0003277259780000061 
Figure BDA0003277259780000071 
Figure BDA0003277259780000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of neodymium iron boron magnets, and in particular to a low-cost rare earth magnet and a manufacturing method thereof. Background Art
[0002] NdFeB sintered permanent magnets are widely used in high-tech fields such as electronic information, medical equipment, new energy vehicles, household appliances, robots, etc. In the past few decades of development, NdFeB permanent magnets have developed rapidly and become an indispensable functional material in the current industry. As we all know, among rare earths, the price of high-abundance Ce is much lower than that of pure Nd and PrNd. If Ce is used to partially replace pure Nd or PrNd, it can still achieve good commercial performance and greatly reduce the raw material cost of the magnet.
[0003] At the same time, the traditional manufacturing process consumes a large amount of Tb or Dy heavy rare earth metals, which greatly increases the cost. The heavy rare earth content can be greatly reduced through grain boundary diffusion technology, but with the current soaring prices of heavy rare earths Tb and Dy, the cost is still very high. Therefore, it is still important to continue to reduce the content of heavy rare earths. According to the diffusion mechanism, a large number of core-shell structures are formed to increase the coercive force through the diffusion hardening of the Nd2Fe14B main phase containing heavy rare earth elements. Therefore, the research on magnets and diffusion sources has become a hot topic.
[0004] However, after Ce partially replaces pure Nd or PrNd, the coercive force performance of the magnet is significantly lower than that before the replacement. The most significant effect of improving coercive force is through heavy rare earth diffusion, but heavy rare earth has low abundance and is expensive. Therefore, more and more researchers are preparing heavy rare earth alloys as diffusion sources for diffusion to achieve the same performance of NdFeB magnets. At the same time, the melting point of the grain boundary of Ce-containing magnets is low and the melting point of the diffusion source is low, so the high temperature resistance of the diffused magnets is poor. There are many patent applications for special grain boundary phases. For example, patent CN 108417380 A coats the magnet surface with alloy Cex(LREaHRE1-a)yM100-xy. This alloy is a Ce-containing magnet that reduces costs and improves the high temperature resistance of the magnet through diffusion. Patent CN111640549 A effectively regulates the magnetic moment and microstructure of the material by adding heavy rare earth elements, cobalt elements and trace elements, optimizes the grain boundary phase and grain boundary structure of sintered rare earth permanent magnet materials, and forms a sintered rare earth permanent magnet material with high temperature stability containing cobalt amorphous grain boundaries. However, there are few methods for diffusing low-cost magnets with low melting point diffusion sources to significantly increase coercivity and have good high temperature stability. Summary of the invention
[0005] In order to solve the above technical problems, the present invention proposes a low-cost rare earth magnet and a manufacturing method, by making a low-cost NdFeB magnet containing Ce and covering it with a diffusion source with a low melting point, and achieving a high coercive force increment after diffusion aging, that is, the combination of a low-cost magnet and a low-cost diffusion source achieves the purpose of high-performance NdFeB magnet.
[0006] In order to achieve the aforementioned invention object, the present invention provides the following technical solutions:
[0007] A low-cost rare earth magnet is prepared from a neodymium iron boron alloy and a diffusion source film coated on the surface of the neodymium iron boron alloy. The neodymium iron boron alloy is prepared by mixing a neodymium iron boron alloy raw material, a low melting point powder and other additives. The mixed low melting point powder contains CeCu, CeAl and CeGa, and the weight percentage of each component is 0%≤CeCu≤3%, 0%≤CeAl≤3%, and 0%≤CeGa≤3%; the diffusion source has a formula R1 x R2 y H z M 1-x-y-z The composition shown, wherein R1 refers to at least one of Nd and Pr, R2 is at least one of Ho and Gd, H refers to at least one of Tb and Dy, M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and x, y, and z are weight percentages, wherein 15%<x<50%, 0%<y≤10%, and 40%≤z≤70%.
[0008] Among them, the raw material components of the NdFeB alloy include rare earth R with a weight percentage of 28%≤R≤30%, R refers to at least two of Nd, Pr, Ho, and Gd, B with a weight percentage of 0.8%≤B≤1.2%, M with a weight percentage of 0≤M≤3%, wherein M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe.
[0009] The present invention also provides a method for manufacturing the above-mentioned low-cost rare earth magnet, comprising the following steps:
[0010] S1. The raw material composition of the iron-boron alloy includes rare earth R with a weight percentage of 28%≤R≤30%, where R refers to at least two of Nd, Pr, Ho, and Gd, B with a weight percentage of 0.8%≤B≤1.2%, and M with a weight percentage of 0≤M≤3%, where M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe. The prepared NdFeB alloy raw material is melted and rapidly solidified to obtain NdFeB alloy thin sheets;
[0011] S2, mechanically crushing the NdFeB alloy flakes into 150-400 μm flaky NdFeB alloy flakes, mixing low melting point powder, wherein the mixed low melting point powder contains CeCu, CeAl and CeGa, and the weight percentage of each component is 0%≤CeCu≤3%, 0%≤CeAl≤3%, 0%≤CeGa≤3%, and then high temperature dehydrogenation is carried out, and the low melting point powder is adhered to the flaky NdFeB alloy flakes, and NdFeB magnets are prepared by air flow milling, magnetic field orientation molding, sintering and heat treatment;
[0012] S3, machining the sintered NdFeB magnet into a desired shape, and then coating the surface of the NdFeB magnet with a diffusion source to form a diffusion source film, wherein the diffusion source has a formula R1 x R2 y H z M 1-x-y-z The composition shown, wherein R1 refers to at least one of Nd and Pr, R2 is at least one of Ho and Gd, H refers to at least one of Tb and Dy, M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and x, y, and z are weight percentages, wherein 15%<x<50%, 0%<y≤10%, and 40%≤z≤70%.
[0013] S4. Perform diffusion and aging treatment on the NdFeB magnet coated with the diffusion source film to produce a low-cost rare earth magnet.
[0014] Wherein, the high temperature hydrogen absorption and dehydrogenation treatment described in step S2 includes hydrogen absorption and dehydrogenation treatment, the hydrogen absorption temperature is 100-300°C, and the dehydrogenation temperature is 400-600°C.
[0015] Preferably, in the high temperature dehydrogenation treatment, the hydrogen content is less than 1000 ppm and the oxygen content is less than 500 ppm.
[0016] The particle size range of the low melting point powder in step S2 is 200nm-4μm, and the particle size of the D50 alloy powder produced by the air flow mill is 3-5μm.
[0017] Among them, the sintering temperature of the sintering process described in step S2 is 980-1060°C, the sintering time is 6-15h, the primary aging temperature is 850°C, the primary aging time is 3h, and the secondary aging temperature is 450-660°C, and the aging time is 3h.
[0018] Wherein, the preparation method of the diffusion source in step S3 is atomization powder making, amorphous belt spinning powder making or ingot casting.
[0019] Wherein, the diffusion temperature of the NdFeB magnet described in step S4 is 850-930°C, the diffusion time is 6-30h, the aging temperature is 420-680°C, and the aging time is 3-10h.
[0020] Wherein, the heating rate of the aging temperature of the NdFeB magnet in step S4 is 1-5°C / min, and the cooling rate is 5-20°C / min.
[0021] Compared with the prior art, the present invention is beneficial in that:
[0022] 1. The grain boundary is designed to be a low melting point magnet, that is, a low-cost NdFeB magnet containing Ce.
[0023] 2. Design a low melting point diffusion source, which has the dual role of low melting point and high temperature resistant elements and has low cost.
[0024] 3. The diffusion source is a low-heavy rare earth alloy diffusion source, which contains elements Ho and Gd that increase the high temperature resistance of the magnet, and can greatly increase the diffusion depth of the heavy rare earth, forming a double shell or even a triple shell structure of heavy rare earth Dy and Ho or Gd.
[0025] 4. The double-shell or even triple-shell structure and grain boundary structure of the deeply diffused heavy rare earth Dy and Ho or Gd can have good high temperature resistance.
[0026] 5. With less heavy rare earth content, the coercive force of the magnet is greatly increased, and the Dy diffusion range can be increased by more than 8kOe, basically achieving the diffusion effect of pure Tb metal and having high temperature resistance, which can greatly reduce the production cost of the magnet.
[0027] 6. The present invention is capable of significantly reducing the heavy rare earth content in magnets, improving high temperature resistance, and significantly reducing the cost of magnets. The process is simple and can be mass-produced. DETAILED DESCRIPTION
[0028] For better understanding and implementation, the present invention is described in detail below in conjunction with embodiments; the embodiments are only used to explain the present invention but are not used to limit the scope of the present invention.
[0029] A low-cost rare earth magnet, comprising a neodymium iron boron alloy and a diffusion source film coated on the surface of the neodymium iron boron alloy, wherein the neodymium iron boron alloy is prepared by mixing a neodymium iron boron alloy raw material, a low melting point powder and other additives, wherein the mixed low melting point powder contains CeCu, CeAl and CeGa, and the weight percentage of each component is 0%≤CeCu≤3%, 0%≤CeAl≤3%, and 0%≤CeGa≤3%; the diffusion source has a formula R1 x R2 y H z M 1-x-y-zThe composition shown, wherein R1 refers to at least one of Nd and Pr, R2 is at least one of Ho and Gd, H refers to at least one of Tb and Dy, M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and x, y, and z are weight percentages, wherein 15%<x<50%, 0%<y≤10%, and 40%≤z≤70%.
[0030] Among them, the raw material components of the NdFeB alloy include rare earth R with a weight percentage of 28%≤R≤30%, R refers to at least two of Nd, Pr, Ho, and Gd, B with a weight percentage of 0.8%≤B≤1.2%, M with a weight percentage of 0%≤M≤3%, wherein M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe.
[0031] The diffusion source is a low-heavy rare earth alloy diffusion source, which contains elements Ho and Gd that can increase the high temperature resistance of the magnet, that is, it can greatly improve the coercive force of the magnet and also make the magnet have better high temperature resistance.
[0032] With a lower content of heavy rare earth, the coercive force of the magnet can be greatly increased, and the Dy diffusion range can be increased by 8-11.5kOe, basically achieving the diffusion effect of pure Tb metal with high temperature resistance, and can greatly reduce the production cost of the magnet.
[0033] The double shell or even triple shell structure and grain boundary structure of deeply diffused heavy rare earth Dy and Ho or Gd have good high temperature resistance.
[0034] Wherein, the method of mixing the NdFeB alloy with the low melting point powder can be a method known to those skilled in the art, and can be uniformly mixed in a mixer. Preferably, other additives such as lubricants can be added when the NdFeB alloy powder is mixed with the low melting point powder. The lubricant is a commonly used lubricant, and the type, amount and usage of the lubricant are known to those skilled in the art and are not particularly limited.
[0035] According to the preparation method of the present application, after the NdFeB magnet is prepared, it is machined into a magnet of corresponding size and then covered with a diffusion source for diffusion and aging process. For details, see below.
[0036] 1. Composition of NdFeB alloy:
[0037] The composition examples are 1-29, and the comparative examples are 1-7, wherein 1-29 are NdFeB alloy raw materials mixed with low melting point alloy powders of different CeCu, CeAl, and CeGa component ratios, and 1-7 are for removing Ce components, and the unit is weight percentage, i.e., wt%, as shown in Table 1 below:
[0038] Table 1
[0039]
[0040] The blank means that the element is not contained. The composition is designed as above. The method for making the NdFeB alloys with embodiment numbers 1-29 is as follows:
[0041] (1) melting a quick-solidified NdFeB alloy raw material sheet without adding a low melting point powder component, and then mechanically crushing it into a scaly NdFeB alloy sheet with a particle size ranging from 150 to 400 μm;
[0042] (2) mixing CeCu, CeAl, and CeGa powders of corresponding alloy proportions with a particle size range of 200 nm-4 μm and adding them to the above-mentioned crushed scaly NdFeB alloy flakes;
[0043] (3) The mixed material is subjected to high-temperature absorption and dehydrogenation treatment, wherein the absorption temperature is 100-300°C and the dehydrogenation temperature is 400-600°C, the low melting point powder is adhered to the thin slice, and the air flow mill is used to obtain a NdFeB alloy powder with a D50 of 3-5 μm;
[0044] (4) The NdFeB alloy powder after air flow milling is subjected to magnetic field orientation molding and cold isostatic pressing to form a blank.
[0045] (5) The blank is subjected to vacuum sintering, argon gas is introduced for rapid cooling, and then primary tempering and secondary aging are performed, and the magnet performance is tested by digging out the column. The specific process is shown in Table 2 below;
[0046] Table 2
[0047]
[0048] (6) The blank is machined and cut into samples of corresponding sizes, and a diffusion source is made into a slurry and coated on two surfaces of the sample perpendicular to the C axis, the weight gain of the metal Dy is 1.0%, the content of Dy in the Dy alloy is 1.0%, and the weight gain is weight percentage, i.e., wt%;
[0049] The diffused Dy alloy is used as an example, and the diffused metal Dy is used as a comparative example. The specific process is shown in Table 3 below:
[0050] Table 3
[0051]
[0052] Based on the above data, NdFeB magnets with low melting point grain boundary channels were first made by adding CeCu, CeAl, and CeGa phase powders at the grain boundaries in the spinning strip slices. Diffusion of this low-cost NdFeB magnet is beneficial to diffusion, especially to the diffusion of heavy rare earth alloy diffusion sources. After diffusion, △Hcj>8kOe, and the coercive force increased significantly.
[0053] The embodiments and comparative examples are specifically analyzed as follows:
[0054] In Examples 1, 2, 3, 4 and Comparative Example 1, except for the change in Ce content, under the same NdFeB magnet composition and size, the same diffusion temperature and aging temperature, etc., compared with before diffusion, after diffusion of PrHoDyCu, Examples 1, 2, 3, 4 and Comparative Example 1, the decrease in Br is 0.22, 0.21, 0.23, 0.2, 0.23 kGS, and the increase in Hcj is 11.61, 11.2, 11.3, 11.2 and 10.21, respectively. It can be seen from the above that after Ce substitution, the increase in magnet performance is increased, and the performance of Example 1 and Comparative Example 1 only differs by 0.3 kOe, the temperature coefficient of Hcj is basically the same, the coercive force temperature coefficient of the comparative example is βHcj150℃=-0.520%, and the temperature coefficient of Example 1 is βHcj150℃=-0.521%, which is not much different, thus indicating that low-cost Ce-containing magnets have more obvious cost advantages.
[0055] In Examples 5, 6, 7, 8 and Comparative Example 2, except for the change in Ce content, under the same NdFeB magnet composition and size, the same diffusion temperature and aging temperature, compared with before diffusion, the diffusion of NdHoDyCu, Examples 5, 6, 7, 8 and Comparative Example 2, the Br decreases by 0.25, 0.26, 0.25, 0.23, 0.27 kGS, and the Hcj increases by 11.5, 11.1, 11.6, 11.3 and 10.11 respectively. It can be seen from the above that after Ce substitution, the increase in magnet performance is increased and the performance of Example 5 and Comparative Example 2 only differs by 0.5 kOe, the temperature coefficient of Hcj is basically the same, the coercive force temperature coefficient of Comparative Example 2 is βHcj150℃=-0.490%, and the temperature coefficient of Example 4 is βHcj150℃=-0.495%, which is not much different, thus indicating that low-cost Ce-containing magnets have more obvious cost advantages.
[0056] In Examples 9, 10, 11, 12 and Comparative Example 3, except for the change in Ce content, under the same NdFeB magnet composition and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, when PrGdDyCu was diffused, the decreases in Br in Examples 9, 10, 11, 12 and Comparative Example 3 were 0.25, 0.24, 0.24, 0.27, 0.26 kGS, respectively, and the increases in Hcj were 11.15, 11.3, 11.6, 11.3 and 9.85, respectively. From the above, it can be seen that after Ce substitution, the increase in magnet performance is increased and the performance of Example 5 and Comparative Example 2 only differs by 0.5 kOe, and the temperature coefficient of Hcj is basically the same. The coercive force temperature coefficient of Comparative Example 3 is βHcj150℃=-0.495%, and the temperature coefficient of Example 4 is βHcj150℃=-0.497%, which is not much different. This shows that low-cost Ce-containing magnets have more obvious cost advantages.
[0057] In Examples 13, 14, 15, 16 and Comparative Example 4, except for the change in Ce content, under the same NdFeB magnet composition and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, when PrGdDyCuGa was diffused, the decreases in Br in Examples 13, 14, 15, 16 and Comparative Example 4 were 0.25, 0.27, 0.26, 0.24, 0.25 kGS, and the increases in Hcj were 9.2, 9.4, 9.5, 9.0 and 7.9, respectively. From the above, it can be seen that after Ce substitution, the increase in magnet performance is increased and the performance of Example 13 and Comparative Example 4 only differs by 0.4kOe, and the temperature coefficient of Hcj is basically the same. The coercive force temperature coefficient of Comparative Example 4 is βHcj150℃=-0.485%, and the temperature coefficient of Example 13 is βHcj150℃=-0.486%, which is not much different. This shows that low-cost Ce-containing magnets have more obvious cost advantages.
[0058] In Examples 17, 18, 19, 20 and Comparative Example 5, except for the change in Ce content, under the same NdFeB magnet composition and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, when PrHoDyCuGa was diffused, the decreases in Br in Examples 17, 18, 19, 20 and Comparative Example 5 were 0.25, 0.25, 0.27, 0.25, 0.27 kGS, and the increases in Hcj were 10.8, 10.7, 10.5, 10 and 9.48, respectively. From the above, it can be seen that after Ce substitution, the increase in magnet performance is increased and the performance of Example 17 and Comparative Example 5 only differs by 0.5 kOe, and the temperature coefficient of Hcj is basically the same. The coercive force temperature coefficient of Comparative Example 4 is βHcj150℃=-0.495%, and the temperature coefficient of Example 13 is βHcj150℃=-0.496%, which is not much different. This shows that low-cost Ce-containing magnets have more obvious cost advantages.
[0059] In Examples 21, 22, 23, 24 and Comparative Example 6, except for the change in Ce content, under the same NdFeB magnet composition and size, the same diffusion temperature and aging temperature, etc., compared with before diffusion, after diffusion of PrHoDyCuAl, Examples 21, 22, 23, 24 and Comparative Example 6, the Br decreases by 0.2, 0.23, 0.23, 0.2, 0.2 kGS, and the Hcj increases by 10, 9.7, 9.5, 9.3 and 8.77, respectively. It can be seen from the above that after Ce substitution, the increase in magnet performance increases, and the performance of Example 21 and Comparative Example 6 only differs by 0.5 kOe, and the temperature coefficient of Hcj is basically the same. The coercive force temperature coefficient of Comparative Example 6 is βHcj150℃=-0.505%, and the temperature coefficient of Example 21 is βHcj150℃=-0.509%, which is not much different, so it shows that low-cost Ce-containing magnets have more obvious cost advantages.
[0060] In Examples 26, 27, 28, 29 and Comparative Example 7, except for the change in Ce content, under the same NdFeB magnet composition and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, when PrGdDyCu was diffused, the decreases in Br in Examples 26, 27, 28, 29 and Comparative Example 7 were 0.22, 0.21, 0.2, 0.22, 0.21 kGS, and the increases in Hcj were 9.57, 9.8, 9.15, 8.87 and 8.17, respectively. From the above, it can be seen that after Ce substitution, the increase in magnet performance is increased and the performance of Example 26 and Comparative Example 7 differs by only 0.3kOe, and the temperature coefficient of Hcj is basically the same. The coercive force temperature coefficient of Comparative Example 6 is βHcj150℃=-0.560%, and the temperature coefficient of Example 21 is βHcj150℃=-0.565%, which is not much different. This shows that low-cost Ce-containing magnets have more obvious cost advantages.
[0061] With reference to the above embodiments, experiments were conducted with other raw materials and conditions listed in this specification, and the low-cost rare earth magnet of the present invention was also produced.
[0062] According to the above analysis, the comparison between the heavy rare earth alloy diffusion source Ce-containing magnet and the conventional magnet shows that the heavy rare earth alloy diffusion Ce-containing magnet has obvious cost advantage, and the increase of coercivity is obviously greater than that of the conventional magnet. Through the combined effect of the diffusion source and the Ce-containing magnet, the Ce-containing magnet can meet the use of many magnet brands and has obvious cost advantage.
[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
[0064] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0065] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A low-cost rare earth magnet, prepared from a neodymium iron boron alloy and a diffusion source film coated on the surface of the neodymium iron boron alloy, Features: The NdFeB alloy is prepared by mixing NdFeB alloy raw material, low melting point powder and other additives. The mixed low melting point powder contains CeCu, CeAl and CeGa, and the weight percentage of each component is 0%≤CeCu≤3%, 0%≤CeAl≤3%, 0%≤CeGa≤3%; the diffusion source has the formula R1 x R2 y Hz 1-x-y-z The composition shown, wherein R1 refers to at least one of Nd and Pr, R2 refers to at least one of Ho and Gd, H refers to at least one of Tb and Dy, M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, Sn, x, y, z are weight percentages, wherein 15%<x<50%, 0%<y≤10%, 40%≤z≤70%; The method for manufacturing the low-cost rare earth magnet comprises the following steps: S1. The raw material composition of the NdFeB alloy includes rare earth R with a weight percentage of 28%≤R≤30%, where R refers to at least two of Nd, Pr, Ho, and Gd, B with a weight percentage of 0.8%≤B≤1.2%, M with a weight percentage of 0≤M≤3%, where M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe. The prepared NdFeB alloy raw material is melted and rapidly solidified to obtain NdFeB alloy thin sheets; S2, mechanically crushing the NdFeB alloy flakes into 150-400 μm flaky NdFeB alloy flakes, mixing low melting point powder, the mixed low melting point powder containing CeCu, CeAl and CeGa, the weight percentage of each component is 0%≤CeCu≤3%, 0%≤CeAl≤3%, 0%≤CeGa≤3%, after mixing, high temperature absorption and dehydrogenation, the low melting point powder is adhered to the flaky NdFeB alloy flakes, and prepared into NdFeB magnets by air flow milling, magnetic field orientation molding, sintering and heat treatment; S3, machining the sintered NdFeB magnet into a desired shape, and then coating the surface of the NdFeB magnet with a diffusion source to form a diffusion source film, wherein the diffusion source has a formula R1 x R2 y H z M 1-x-y-z The composition shown, wherein R1 refers to at least one of Nd and Pr, R2 refers to at least one of Ho and Gd, H refers to at least one of Tb and Dy, M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, Sn, x, y, z are weight percentages, wherein 15%<x<50%, 0%<y≤10%, 40%≤z≤70%; S4, subjecting the NdFeB magnet coated with the diffusion source to diffusion and aging treatment to produce the low-cost rare earth magnet.
2. The low-cost rare earth magnet according to claim 1, It is characterized in that The raw material components of the NdFeB alloy include rare earth R with a weight percentage of 28%≤R≤30%, where R refers to at least two of Nd, Pr, Ho, and Gd, B with a weight percentage of 0.8%≤B≤1.2%, M with a weight percentage of 0≤M≤3%, where M refers to at least one of Co, Mg, Ti, Zr, Nb, and Mo, and the remaining component is Fe.
3. The low-cost rare earth magnet according to claim 1, Features The high temperature hydrogen absorption and dehydrogenation treatment in step S2 includes hydrogen absorption and dehydrogenation treatment, the hydrogen absorption temperature is 100-300°C, and the dehydrogenation temperature is 400-600°C.
4. The low-cost rare earth magnet according to claim 3, Features In the high-temperature dehydrogenation treatment, the hydrogen content is less than 1000 ppm and the oxygen content is less than 500 ppm.
5. The low-cost rare earth magnet according to claim 1, Features In step S2, the particle size range of the low melting point powder is 200nm-4μm, and the particle size of the D50 alloy powder produced by the air flow mill is 3-5μm.
6. The low-cost rare earth magnet according to claim 1, Features In step S2, the sintering temperature of the sintering process is 980-1060°C, the sintering time is 6-15h, the primary aging temperature is 850°C, the primary aging time is 3h, and the secondary aging temperature is 450-660°C, and the aging time is 3h.
7. The low-cost rare earth magnet according to claim 1, Features , The preparation method of the diffusion source in step S3 is atomization powder making, amorphous belt powder making or ingot casting.
8. The low-cost rare earth magnet according to claim 1, It is characterized in that In step S4, the diffusion temperature of the NdFeB magnet is 850-930°C, the diffusion time is 6-30h, the aging temperature is 420-680°C, and the aging time is 3-10h.
9. The low-cost rare earth magnet according to claim 8, It is characterized in that In step S4, the heating rate of the aging temperature of the NdFeB magnet is 1-5°C / min, and the cooling rate is 5-20°C / min.
Citation Information
Patent Citations
Low-cost diffusion source alloy, grain boundary diffusion magnet and preparation method thereof
CN108417380A
Method for preparing high-performance sintered Nd-Fe-B magnet by using two-step grain boundary diffusion technique
CN107256795A
Coating material for permeable magnet and preparation method of high-coercivity neodymium-iron-boron magnet