Polysilicon surface metal detection sample preparation method and detection method

Through high-acidity mixed liquid elution and evaporation to dryness, polycrystalline silicon surface metal detection samples are directly obtained, which solves the problems of long leaching time and impurity introduction, and achieves fast and accurate polycrystalline silicon surface metal detection.

CN113899600BActive Publication Date: 2024-10-22XINJIANG XINTE XINNENG MATERIAL TESTING CENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010567959.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-19
Publication Date
2024-10-22
Estimated Expiration
2040-06-19

AI Technical Summary

Technical Problem

In the existing polysilicon surface metal detection methods, the leaching time is long and environmental impurities are easily introduced, resulting in a long detection cycle and low accuracy.

Method used

A mixture of high acidity nitric acid and hydrofluoric acid is used for rapid elution, combined with water elution and evaporation to dryness. The leaching process is omitted, and the polycrystalline silicon surface metal detection sample is obtained directly by dissolving the heating residue and nitric acid.

Benefits of technology

It significantly shortens the detection sample preparation time, reduces the introduction of environmental impurities, improves detection accuracy and efficiency, and simplifies the operation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113899600B_ABST
    Figure CN113899600B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a polysilicon surface metal detection sample, comprising: weighing polysilicon; using a mixed acid solution of nitric acid and hydrofluoric acid to quickly rinse the surface of the polysilicon to obtain an acid wash solution; then rinsing the acid-washed polysilicon with water to obtain a water wash solution; heating the acid wash solution and the water wash solution together until evaporated to dryness; adding nitric acid to the evaporated residue to dissolve it, and then constant-volume the dissolved solution to obtain a sample for polysilicon surface metal detection. The present invention also discloses a polysilicon surface metal detection method comprising the above sample preparation method. The present invention can greatly shorten the time for sample preparation and detection cycle, and improve detection accuracy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polysilicon, and in particular relates to a polysilicon surface metal detection sample preparation method and a polysilicon surface metal detection method. Background Art

[0002] Polysilicon is the main raw material for manufacturing high-purity silicon products such as silicon polishing wafers, solar cells, and electronic chips. Its purity requirements are very high, especially for electronic-grade polysilicon, the purity requirement is above 99.9999%. Impurities in polysilicon are divided into surface metal impurities and matrix metal impurities according to their source and distribution. Matrix metal impurities come from materials such as raw silicon powder used to produce polysilicon products. They can be basically removed by distillation, and the content of B and P can be reduced to the ppta order of magnitude. Surface metal impurities come from the external environment. For example, in the storage, crushing, and packaging of polysilicon products, metals, non-metals, and indoor dust come into contact with polysilicon products, resulting in the deposition of metal elements such as Fe, Cr, Ni, Cu, and Zn on the surface of polysilicon materials.

[0003] If such polycrystalline silicon with metal impurities on its surface is used to pull single crystal silicon and make solar cells, it will directly affect the crystallization of single crystal pulling and the minority carrier life after casting, and further affect the conversion efficiency of the manufactured solar cells, causing the battery components to decay seriously during the power generation process, affecting the power generation. Therefore, it is necessary to strictly control the surface metal impurity content of polycrystalline silicon.

[0004] At present, the detection process of metal impurities on the surface of polysilicon includes: taking a polysilicon sample and putting it into a mixed solution of nitric acid, hydrofluoric acid, hydrogen peroxide and water, leaching at a certain temperature for a period of time (about 1h), so that the impurities on the surface of the polysilicon are deposited in the leaching solution, and then evaporating to dryness (about 2h), and after constant volume, using an inductively coupled plasma mass spectrometer to determine the metal impurity content therein. In the process of preparing the test sample, due to the use of leaching, it takes a long time to prepare the test sample, and the long-term exposure of the leaching solution to the environment will cause impurities such as K, Ca, Al, Fe in the environment to settle into the leaching solution, thereby causing the test results to be unable to accurately reflect the surface metal impurity content of the polysilicon product and the long detection cycle. In addition, due to the low acidity of the mixed solution (the volume ratio of nitric acid, hydrofluoric acid, hydrogen peroxide and water is 1:1:1:50), only the leaching method can be used, and even heating is required during leaching to make the metal impurities on the surface of the polysilicon react with the mixed solution and deposit in the leaching solution, which increases the difficulty of operation. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a polysilicon surface metal detection sample preparation method and detection method in view of the above-mentioned deficiencies in the prior art, which can greatly shorten the sample preparation time and detection cycle and improve the detection accuracy.

[0006] According to one aspect of the present invention, a method for preparing a polysilicon surface metal detection sample is provided, and its technical solution is as follows:

[0007] A method for preparing a polysilicon surface metal detection sample, comprising:

[0008] S101 Sampling: weigh polysilicon;

[0009] S102 pickling: using a mixed acid solution of nitric acid and hydrofluoric acid to quickly rinse the surface of the polysilicon to obtain a pickling solution;

[0010] S103 water washing: washing the polycrystalline silicon after acid washing with water to obtain a water washing liquid;

[0011] S104 evaporation: heating the acid wash liquid and the water wash liquid together until evaporated to dryness;

[0012] S105 volume fixing: adding nitric acid solution to the residue after evaporation to dissolve it, and then fixing the volume of the solution obtained by the solution to obtain a polysilicon surface metal detection sample.

[0013] Preferably, the amount of the mixed acid solution is: when the amount of the polysilicon is 30-50 g, the amount of the mixed acid solution is 10-15 ml.

[0014] Preferably, in the mixed acid solution, the volume ratio of the nitric acid to the hydrofluoric acid is (0.5-5):1.

[0015] Preferably, the nitric acid and the hydrofluoric acid are both electronic grade, and the mass fraction of the nitric acid is 55% to 68%, and the mass fraction of the hydrofluoric acid is 38 to 44%.

[0016] Preferably, in step S102, the cleanliness of the washing environment is at least Class 10 (national standard GB50073-2001), and the washing speed is 2 to 3 drops per second.

[0017] Preferably, in the step S103, the grade of water used for the water washing is at least laboratory grade one water, and the amount of the water used is 0.5 to 1 times the volume of the mixed acid solution.

[0018] Preferably, in the step S104, the heating temperature is 170-210°C.

[0019] Preferably, in the step S105, the amount of nitric acid used is 2% to 5% of the volume of the polycrystalline silicon surface metal detection sample obtained by constant volume.

[0020] Preferably, in the step S105, deionized water is used for the constant volume.

[0021] According to another aspect of the present invention, a method for detecting metal on the surface of polysilicon is provided, and its technical solution is as follows:

[0022] A method for detecting metal on the surface of polysilicon, comprising:

[0023] S201, preparing a polycrystalline silicon surface metal detection sample by using the polycrystalline silicon surface metal detection sample preparation method described above;

[0024] S202, using an inductively coupled plasma mass spectrometer to detect the metal impurity content of the prepared polysilicon surface metal detection sample.

[0025] The beneficial effects of the present invention are as follows:

[0026] By leaching the polysilicon surface with an acid solution with higher acidity, the metal impurities on the polysilicon surface can be quickly dissolved. Compared with the traditional leaching method using an acid solution with lower acidity, the leaching process is omitted and the sample preparation speed is faster. It can not only greatly shorten the preparation time of the test sample and shorten the test cycle, but also reduce or avoid the introduction of impurity elements such as K, Ca, Al, Fe, etc. from the environment, improve the detection efficiency and detection accuracy. In addition, the pickling process does not require heating and the operation is simpler. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a flow chart of a method for preparing a polysilicon surface metal detection sample in an embodiment of the present invention. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further clearly and completely described below in conjunction with the accompanying drawings and specific embodiments of the present invention.

[0029] In view of the prior art, the leaching time is long during the preparation of polycrystalline silicon surface metal detection samples, and impurities such as K, Ca, Al, and Fe are easily introduced from the environment, resulting in long detection cycles and low detection accuracy. Therefore, the present invention discloses a method for preparing polycrystalline silicon surface metal detection samples, comprising:

[0030] S101 Sampling: weigh polysilicon;

[0031] S102 pickling: using a mixed acid solution of nitric acid and hydrofluoric acid to quickly rinse the surface of the polysilicon to obtain a pickling solution;

[0032] S103 water washing: washing the acid-washed polysilicon with water to obtain a water washing solution;

[0033] S104 evaporation: heating the acid wash liquid and the water wash liquid together until evaporated to dryness;

[0034] S105 volume fixing: adding nitric acid to the residue after evaporation to dissolve it, and then fixing the volume of the solution obtained by the solution to obtain a sample for metal detection on the surface of polycrystalline silicon.

[0035] Accordingly, the present invention further provides a method for detecting metal on the surface of polycrystalline silicon, comprising:

[0036] S201, preparing a polycrystalline silicon surface metal detection sample by using the polycrystalline silicon surface metal detection sample preparation method described above;

[0037] S202, using an inductively coupled plasma mass spectrometer to detect the metal impurity content of the prepared polysilicon surface metal detection sample.

[0038] Example 1

[0039] like Figure 1 As shown, this embodiment discloses a method for preparing a polysilicon surface metal detection sample, comprising:

[0040] S101 Sampling: Weigh polycrystalline silicon.

[0041] Among them, considering that too much polysilicon will increase the amount of acid and water required for subsequent pickling and water washing, prolong the time required for subsequent evaporation and other processes, and reduce the sample preparation speed, too little polysilicon will increase the difficulty of operation and increase the operation error. Therefore, after a large number of tests, the amount of polysilicon in this embodiment is preferably 30-50g, and since the content of metal on the surface of polysilicon is at the ppbw level, the mass of the polysilicon weighed should be accurate to 0.0001g.

[0042] S102 pickling: The surface of the polysilicon is quickly rinsed with a mixture of nitric acid and hydrofluoric acid to obtain a pickling solution.

[0043] Wherein, the nitric acid and hydrofluoric acid for preparing mixed acid solution are both electronic grade, to reduce the influence of metal ions that may be contained therein on the subsequent sample detection results. And, the mass fraction of electronic grade nitric acid is 55%~68%, preferably 55% nitric acid, the mass fraction of electronic grade hydrofluoric acid is 38%~44%, preferably 38% hydrofluoric acid, the volume ratio of nitric acid and hydrofluoric acid is (0.5~5):1, more preferably, the volume ratio of nitric acid and hydrofluoric acid is (2~3):1, the mixed acid prepared in this way has higher acidity, can react with polysilicon surface metal in leaching process, make polysilicon surface metal impurities dissolve and deposit in acid solution, the acid solution containing metal impurities is the above-mentioned pickling solution, compared with traditional acid solution leaching method, the leaching time is short, can greatly shorten the preparation time of detection sample, improve detection efficiency, and do not need heating, operation is simpler. The main reaction formula of pickling process is:

[0044] X+H + +NO3→X + +NO+H2O

[0045] In the formula: X represents metals such as Cu, Fe, Zn, Ni, K, Ca, Al, Fe, etc.

[0046] In this embodiment, the amount of mixed acid solution is mainly determined based on the weighed polysilicon sample. When the amount of polysilicon is 30-50g, the amount of mixed acid solution is 10-15ml to ensure that the surface metal of the polysilicon can be dissolved as completely as possible in the pickling solution.

[0047] In this embodiment, the cleanliness of the environment for mixed acid washing is at least Class 10 (National Standard GB50073-2001) to avoid the introduction of impurity elements such as K, Ca, Al, and Fe from the environment. During acid washing, the washing speed is 2 to 3 drops per second (measured by a commercially available pipette) to ensure that the acid and the metal impurities on the surface of the polysilicon react completely.

[0048] S103 water washing: rinse the acid-washed polysilicon with water to obtain a washing solution.

[0049] In this embodiment, the grade of water used in the water rinsing process is at least laboratory grade one water, such as deionized water, ultrapure water, etc., and the amount of water used is 0.5-1.0 times the volume of the mixed acid solution in the pickling process.

[0050] It should be noted that, since the mixed acid solution in this embodiment is highly corrosive, the containers used in the pickling and water washing processes are preferably made of acid-corrosive materials, such as beakers made of polytetrafluoroethylene.

[0051] S104 evaporation: heating the acid wash liquid and the water wash liquid together until evaporated to dryness;

[0052] In this embodiment, the heating temperature of the evaporation process is 170-210°C, so that the silicon in the pickling solution and the water washing solution can be completely volatilized in the form of silicon tetrafluoride (SiF4), so as to reduce the influence of the matrix effect on the subsequent detection of the metal impurity content and improve the detection accuracy. Moreover, under the condition of 170-210°C, it can also ensure that the impurities in the polytetrafluoroethylene beaker will not precipitate (the precipitation temperature is about 250°C).

[0053] S105 volume fixing: adding nitric acid to the residue after evaporation to dissolve it, and then fixing the volume of the solution obtained by the solution to obtain a sample for metal detection on the surface of polycrystalline silicon.

[0054] In this embodiment, the residue after evaporation is preferably dissolved with nitric acid, the mass fraction of nitric acid is 55% to 68%, preferably 55% nitric acid, and the amount of nitric acid used is 2% to 5% of the volume of the polycrystalline silicon surface metal detection sample obtained by constant volume, that is, when the volume of the polycrystalline silicon surface metal detection sample after constant volume is 10ml, the amount of nitric acid used is 0.2 to 0.5ml. After the residue is completely dissolved, deionized water, ultrapure water or other water that does not contain metal impurities is used for constant volume, such as transferring the residue solution to a 10ml volumetric flask and constant volume to obtain the above-mentioned sample that can be used for polycrystalline silicon surface metal detection.

[0055] It should be noted that, because the metal content on the surface of polysilicon is at the ppbw level, the entire process in this embodiment is preferably carried out in an environment with a cleanliness level of at least Class 10 to reduce the introduction of metal impurities from the environment.

[0056] The polysilicon surface metal detection sample preparation method of this embodiment adopts nitric acid and hydrofluoric acid to prepare a high acidity (H + The mixed acid solution (the acidity of the mixed acid solution is 1.82%-1.91%) is used to wash the surface of the polycrystalline silicon, which can quickly dissolve the metal impurities on the surface of the polycrystalline silicon. Compared with the traditional leaching method using an acid solution with lower acidity, the leaching process is omitted and the sample preparation speed is faster. Not only can the preparation time of the test sample be greatly shortened, but also the introduction of impurity elements such as K, Ca, Al, Fe, etc. from the environment can be reduced or avoided. In addition, the pickling process does not require heating, and the operation is simpler.

[0057] Disclosed below are several groups of preparation examples of polycrystalline silicon surface metal detection samples prepared using the above-mentioned polycrystalline silicon surface metal detection sample preparation method. It should be noted that the following preparation examples are only a few limited examples and are not limited to them.

[0058] Preparation Example 1

[0059] This preparation embodiment discloses a method for preparing a polysilicon surface metal detection sample, comprising:

[0060] (1) Weigh 30.0000 g of polycrystalline silicon and put it into a polytetrafluoroethylene beaker.

[0061] (2) placing the beaker containing the polycrystalline silicon in a fume hood with a cleanliness level of Class 10; using a mixed acid solution prepared by a nitric acid solution with a mass fraction of 55% and a hydrofluoric acid solution with a mass fraction of 38% in a volume ratio of 2:1; using a pipette to take 10 ml of the mixed acid solution, and rapidly pouring it onto the surface of the polycrystalline silicon at a speed of 2 to 3 drops per second (the amount of each drop is controlled to be about 0.2 ml) (i.e., acid leaching), so that the metal impurities on the surface of the polycrystalline silicon are rapidly dissolved, and an acid washing solution containing metal impurities is obtained.

[0062] (3) Slowly pour 5 ml of deionized water onto the surface of the polycrystalline silicon after the mixed acid solution washing (i.e., water washing) to obtain a water washing solution.

[0063] (4) After the acid wash liquid and the water wash liquid are combined, they are heated at 170° C. to evaporate to dryness, and the silicon in the acid wash liquid and the water wash liquid is volatilized in the form of silicon tetrafluoride.

[0064] (5) 0.2 ml of 68% nitric acid was added to the residue obtained after evaporation to fully dissolve the residue, and then 9.8 ml of deionized water was added to make up the volume to obtain a sample for metal detection on the surface of polycrystalline silicon.

[0065] Preparation Example 2

[0066] This embodiment discloses a method for preparing a polysilicon surface metal detection sample, comprising:

[0067] (1) Weigh 40.0000 g of polycrystalline silicon and place it in a polytetrafluoroethylene beaker.

[0068] (2) placing the beaker containing the polycrystalline silicon in a fume hood with a cleanliness level of Class 10; using a mixed acid solution prepared by a nitric acid solution with a mass fraction of 60% and a hydrofluoric acid solution with a mass fraction of 40% in a volume ratio of 3:1; using a pipette to take 15 ml of the mixed acid solution, and rapidly pouring it onto the surface of the polycrystalline silicon at a speed of 2 to 3 drops per second (i.e., acid leaching), so that the metal impurities on the surface of the polycrystalline silicon are rapidly dissolved, and an acid washing solution containing metal impurities is obtained.

[0069] (3) Slowly pour 15 ml of ultrapure water onto the surface of the polycrystalline silicon after the mixed acid solution washing (i.e., water washing) to obtain a water washing solution.

[0070] (4) The acid wash liquid and the water wash liquid are combined and heated to dryness at 180° C. to volatilize the silicon in the acid wash liquid and the water wash liquid in the form of silicon tetrafluoride.

[0071] (5) 0.4 ml of 60% by mass nitric acid was added to the residue obtained after evaporation to fully dissolve the residue, and then 9.6 ml of ultrapure water was added to make up the volume to obtain a sample for metal detection on the surface of polycrystalline silicon.

[0072] Preparation Example 3

[0073] This embodiment discloses a method for preparing a polysilicon surface metal detection sample, comprising:

[0074] (1) Weigh 50.0000 g of polycrystalline silicon and put it into a polytetrafluoroethylene beaker.

[0075] (2) placing the beaker containing the polycrystalline silicon in a fume hood with a cleanliness level of Class 10; using a mixed acid solution prepared by a nitric acid solution with a mass fraction of 65% and a hydrofluoric acid solution with a mass fraction of 4:1; using a pipette to take 12 ml of the mixed acid solution, and rapidly pouring it onto the surface of the polycrystalline silicon at a speed of 2 to 3 drops per second (i.e., acid leaching), so that the metal impurities on the surface of the polycrystalline silicon are rapidly dissolved, and obtaining an acid washing solution containing metal impurities.

[0076] (3) Slowly pour 18 ml of deionized water onto the surface of the polycrystalline silicon after the mixed acid solution washing (i.e., water washing) to obtain a water washing solution.

[0077] (4) The acid wash liquid and the water wash liquid are combined and heated to dryness at 190°C to volatilize the silicon in the acid wash liquid and the water wash liquid in the form of silicon tetrafluoride.

[0078] (5) Add 0.5 ml of 55% by mass nitric acid to the residue obtained after evaporation to fully dissolve the residue, then add 9.5 ml of deionized water to make up the volume, and obtain a sample for metal detection on the surface of polycrystalline silicon.

[0079] Example 2

[0080] This embodiment also discloses a method for detecting metal on the surface of polysilicon, comprising:

[0081] S201 Sample preparation: Prepare a polycrystalline silicon surface metal detection sample using the polycrystalline silicon surface metal detection sample preparation method described in Example 1.

[0082] S202 detection: The metal impurity content of the prepared polysilicon surface metal detection sample is detected using an inductively coupled plasma mass spectrometer.

[0083] It should be noted that, in the detection process of this embodiment, other methods other than the ICP-MS method of the inductively coupled plasma mass spectrometer (such as the ICP-AES method of the inductively coupled plasma atomic emission spectrometer) may be used to detect the metal impurity content, which is not further limited in this embodiment.

[0084] In this embodiment, six groups of mixed acid solutions were prepared according to the volume ratio of nitric acid to hydrofluoric acid of 0.5:1, 1:1, 2:1, 3:1, 4:1, and 5:1, respectively. The polycrystalline silicon surface metal detection sample preparation method described in Preparation Example 1 in Example 1 was used to prepare six groups of polycrystalline silicon surface metal detection samples. Then, the six groups of polycrystalline silicon surface metal detection samples were tested for metal impurity content using an inductively coupled plasma mass spectrometer under the same conditions. The test results are shown in Table 1:

[0085] Table 1 Metal impurity content on the surface of polysilicon detected under mixed acid solutions with different ratios

[0086]

[0087] As can be seen from Table 1, when the volume ratio of nitric acid to hydrofluoric acid is 2:1 and 3:1, the detected data of the metal content on the surface of polycrystalline silicon is relatively stable and close. At this time, it can be basically considered that the mixed acid solution prepared at this volume ratio can just dissolve the metal impurities on the surface of polycrystalline silicon. Therefore, in this embodiment, it is preferred to use a mixed acid solution prepared at a volume ratio of nitric acid to hydrofluoric acid of (2-3):1 as the eluent for the pickling process.

[0088] The polysilicon surface metal detection method of the present embodiment can quickly dissolve the metal impurities on the polysilicon surface by leaching the polysilicon surface with an acid solution with higher acidity. Compared with the traditional leaching method using an acid solution with lower acidity, the leaching process is omitted and the sample preparation speed is faster. It can not only greatly shorten the preparation time of the test sample and shorten the detection cycle, but also reduce or avoid the introduction of impurity elements such as K, Ca, Al, Fe, etc. from the environment, thereby improving the detection efficiency and detection accuracy. In addition, the pickling process does not require heating, and the operation is simpler.

[0089] It is to be understood that the above is only a preferred embodiment of the present invention, but the present invention is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered as the protection scope of the present invention.

Claims

1. A method for preparing a polysilicon surface metal detection sample, comprising: S101 Sampling: weigh polysilicon; S102 pickling: using a mixed acid solution of nitric acid and hydrofluoric acid to quickly rinse the surface of the polysilicon to obtain a pickling solution; S103 water washing: washing the polycrystalline silicon after acid washing with water to obtain a water washing liquid; S104 evaporation: heating the acid wash liquid and the water wash liquid together until evaporated to dryness; S105 volume fixing: adding nitric acid to the residue after evaporation to dissolve it, and then fixing the volume of the solution obtained by the dissolution to obtain a polysilicon surface metal detection sample; Among them, H + The acidity of the mixed acid solution is 1.82%-1.91% by mass percentage, the nitric acid and hydrofluoric acid used to prepare the mixed acid solution are both electronic grade, the mass fraction of electronic grade nitric acid is 55%-68%, the mass fraction of electronic grade hydrofluoric acid is 38%-44%, the volume ratio of nitric acid to hydrofluoric acid is (0.5-5):1, the amount of the mixed acid solution is 10-15ml when the amount of the polycrystalline silicon is 30-50g, and the elution speed during pickling is 2-3 drops / second.

2. The method for preparing a polysilicon surface metal detection sample according to claim 1, characterized in that: In step S102, The cleanliness level of the washing environment is at least Class 10.

3. The method for preparing a polysilicon surface metal detection sample according to claim 1, characterized in that: In the step S103, the grade of water used for the water washing is at least laboratory grade one water, and the amount of the water used is 0.5 to 1 times the volume of the mixed acid solution.

4. The method for preparing a polysilicon surface metal detection sample according to claim 1, characterized in that: In the step S104, the heating temperature is 170-210°C.

5. The method for preparing a polysilicon surface metal detection sample according to claim 1, characterized in that: In the step S105, the amount of nitric acid used is 2% to 5% of the volume of the polycrystalline silicon surface metal detection sample obtained by constant volume.

6. The method for preparing a polysilicon surface metal detection sample according to claim 1, characterized in that: In the step S105, deionized water is used for the constant volume.

7. A method for detecting metal on the surface of polysilicon, characterized in that: include: S201, preparing a polycrystalline silicon surface metal detection sample by using the polycrystalline silicon surface metal detection sample preparation method according to any one of claims 1 to 6; S202, using an inductively coupled plasma mass spectrometer to detect the metal impurity content of the prepared polysilicon surface metal detection sample.