Method for preparing anti-reflection film with gradient refractive index characteristics

By adjusting the CO2 flow rate in the reaction gas in silicon-based laminated solar cells, the refractive index gradient of hydrogenated nanocrystalline silicon oxygen is changed, and an anti-reflection film suitable for the full spectrum range is prepared, which solves the problem of insufficient anti-reflection effect in the existing technology. Optimize the problem and improve the efficiency and applicability of solar cells.

CN113921620BActive Publication Date: 2024-10-29NANKAI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111359180.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-17
Publication Date
2024-10-29
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

The anti-reflection effect of the anti-reflection film in existing silicon-based tandem solar cells is poor, especially in the long-wave range of 800-1200 nm, resulting in low current and sensitivity to the selection and thickness of the absorber layer material, which limits the improvement of cell efficiency. .

Method used

By adjusting the CO2 flow rate in the reaction gas, the ratio of Si and O in nc-SiOx:H is adjusted to achieve a gradient change in the refractive index, thereby preparing an anti-reflective film with gradient refractive index characteristics, which can be used in silicon-based laminated solar cells to reduce Optical reflection.

Benefits of technology

It achieves effective anti-reflection in the full spectrum range, improves the efficiency of solar cells, solves the dependence on the incident angle of the solar spectrum and the thickness of the absorbing layer material, is suitable for different types of silicon-based stacked cells, and has high transparency and simple process .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113921620B_ABST
    Figure CN113921620B_ABST
Patent Text Reader

Abstract

A method for preparing an antireflection film with a refractive index gradient characteristic. The present invention develops an nc-SiOx:H antireflection film with a refractive index gradient characteristic. By adjusting the flow rate of CO2 in the reaction gas, the ratio of Si and O in nc-SiOx:H, that is, the value of x (0 < x ≤ 2), is adjusted to achieve a gradient change in the refractive index, which can achieve effective antireflection in the full spectral range and solve the dependence of traditional antireflection films on the incident angle of the solar spectrum and the thickness of the absorption layer material. On the other hand, this antireflection film is deposited at low temperature and low power, effectively reducing the bombardment of charged particles in the plasma on the absorption layer. While taking into account the wide bandgap and high transparency of the material, the optical reflection is reduced through the refractive index gradient structure, so it becomes an ideal choice for the antireflection film of silicon-based tandem cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and particularly relates to the preparation of an anti-reflection film with a gradient refractive index characteristic and its application in silicon-based laminated solar cells. Background Art

[0002] Silicon-based tandem solar cells have attracted the attention of many researchers due to their higher conversion efficiency, especially III-V / Si and perovskite / Si tandem cells. The former has the advantages of stability and high efficiency, while the latter has the advantages of low cost and simple process. 0.51 In 0.49 P / Ga 0.93 In 0.07 As 0.87 P 0.13 / / The efficiency of Si tandem cells is 35.9%, and the highest efficiency of two-terminal perovskite tandem cells is 29.5%. Among them, the main factors limiting efficiency include optical loss, non-radiative recombination, and contact resistance. Optical loss can be effectively reduced by anti-reflection film. Since 1817, when the Fraunhofer Laboratory in Germany prepared the first batch of anti-reflection films, different types of anti-reflection films, including single-layer, double-layer, and triple-layer anti-reflection film combinations, have been widely studied. Among them, high-refractive index anti-reflection films include ZnS (n=2.37, 587nm), TiO 2 (n = 2.61, 587nm), Ta 2 O 5 (n = 2.13, 587nm), CeO 2 (n = 2.2, 587nm), etc., low refractive index anti-reflection films include MgF 2 (n = 1.38, 587nm), Al 2 O 3 (n = 1.77, 587nm), SiO 2 (n=1.46, 587nm), LiF (n=1.39, 587nm), PDMS (n=1.4, 587nm), etc. In order to improve the effect of anti-reflection film, researchers combine high refractive index materials with low refractive index materials to form a double-layer anti-reflection film, such as MgF 2 / ZnS、MgF 2 / Ta 2 O 5 、Al 2 O 3 / TiO 2 MgF 2 / TiO 2 However, the double-layer anti-reflection film has a good anti-reflection effect only in special bands, such as MgF 2The / ZnS antireflection film can reduce the reflection loss of the battery to 1.6% within the wavelength range of 300 - 650 nm. The antireflection effect is not good in the range of 650 - 1200 nm. Moreover, the double-layer antireflection film increases the process difficulty, and the selection of the absorber layer material and its thickness change window are relatively narrow. From the currently published results, all silicon-based tandem solar cells use single-layer or double-layer antireflection films, which will cause partial sunlight to be reflected at the interface,不利于 the absorption of the tandem cell and result in a low cell efficiency at the same time.

[0003] In summary, the deficiencies of the antireflection film in the existing silicon-based tandem solar cells can be summarized as follows: 1) For single-layer or double-layer antireflection films, the antireflection effect is not good, especially in the long-wavelength range of 800 - 1200 nm, the absorption of the tandem cell becomes worse, leading to a low current. 2) The current antireflection film is sensitive to the selection of the absorber layer material and its thickness, is relatively dependent on the incident angle of sunlight, has a narrow application window, is not conducive to improving the cell efficiency, and limits the practical application of the cell. Summary of the Invention

[0004] The object of the present invention is to overcome the above deficiencies of the prior art, and propose a preparation of an antireflection film based on the refractive index gradient characteristic and its application in a silicon-based tandem solar cell. By adjusting the CO 2 flow rate in the reaction gas to adjust the ratio of Si and O in nc-SiOx:H, that is, the x value, to achieve the gradient change of the refractive index, where 0 < x ≤ 2. This antireflection film effectively reduces the reflection loss on the front surface of the tandem cell and improves the cell efficiency.

[0005] The technical solution of the present invention:

[0006] A preparation method of an antireflection film with refractive index gradient characteristics, the method comprising:

[0007] 1) Place the silicon-based tandem solar cell sample in a high-vacuum deposition equipment, with the surface temperature being 50 - 300 °C, the background vacuum degree being 10 -5 -10 -9 Pa, introduce the reaction gas, the pressure of the reaction gas being 0.5 - 5 Torr, and glow-deposit the nc-SiOx:H antireflection film under the condition that the glow power density is 0.01 - 0.1 W / cm 2 condition.

[0008] 2) Introduce the CO 2 flow rate in the reaction gas according to: G(t) = G 0 + At, where G(t) is the CO 2 flow rate, G 0 is the initial CO 2 flow rate, A is the linear change rate, and t is the glow time. CO 2The flow rate gradually increases from 1 sccm to 50 sccm.

[0009] 3) Finally, the thickness of the single-layer antireflection film deposited by glow discharge is 2 - 20 nm, and the total thickness of the multi-layer nc-SiOx:H antireflection film is 20 - 200 nm, where 0 < x ≤ 2. The refractive index changes gradually in the longitudinal direction of the film, and the change range is 4 - 1.5 at a wavelength of 600 nm.

[0010] Among them, the reaction gas includes: the source gas is silane such as SiH 4 , Si 2 H 6 or Si 3 H 8 ; the dilution gas is H 2 , He or Ar; the doping gas is CO 2 , PH 3 , B 2 H 6 or B(CH 3 ) 3 ; the flow rate ratio of the dilution gas to the source gas is 50 - 500∶1.

[0011] The deposition equipment is a plasma-enhanced chemical vapor deposition PECVD or hot wire chemical vapor deposition (HWCVD) equipment with a frequency of 13.56 MHz - 100 MHz. The nc-SiOx:H is p-type or n-type.

[0012] The stacked cell is a III-V group and crystalline silicon stacked solar cell, or a perovskite and crystalline silicon stacked solar cell. Among them, the light incident surface of the silicon-based stacked solar cell is a textured surface or a flat surface; the silicon-based stacked solar cell is a two-terminal stacked cell, a three-terminal stacked cell or a four-terminal stacked cell.

[0013] The III-V group top cell is a single-junction GaInP, AlGaAs, GaAs structure, or a two-junction GaInP / GaAs, GaInP / AlGaAs, GaInP / GaInAsP structure, or a three-junction AlGaInP / AlGaAs / GaAs, AlGaInP / GaInP / AlGaInAs structure, or a four-junction AlGaInP / GaInP / AlGaInAs / GaInAs, AlGaInP / GaInP / AlGaAs / GaAs structure.

[0014] The perovskite top cell is an organic-inorganic hybrid perovskite cell with a band gap of 1.6 - 2.1 eV, or an all-inorganic perovskite cell.

[0015] The silicon bottom cell of the silicon-based tandem solar cell is a HJT cell, a TOP-Con cell, a POLO cell, a DASH cell, a PERC cell, a PERL cell or a PERT cell.

[0016] Mechanism analysis of the present invention:

[0017] When light propagates in a medium, the refractive index n is generally used to quantify the speed of light in the current medium relative to the speed of light in a vacuum. When light enters a medium with a small refractive index from a medium with a large refractive index, obvious interface reflection will occur. Therefore, in solar cells, a low-refractive-index transparent film is generally used as an anti-reflection film. In theory, the anti-reflection effect is best when the square of the refractive index of the anti-reflection film is equal to the refractive index of the air multiplied by the refractive index of the window layer. However, the window layer of a silicon-based tandem cell is generally a single-element structure with a fixed and unique refractive index. When sunlight shines on the tandem cell, only light of a specific wavelength can achieve zero reflection at the interface. At this time, the relationship between the reflectivity and the wavelength of the reflected light is V-shaped, and the color neutrality is poor. This design uses an anti-reflection film of hydrogenated nanocrystalline silicon oxygen with a gradient refractive index to adjust the CO in the reaction gas. 2 The ratio of Si and O in nc-SiOx:H is adjusted by the flow rate, that is, the x value to achieve a gradient change in the refractive index. As the x value gradually increases, the refractive index decreases in turn, which solves the limitation that traditional anti-reflection films can only achieve single-wavelength anti-reflection. On the other hand, the anti-reflection film adopts low-temperature and low-power deposition, which effectively reduces the bombardment of charged particles in the plasma on the absorption layer. While taking into account the wide band gap and high transparency of the material, the refractive index gradient structure reduces optical reflection, making it an ideal choice for anti-reflection films for silicon-based laminated cells.

[0018] Advantages and positive effects of the present invention:

[0019] The present invention uses a gradient anti-reflection film of hydrogenated nanocrystalline silicon oxygen to adjust the CO 2 The ratio of Si and O in nc-SiOx:H is adjusted by the flow rate, that is, the value of x is taken to achieve a gradient change in the refractive index, thereby achieving effective anti-reflection in the full spectrum. Compared with the existing technology, this method has the following advantages: 1) It solves the dependence of traditional anti-reflection films on the incident angle of the solar spectrum and the thickness of the absorption layer material. 2) It can achieve effective anti-reflection in the full spectrum range, which is suitable for III-V / crystalline silicon stacked cells and perovskite / crystalline silicon stacked cells. 3) The anti-reflection film has high transparency and simple process, and is not only suitable for planar stacked cells, but also for velvet stacked cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a schematic diagram of an anti-reflection film with a gradient refractive index prepared based on a silicon-based laminated solar cell substrate.

[0021] Figure 2 It is a graph of the volt-ampere characteristic of a III-V group / Si stacked solar cell having a nc-SiOx:H (0.1≤x≤1.5) multilayer anti-reflection film with a refractive index gradient characteristic according to a specific embodiment of the present invention.

[0022] Figure 3 It is a graph of the volt-ampere characteristic of a III-V group / Si stacked solar cell having a nc-SiOx:H (0.1≤x≤2) multilayer anti-reflection film with a gradient refractive index according to a specific embodiment of the present invention.

[0023] Figure 4 It is a graph of the volt-ampere characteristic of a perovskite / Si stacked solar cell having a nc-SiOx:H (1≤x≤1.8) multilayer anti-reflection film with a gradient refractive index according to a specific embodiment of the present invention.

[0024] Figure 5 It is a graph of the volt-ampere characteristic of a perovskite / Si stacked solar cell having a nc-SiOx:H (1≤x≤2) multilayer anti-reflection film with a gradient refractive index according to a specific embodiment of the present invention. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0026] Embodiment 1:

[0027] The III-V group / silicon heterojunction stacked solar cell used in the method of this embodiment includes, from top to bottom: (n)nc-SiOx:H (0.1≤x≤1.5) anti-reflection film, front metal grid electrode Au / Ag, GaAs contact layer, n-AlInP window layer, n-GaInP absorption layer, p-AlGaInP back field, tunnel junction, n-AlGaAs window layer, p-AlGaAs absorption layer, p-GaInP back field, p-GaAs contact layer, ITO connection layer, conductive adhesive, ITO connection layer, silicon heterojunction bottom cell electron selection layer na-Si:H, passivation layer ia-Si:H, silicon substrate n-Silicon, passivation layer ia-Si:H, hole selection layer pa-Si:H and back electrode Al.

[0028] In III-V / silicon heterojunction tandem solar cells, the band gap of the GaInP absorber is 1.91 eV, the band gap of the AlGaAs absorber is 1.51 eV, and the area is 2.2×2.2 cm 2 .

[0029] The anti-reflection film with a gradient refractive index characteristic of this embodiment is prepared by the following method:

[0030] 1. Place the III-V / silicon heterojunction tandem solar cell into the PECVD equipment. The surface temperature of the tandem solar cell is 300°C and the background vacuum is 1×10 -5 Pa, the reaction gas H 2 、SiH 4 , PH 3 The flow rates are 500, 5, and 8 sccm respectively, the reaction gas pressure is 0.5 Torr, and the glow power density is 0.1 W / cm 2 Glow deposition of nc-SiOx:H (0.1≤x≤1.5) anti-reflection film under the conditions;

[0031] 2. Remove CO from the reaction gas 2 The flow rate is: G(t) = 1 + 0.633t, where G(t) is CO 2 flow rate, t is the glow time. CO 2 The flow rate was gradually increased from 1 sccm to 20 sccm.

[0032] 3. The final glow deposition thickness is 200nm, and the refractive index of the nc-SiOx:H anti-reflection film increases from 4.2 to 1.6 in the longitudinal growth direction of the film at a wavelength of 600nm. The schematic diagram of the anti-reflection film with a gradient refractive index is shown in Figure 1 .

[0033] 4. ZnS / MgF ​​by electron beam evaporation 2 The thickness is 41 / 97nm as a comparison sample.

[0034] Experimental results: Conduct performance tests on solar cells, such as Figure 2 As shown, at AM1.5G, 100mW / cm 2 Under the irradiation of standard light intensity, the gradient nc-SiOx:H (0.1≤x≤1.5) anti-reflection film solar cell prepared in this embodiment has an open circuit voltage of 3.051V and a short circuit current density of 11.22mA / cm 2 , filling factor 79.54%, efficiency 27.2%. Traditional ZnS / MgF 2 The open circuit voltage of the anti-reflection film solar cell is 2.999V and the short circuit current density is 9.61mA / cm 2 , fill factor 79% and efficiency 22.77%.

[0035] Embodiment 2:

[0036] The III-V group / silicon heterojunction stacked solar cell used in the method of this embodiment includes, from top to bottom: (n)nc-SiOx:H (0.1≤x≤2) anti-reflection film, front metal grid electrode Au / Ag, GaAs contact layer, n-AlInP window layer, n-GaInP absorption layer, p-AlGaInP back field, tunnel junction, n-AlGaAs window layer, p-AlGaAs absorption layer, p-GaInP back field, p-GaAs contact layer, ITO connection layer, conductive adhesive, ITO connection layer, silicon heterojunction bottom cell electron selection layer na-Si:H, passivation layer ia-Si:H, silicon substrate n-Silicon, passivation layer ia-Si:H, hole selection layer pa-Si:H and back electrode Al.

[0037] In III-V / silicon heterojunction tandem solar cells, the band gap of the GaInP absorber is 1.91 eV, the band gap of the AlGaAs absorber is 1.51 eV, and the area is 2.2×2.2 cm 2 .

[0038] The anti-reflection film with a gradient refractive index characteristic of this embodiment is prepared by the following method:

[0039] 1. Place the III-V / silicon heterojunction stacked solar cell into the PECVD equipment. The surface temperature of the sample to be processed is 300°C and the background vacuum is 1×10 -5 Pa, the reaction gas H 2 、SiH 4 , PH 3 The flow rates are 500, 5, and 8 sccm respectively, the reaction gas pressure is 0.5 Torr, and the glow power density is 0.1 W / cm 2 Glow deposition of nc-SiOx:H (0.1≤x≤2) anti-reflection film under the conditions;

[0040] 2. Remove CO from the reaction gas 2 The flow rate is: G(t) = 1 + 0.9t, where G(t) is CO 2 flow rate, t is the glow time. CO 2 The flow rate was gradually increased from 1 sccm to 20 sccm.

[0041] 3. The final glow deposited thickness is 200nm, and the refractive index at 600nm wavelength increases from 4 to 1.5 in the longitudinal growth direction of the film. nc-SiOx:H anti-reflection film.

[0042] 4. ZnS / MgF ​​by electron beam evaporation 2 The thickness is 41 / 97nm as a comparison sample.

[0043] Experimental results: Conduct performance tests on solar cells, such as Figure 3 As shown, at AM1.5G, 100mW / cm 2 Under standard light intensity, the gradient nc-SiOx:H (0.1≤x≤2) anti-reflection film solar cell prepared in this embodiment has an open circuit voltage of 3.053V and a short circuit current density of 12.35mA / cm 2 , filling factor 73.26%, efficiency 27.62%. Traditional ZnS / MgF 2 The open circuit voltage of the anti-reflection film solar cell is 2.999V and the short circuit current density is 9.61mA / cm 2 , fill factor 79% and efficiency 22.77%.

[0044] Embodiment 3:

[0045] The perovskite / silicon heterojunction stacked solar cell used in the method of this embodiment includes, from top to bottom: (n)nc-SiOx:H (1≤x≤1.8) anti-reflection film, front metal grid electrode Ag, transparent conductive film IZO, intermediate protective layer SnO 2 , perovskite top cell electron transport layer PCBM, perovskite absorption layer Perovskite, perovskite hole transport layer PTAA, connection layer ITO, silicon heterojunction bottom cell electron selection layer na-Si:H, passivation layer ia-Si:H, silicon substrate n-Silicon, passivation layer ia-Si:H, hole selection layer pa-Si:H and back electrode Al.

[0046] In the perovskite / silicon heterojunction tandem solar cell, the perovskite absorber layer is a lead-tin mixed pin-type perovskite Cs with a band gap of about 1.68 eV prepared by solution deposition. 0.05 (FA 0.77 MA 0.23 ) 0.95 Pb(I 0.77 Br 0.23 ) 3 Cb x Sn 1-x (I y Br 1-y ) 3 .

[0047] The anti-reflection film with a gradient refractive index characteristic of this embodiment is prepared by the following method:

[0048] 1. Place the III-V / Si stacked battery into the PECVD equipment. The surface temperature of the sample to be processed is 300°C and the background vacuum is 1×10 -7 Pa, the reaction gas H 2 、SiH 4 , PH 3The flow rates are 500, 5, and 8 sccm respectively, the reaction gas pressure is 1 Torr, and the glow power density is 0.1 W / cm 2 Glow deposition of nc-SiOx:H (1≤x≤1.8) anti-reflection film under the conditions;

[0049] 2. Remove CO from the reaction gas 2 The flow rate is: G(t) = 10 + 0.633t, where G(t) is CO 2 flow rate, t is the glow time. CO 2 The flow rate was gradually increased from 10 sccm to 30 sccm.

[0050] 3. The final glow deposition thickness is 200nm, and the refractive index of the nc-SiOx:H anti-reflection film increases from 2.4 to 1.5 in the longitudinal growth direction of the film at a wavelength of 600nm. The schematic diagram of the anti-reflection film with a gradient refractive index is shown in Figure 1 . ZnS / MgF ​​by electron beam evaporation 2 The thickness is 41 / 97nm as a comparison sample.

[0051] Experimental results: Conduct performance tests on solar cells, such as Figure 4 As shown, at AM1.5G, 100mW / cm 2 Under standard light intensity, the gradient nc-SiOx:H anti-reflection film solar cell prepared in this embodiment has an open circuit voltage of 1.864V, a short circuit current density of 18.73mA / cm, a fill factor of 76.58%, and an efficiency of 26.75%. 2 The open circuit voltage of the anti-reflection film solar cell is 1.856V, and the short circuit current density is 17.91mA / cm 2 , fill factor 75.3% and efficiency 25.03%.

[0052] Embodiment 4:

[0053] The perovskite / silicon heterojunction stacked solar cell used in the method of this embodiment includes, from top to bottom: (n)nc-SiOx:H (1≤x≤2) antireflection film, front metal grid electrode Ag, transparent conductive film IZO, intermediate protective layer SnO 2 , perovskite top cell electron transport layer PCBM, perovskite absorption layer Perovskite, perovskite hole transport layer PTAA, connection layer ITO, silicon heterojunction bottom cell electron selection layer na-Si:H, passivation layer ia-Si:H, silicon substrate n-Silicon, passivation layer ia-Si:H, hole selection layer pa-Si:H and back electrode Al.

[0054] In the perovskite / silicon heterojunction tandem solar cell, the perovskite absorber layer is a lead-tin mixed pin-type perovskite Cs with a band gap of about 1.68 eV prepared by solution deposition. 0.05 (FA 0.77 MA 0.23 ) 0.95 Pb(I 0.77 Br 0.23 ) 3 Cb x Sn 1-x (I y Br 1-y ) 3 .

[0055] The anti-reflection film with a gradient refractive index characteristic of this embodiment is prepared by the following method:

[0056] 1. Place the perovskite / silicon tandem solar cell into the PECVD equipment. The surface temperature of the sample to be processed is 100°C and the background vacuum is 1×10 -7 Pa, the reaction gas H 2 、SiH 4 , PH 3 The flow rates are 500, 5, and 8 sccm respectively, the reaction gas pressure is 1 Torr, and the glow power density is 0.1 W / cm 2 Glow deposition of nc-SiOx:H (1≤x≤2) anti-reflection film under the conditions;

[0057] 2. Remove CO from the reaction gas 2 The flow rate is: G(t) = 12 + 0.633t, where G(t) is CO 2 flow rate, t is the glow time. CO 2 The flow rate was gradually increased from 12 sccm to 30 sccm.

[0058] 3. The final glow deposited thickness is 200nm, and the refractive index at 600nm wavelength increases from 2.2 to 1.5 in the longitudinal growth direction of the film. nc-SiOx:H anti-reflection film.

[0059] 4. Evaporation of MgF using an electron beam 2 The thickness of the sample is 80 nm as a comparison sample.

[0060] Experimental results: Conduct performance tests on solar cells, such as Figure 5 As shown, at AM1.5G, 100mW / cm 2 Under standard light intensity, the open circuit voltage of the gradient nc-SiOx:H anti-reflection film solar cell prepared in this embodiment is 1.863V and the short circuit current density is 19.27mA / cm 2, filling factor 75.77%, efficiency 27.26%. Traditional MgF 2 The open circuit voltage of the anti-reflection film solar cell is 1.856V, and the short circuit current density is 17.91mA / cm 2 , fill factor 75.3% and efficiency 25.03%.

[0061] In summary, the present invention adjusts the CO in the reaction gas 2 flow rate to adjust the ratio of Si and O in nc-SiOx:H, that is, the value of x (0

Claims

1. A method for preparing an anti-reflection film with a gradient refractive index, characterized in that: By adjusting the CO2 flow rate in the reaction gas to adjust the ratios of Si and O in nc-SiOx:H, i.e., the x value, to achieve a gradient change in the refractive index and realize effective antireflection in the full spectral range, the specific steps are as follows: 1) Place the silicon-based laminated solar cell sample in a high vacuum deposition device with a surface temperature of 50-300°C and a background vacuum of 10 -5 -10 -9 Pa, the reaction gas is introduced, the reaction gas pressure is 0.5-5Torr, and the glow power density is 0.01-0.1W / cm 2 Glow deposition of nc-SiOx:H anti-reflection film under conditions; 2) The CO2 flow rate in the reaction gas is introduced according to: G(t) = G0 + At, where G(t) is the CO2 flow rate, G0 is the initial CO2 flow rate, A is the linear change rate, and t is the glow time; the CO2 flow rate gradually increases from 1 sccm to 50 sccm; The reaction gas includes: the source gas is SiH4, Si2H6 or Si3H8 of silane type; the dilution gas is H2, He or Ar; the doping gas is CO2, PH3, B2H6 or B(CH3)3; the flow rate ratio of the dilution gas to the source gas is 50 - 500:1; 3) The final glow-deposited single-layer antireflection thin film has a thickness of 2 - 20 nm, and the total thickness of the multi-layer nc-SiOx:H antireflection film is 20 - 200 nm, where 0 < x ≤ 2; the refractive index changes progressively in the longitudinal direction of the thin film, and the change range at a wavelength of 600 nm is 4 - 1.

5.

2. The method for preparing an anti-reflection film with a gradient refractive index according to claim 1, characterized in that The deposition equipment is a plasma-enhanced chemical vapor deposition PECVD or hot wire chemical vapor deposition (HWCVD) equipment with a frequency of 13.56 MHz - 100 MHz.

3. The method for preparing an anti-reflection film with a gradient refractive index according to claim 1, characterized in that The nc-SiOx:H is p-type or n-type.

4. The method for preparing an anti-reflection film with a gradient refractive index characteristic according to claim 1, characterized in that: The stacked cell is a III-V / crystalline silicon stacked solar cell or a perovskite / crystalline silicon stacked solar cell.

5. The method for preparing an anti-reflection film with a gradient refractive index according to claim 1, characterized in that The light-incident surface of the silicon-based stacked solar cell is a textured surface or a planar surface.

6. The method for preparing an anti-reflection film with a gradient refractive index according to claim 1, characterized in that The silicon-based stacked solar cell is a two-terminal stacked cell, a three-terminal stacked cell or a four-terminal stacked cell.

7. The method for preparing an anti-reflection film with a gradient refractive index according to claim 4, characterized in that: The III-V top cell is a single-junction GaInP, AlGaAs, GaAs structure, or a two-junction GaInP / GaAs, GaInP / AlGaAs, GaInP / GaInAsP structure, or a three-junction AlGaInP / AlGaAs / GaAs, AlGaInP / GaInP / AlGaInAs structure, or a four-junction AlGaInP / GaInP / AlGaInAs / GaInAs, AlGaInP / GaInP / AlGaAs / GaAs structure.

8. The method for preparing an anti-reflection film with a gradient refractive index characteristic according to claim 4, characterized in that: The perovskite top cell is an organic-inorganic hybrid perovskite cell with a bandgap of 1.6 - 2.1 eV or an all-inorganic perovskite cell 9. The method for preparing an anti-reflection film with a gradient refractive index characteristic according to claim 1, characterized in that: The silicon bottom cell of the silicon-based stacked solar cell is an HJT cell, a TOP-Con cell, a POLO cell, a DASH cell, a PERC, a PERL or a PERT cell.

Citation Information

Patent Citations

  • Back reflector for silicon-based thin film solar cell and preparation method thereof

    CN101556971A

  • Broad Band Anti-Reflection Coating for Photovoltaic Devices and Other Devices

    US20150349147A1