UV conductive prepolymer and preparation method thereof, transparent conductive UV curing coating and preparation method thereof
By combining polythiophene groups and photo-curing units, UV conductive prepolymers are prepared, and nanosilver wires are added to solve the problem of poor cohesion properties of polythiophene coatings and achieve transparent conductivity with high transparency and excellent conductivity. UV curable coatings improve surface strength and stability and are suitable for plastic and glass surfaces.
Patent Information
- Application Number
- CN202111245966.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-25
AI Technical Summary
The existing polythiophene-based conductive coatings have poor cohesion properties, dissolution/melting properties, weather resistance and stable conductivity properties, resulting in low surface strength and easy wear and tear. The transparent conductive coatings are easy to fall off after long-term sunlight exposure, and The addition of non-conductive materials to the system reduces the overall conductivity.
Under the protection of inert gas, the resin prepolymer is prepared through the reaction of small molecule polyol and thiophene derivatives, and then reacts with the monomer, adding isocyanate and acrylate double bonds to form a UV conductive prepolymer, and passes through the nano silver wire Prepare transparent conductive UV curable coatings with photoinitiators and other components to improve the cross-linking strength and conductive properties of the coating.
It achieves high transparency and excellent conductive properties of the coating, improves surface strength and weather resistance, ensures the stability of the coating and is not easy to fall off, and improves the overall conductive performance through nano-silver wires, forming a product that can be commercially applied.
Smart Images

Figure BDA0003319872500000031 
Figure BDA0003319872500000032 
Figure BDA0003319872500000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of conductive polymer materials, and more specifically to a UV conductive prepolymer and a preparation method thereof, a transparent conductive UV curing coating and a preparation method thereof. Background Art
[0002] Conductive polymer materials such as polyaniline (PAN), polypyrrole (PPy) and polythiophene (PT) have great application prospects compared to traditional metal conductive materials due to their advantages of light weight, good ductility, easy processing and corrosion resistance. Conductive polymers, as a new type of optoelectronic material, have long been a hot topic of research at home and abroad, and have gradually achieved industrialization. They are widely used in dye-sensitized solar cells, electroluminescent materials, flexible transparent electrodes, conductive and antistatic coatings, etc.
[0003] Polythiophene has a structure similar to an aromatic ring, has good stability in the environment, and can maintain this stability in the doped state; different synthetic methods can be used to obtain polythiophene derivatives with different substitutions, thereby achieving different photoelectric properties. Therefore, polythiophene materials are the most widely studied and applied conductive polymer materials.
[0004] Among them, making polythiophene materials into coatings so that they can be coated on plastic films to make the insulating plastic surface conductive is an important research direction. However, the cohesive properties, dissolution / melting properties, weather resistance, and stable conductivity of polythiophene materials are relatively poor, which restricts their development in the direction of conductive coatings.
[0005] For example, patents CN 101389710 B and CN 101848962 B of SKC Co., Ltd. of South Korea disclose a method for preparing a transparent conductive coating based on a polythiophene system, which is prepared by mixing a polythiophene aqueous solution, aprotic polar solvents, alcohol solvents, melamine resins, adhesives, etc. Chinese patent CN 101665616 B uses a polythiophene aqueous solution, polar solvents, alcohol solvents, film-forming resins, coupling agents, surfactants, etc. to mix and prepare a conductive coating.
[0006] The above technologies all use polythiophene aqueous solution as the basic material of conductive coatings, and can achieve the conductivity and transparency of coatings, meeting some needs. Its disadvantages are low surface strength, easy wear, poor weather resistance and poor performance in maintaining stable conductivity. The possible reason is that polythiophene itself is a polymer with very poor cohesive strength. In order to simply meet the transparency, the above technology uses a water-based system, and the multiple components are simply mixed, which sacrifices some of the strength properties of the coating resin, making the coating surface weak and easy to wear. The coating is easy to fall off after long-term sunlight exposure. In addition, a large amount of non-conductive materials are added to the system, which reduces the overall conductivity of the coating. Therefore, transparent conductive coatings use water-based polythiophene systems, which can be used as permanent antistatic coatings, but there is still a certain gap from transparent conductive coatings that truly meet the needs of commercial applications. Summary of the invention
[0007] In order to overcome the defects of the prior art, the present invention provides a UV conductive prepolymer and a preparation method thereof, a transparent conductive UV curing coating and a preparation method thereof.
[0008] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a UV conductive prepolymer, comprising the steps of:
[0009] (1) Under the protection of an inert gas, in the presence of a solvent and a catalyst, a small molecule polyol and a thiophene derivative having a carboxyl unit at the ortho or meta position are reacted to prepare a resin prepolymer;
[0010] (2) reacting the resin prepolymer with the monomer in the presence of a catalyst, an inhibitor and a solvent to obtain a UV conductive prepolymer,
[0011] The monomer contains isocyanate at one end and acrylate double bond at the other end.
[0012] Preferably, the small molecule polyol is selected from at least one of ethylene glycol, glycerol, trimethylolpropane, trimethylolethane and pentaerythritol.
[0013] Preferably, the thiophene derivative is selected from any one of 2-thiophenecarboxylic acid, 3-methyl-2-thiophenecarboxylic acid, 3-thiophenecarboxylic acid and 3-thiopheneacetic acid.
[0014] Preferably, in step (1) and step (2), the solvent can be selected from at least one of ethyl acetate, toluene, butyl acetate, butanone, methyl isobutyl ketone and N-methylpyrrolidone.
[0015] Preferably, the inert gas in step (1) may be, but is not limited to, nitrogen or carbon dioxide.
[0016] Preferably, in step (1), the catalyst is selected from at least one of p-toluenesulfonic acid and tetrabutyl titanate;
[0017] In step (2), the catalyst is selected from an organic tin catalyst, specifically but not limited to dibutyltin dilaurate.
[0018] Preferably, the molar ratio of the amount of the organotin catalyst to the isocyanate in the monomer is 0.05-0.1%, and the molar ratio of the amount of the inhibitor to the acrylic acid double bond in the monomer is 0.1-0.5%.
[0019] Preferably, the monomer is selected from isocyanate ethyl acrylate or isocyanate ethyl methacrylate.
[0020] Preferably, the polymerization inhibitor is selected from p-hydroxyanisole or hydroquinone.
[0021] Specifically, the thiophene derivative is selected from 3-thiophenecarboxylic acid, the small molecule polyol is selected from ethylene glycol, and the monomer is selected from isocyanate ethyl methacrylate to prepare a UV conductive prepolymer, which is called compound 1, and the reaction principle is as follows:
[0022]
[0023] The small molecule polyol is selected from triol and tetraol, and the same synthesis steps are used to obtain compound 2 and compound 3, respectively, as follows:
[0024]
[0025]
[0026] When the monomer is selected from ethyl isocyanate acrylate, the same synthesis steps are used to obtain compound 4, compound 5, and compound 6, as follows:
[0027]
[0028] Wherein, R is the core of the polyol.
[0029] The second aspect of the present invention provides a UV conductive prepolymer, which is prepared by the above preparation method.
[0030] Preferably, the UV conductive prepolymer may be, but is not limited to, compounds 1-6.
[0031] The third aspect of the present invention provides a transparent conductive UV curing coating, the preparation raw materials include:
[0032]
[0033] Preferably, the UV active diluent is selected from monofunctional acrylate and multifunctional acrylate in a mass ratio of 1:1; wherein the monofunctional acrylate can be selected from at least one of hydroxyethyl methacrylate (HEMA) and isobornyl acrylate (IBOA), and the multifunctional acrylate can be selected from at least one of 1,6-hexanediol diacrylate (HDDA), trimethylolpropane triacrylate (TMPTA), and pentaerythritol triacrylate (PETA).
[0034] Preferably, the length of the silver nanowire is 5 to 30 μm and the diameter is 10 to 100 nm.
[0035] Preferably, the photoinitiator is at least one of 1173 photoinitiator, 184 photoinitiator, TPO photoinitiator, ITX photoinitiator, 907 photoinitiator, and 369 photoinitiator.
[0036] Preferably, the leveling agent is at least one of BYK-333, Tego-100, Deqian 810, and Efka-3883.
[0037] Preferably, the dispersant is at least one of BYK-105, Tego-710, Deqian 912, and Efka-4800.
[0038] Preferably, the solvent is at least one of ethyl acetate, butyl acetate, butanone and methyl isobutyl ketone.
[0039] A fourth aspect of the present invention provides a method for preparing a transparent conductive UV curing coating, comprising the steps of:
[0040] First, the nano silver wire and the dispersant are stirred and dispersed evenly in 10 to 30 parts of solvent, and then the photoinitiator is added and stirred to dissolve, and then the UV conductive prepolymer, UV active diluent and the remaining solvent are added and stirred evenly, and finally the leveling agent is added, stirred evenly, and filtered through a filter element to obtain a transparent conductive UV curing coating.
[0041] The beneficial effects of the present invention are:
[0042] (1) The UV conductive prepolymer of the present invention contains both polythiophene groups and photocurable photosensitive groups, which is conducive to the preparation of coatings by UV light curing. The coatings have good overall transparency and excellent conductive properties. The coatings can be applied on plastic films and glass to form conductive films and conductive glass, so that conductive polymer polythiophene materials can be truly applied to the market to form commercial products.
[0043] (2) UV conductive prepolymers enable UV light curing of coatings, which results in high cross-linking strength of the coatings, thereby improving the surface strength and cohesive strength of the conductive coatings. As a result, the coatings have the advantages of strong wear resistance and weather resistance, are not easy to fall off, and have good stability. In addition, the coatings have the advantages of fast curing speed, are easy to use, and have good adhesion to substrates such as metals, plastic films, and glass.
[0044] (3) One end of the monomer contains isocyanate and the other end contains an acrylate double bond, which greatly simplifies the preparation process and has a higher proportion of photocurable units, which is beneficial to the subsequent curing of the coating.
[0045] (4) Adding silver nanowires to the coating compensates for the effect of non-conductive materials in the system on the conductivity, improving the overall conductivity of the coating without reducing the overall transparency of the coating. The addition of silver nanowires also forms an organic / inorganic nanocomposite material system, thereby improving the strength of the coating.
[0046] (5) The coating production conditions are simple and mild, without using special high temperature environment or special high pressure conditions, with high production efficiency and low cost.
[0047] (6) The coating can be applied on plastic film and glass to make conductive film and conductive glass. DETAILED DESCRIPTION
[0048] The following examples are intended to illustrate the present invention rather than to limit the scope of protection of the claims of the present invention.
[0049] Example 1
[0050] A method for preparing a UV conductive prepolymer comprises the following steps:
[0051] (1) Under nitrogen protection, ethylene glycol and 3-thiophenecarboxylic acid were mixed in a reaction kettle at a molar ratio of 1:1, and stirred at room temperature.
[0052] Dissolve p-toluenesulfonic acid equivalent to 1-3% of the total mass of the reactants in N-methylpyrrolidone to prepare a catalyst solution with a concentration of 1%.
[0053] The catalyst solution is added dropwise to the reactor, and the addition is completed within 30 to 60 minutes. The temperature is then raised to 110 to 150°C, and the condensation reflux device is turned on. The reaction is stirred for 6 to 8 hours. During the reaction, the water generated by the condensation of the alcohol acid forms an azeotrope with the solvent. Through the condensation reflux process, the solvent evaporates and carries out the water. After the oil and water are separated by the water separator, the solvent flows back to the reactor. The reaction is completed, and the resin prepolymer is obtained.
[0054] Ethyl isocyanate methacrylate is added to the resin prepolymer in a molar ratio of 1:1. The reaction temperature is set at 70-80°C, and then an organic tin catalyst solution (concentration of 0.05%) and a p-hydroxyanisole solution (concentration of 1%) are added dropwise in sequence. The solvent is N-methylpyrrolidone, wherein the molar ratio of the organic tin catalyst to the isocyanate in the monomer is 0.05-0.1%, and the molar ratio of the inhibitor to the acrylic acid double bond in the monomer is 0.1-0.5%. The total dropping time is 3 hours, and the reaction is continued for 5-6 hours to obtain a UV conductive prepolymer, namely compound 1.
[0055] Example 2
[0056] This embodiment is the same as the embodiment 1, except that in this embodiment, the small molecule polyol is selected from glycerol to obtain a UV conductive prepolymer, namely compound 2. The rest is the same as the embodiment 1 and will not be described in detail here.
[0057] Example 3
[0058] This embodiment is the same as the embodiment 1, except that in this embodiment, the monomer is selected from ethyl isocyanate acrylate to prepare a UV conductive prepolymer, namely compound 4. The rest is the same as the embodiment 1 and will not be described in detail here.
[0059] Example 4
[0060] This embodiment is the same as the embodiment 1, except that in this embodiment, the small molecule polyol is selected from glycerol, the monomer is selected from ethyl isocyanate acrylate, and the UV conductive prepolymer is prepared, namely compound 5. The rest is the same as the embodiment 1 and will not be described in detail here.
[0061] Example 5
[0062] A transparent conductive UV curing coating, the preparation raw materials include:
[0063]
[0064] The UV-active diluent is selected from hydroxyethyl methacrylate (HEMA) and 1,6-hexanediol diacrylate (HDDA).
[0065] Embodiment 6-8
[0066] Examples 6-8 are basically the same as Example 5, except that the UV conductive prepolymers in Examples 6-8 are Compound 2, Compound 4 and Compound 5, respectively, and the rest are the same as Example 1 and will not be elaborated in detail here.
[0067] Comparative Example 1
[0068] A transparent conductive UV curing coating, the preparation raw materials include:
[0069]
[0070] The UV-active diluent is selected from hydroxyethyl methacrylate (HEMA) and 1,6-hexanediol diacrylate (HDDA).
[0071] Application test methods and results:
[0072] The coating was applied on a 50 μm thick PET film with a wire rod, dried in an oven at 120°C for 2 minutes to evaporate the solvent, and then exposed to UV light with a wavelength of 280 to 395 nm and a light energy of 300 to 600 mJ / cm 2 , the coating is completely cured to obtain a transparent conductive film, and relevant tests are carried out. The test results are shown in Table 1.
[0073] Electrical conductivity, the test standard is GB / T 11007-2008;
[0074] Sheet resistance, the test standard is GB / T 17473.3-2008;
[0075] Transmittance and haze, the test standard is GB / T 2410-2008;
[0076] Adhesion test, the test standard is GB / T 33049-2016.
[0077] Table 1 Test results
[0078]
[0079]
[0080] It can be seen from the test results in Table 1 that the UV conductive prepolymer of the technical solution of the present application can obtain a transparent conductive UV curing coating with good overall transparency, excellent conductive performance, stability and not easy to fall off.
[0081] From the data of comparative example 1, it can be seen that the introduction of nano silver wires in the technical solution of the present application can compensate for the influence of non-conductive materials in the system on the conductivity, improve the overall conductivity of the coating, and do not significantly reduce the overall transparency of the coating.
[0082] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any person with ordinary knowledge in the technical field can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a UV conductive prepolymer, characterized in that: Includes steps: (1) Under the protection of an inert gas, in the presence of a solvent and a catalyst, a small molecule polyol and a thiophene derivative having a carboxyl unit at the ortho or meta position are reacted to prepare a resin prepolymer; (2) reacting the resin prepolymer with the monomer in the presence of a catalyst, an inhibitor and a solvent to obtain a UV conductive prepolymer, Wherein, the small molecule polyol is selected from at least one of ethylene glycol, glycerol, trimethylolpropane, trimethylolethane, and pentaerythritol; The thiophene derivative is selected from any one of 2-thiophenecarboxylic acid, 3-methyl-2-thiophenecarboxylic acid, 3-thiophenecarboxylic acid, and 3-thiopheneacetic acid; The monomer is selected from isocyanate ethyl acrylate or isocyanate ethyl methacrylate; The inhibitor is selected from p-hydroxyanisole or hydroquinone; In step (1), the catalyst is selected from at least one of p-toluenesulfonic acid and tetrabutyl titanate; In step (2), the catalyst is selected from an organotin catalyst.
2. The method for preparing a UV conductive prepolymer according to claim 1, characterized in that: In step (1) and step (2), the solvent can be selected from at least one of ethyl acetate, toluene, butyl acetate, butanone, methyl isobutyl ketone and N-methylpyrrolidone.
3. A UV conductive prepolymer, characterized in that: The UV conductive prepolymer is prepared by the preparation method of any one of claims 1 to 2.
4. A transparent conductive UV curing coating, characterized in that: The raw materials for preparation include: 100 parts of the UV conductive prepolymer as claimed in claim 3; 10-30 parts of UV active diluent; 5. A method for preparing the transparent conductive UV curing coating as claimed in claim 4, comprising the steps of: First, the nano silver wire and the dispersant are stirred and dispersed uniformly in 10 to 30 parts of solvent, and then a photoinitiator is added and stirred to dissolve, and then the UV conductive prepolymer, UV active diluent and the remaining solvent according to claim 4 are added and stirred uniformly, and finally a leveling agent is added, stirred uniformly, and filtered through a filter element to obtain a transparent conductive UV curing coating.
Citation Information
Patent Citations
Composition of polythiophene-based conductive polymers having high conductivity, transparency, waterproof property and a membrane prepared using the same
CN101389710B
Liquid composition of polythienyl-based conducting polymer, conducting polymer film and application thereof
CN101665616B
Polythiophene-based conductive polymer membrane
CN101848962B
Preparation method of intrinsic photo-cured anti-static resin
CN103642383A
Method for preparing light-curing conductive coating
CN104629611A