A Ti-Al-C MAX phase coating and low temperature phase preparation method thereof
The Ti3AlC2 MAX phase coating is prepared at a lower temperature through high-power pulse magnetron sputtering technology, which solves the problem of high synthesis temperature of MAX phase materials, achieves phase preparation at a lower temperature, and improves the quality and quality of the coating. Application scope.
Patent Information
- Application Number
- CN202111175820.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-09
AI Technical Summary
MAX phase materials require higher temperatures during the synthesis process, which limits their application on temperature-sensitive substrates, especially the synthesis of higher-order 312 phases, resulting in a limited range of applications.
High-power pulse magnetron sputtering technology is used with a Ti-Al composite target as the sputtering target, hydrocarbon gas as the reactive gas source, and short pulses at a frequency of 500-1000Hz and a duty cycle of 5-10% to target the substrate. The surface is sputtered to form a TiAlx-C coating, and a Ti3AlC2 MAX phase coating is formed at a heat treatment temperature of 600-700°C.
It reduces the phase formation temperature of the Ti3AlC2 312 series MAX phase, improves the purity and bonding strength of the coating, makes the surface dense and smooth, and refines the particles, solving the temperature limitation problem of high-temperature preparation in traditional technology.
Smart Images

Figure CN113981392B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface treatment, and in particular to a low-temperature phase-forming preparation method of a Ti3AlC2 MAX phase coating. Background Art
[0002] MAX phase materials are a class of thermodynamically stable, layered, high-performance ceramic-metal materials with a close-packed hexagonal structure. n+1 AX n , where the M position is a transition metal element, including Ti, Cr, etc., the A position is usually an element of the third or fourth main group in the periodic table, such as Al, Si, etc., and the X position element is C or N, which can be understood as a metal carbide or metal nitride nanolayered compound divided by a single layer of A atoms. Generally speaking, MX is bonded by strong covalent bonds and ionic bonds, while MA relies on relatively weak metallic bonds. This unique layered structure and bonding method make the MAX phase have the excellent properties of both metals and ceramics, such as excellent mechanical stability, high hardness, good thermal shock tolerance, strong corrosion resistance and high temperature oxidation resistance, good electrical and thermal conductivity, as well as self-healing properties and machinability.
[0003] In the general formula M n+1 AX n In the formula, the n value indicates that the number of M atoms between every two layers of A atoms in the MAX phase crystal structure is n+1. Currently, the n values of most known MAX phase materials are 1, 2, and 3. According to the different n values, the MAX phase is divided into 211, 312, and 413 phases. Typical Al-containing MAX phase materials show significant high-temperature oxidation and corrosion resistance by forming a protective Al2O3 layer. In the most representative Ti-Al-C system and Cr-Al-C system, Ti-Al-C compounds have a thermal expansion coefficient similar to Al2O3, making them suitable protective coatings for substrates such as stainless steel, titanium alloys, and nickel-based high-temperature alloys.
[0004] However, due to the longer c-axis and complex crystal structure of MAX phase materials, a longer diffusion coefficient is required to distribute elements during the synthesis process, resulting in the synthesis of MAX phase being strongly dependent on temperature, and lower temperatures cannot meet the synthesis conditions, especially for the higher-order 312 and 413 phases, which have improved performance compared to the 211 phase, but also require higher synthesis temperatures. Common bulk preparation methods for Ti3AlC2 in the Ti-Al-C system, such as hot pressing and plasma sintering, have synthesis temperatures above 1200°C, while for coating film systems, due to the shorter diffusion length, the synthesis temperature can be reduced, but for magnetron sputtering and cathode arc plating in PVD, the main technologies for preparing MAX phase coatings, the synthesis temperature is also in the range of 800-1000°C.
[0005] The high preparation temperature of the MAX phase limits its application on temperature-sensitive substrates. How to lower the preparation temperature of the MAX phase, especially the synthesis of higher-order 312 phase, can expand its application range and is also one of the bottlenecks of the current MAX phase materials. Summary of the invention
[0006] The invention provides a low-temperature phase forming preparation method of a Ti-Al-C MAX phase coating. The method can prepare a Ti3AlC2 MAX phase coating at a relatively low temperature.
[0007] A low-temperature phase preparation method for a Ti3AlC2 MAX phase coating, comprising:
[0008] (1) Using Ti-Al composite target as sputtering target, hydrocarbon gas as reaction gas source, high power pulse magnetron sputtering technology, with a frequency of 500-1000 Hz, a duty cycle of 5-10%, and a short pulse of 100-200 μs, TiAl is sputtered on the substrate surface. x -C coating;
[0009] (2) Heat treatment of the TiAl x -C coating to obtain Ti3AlC2 MAX phase coating, the heat treatment temperature is 600-700℃.
[0010] The present invention adjusts the parameters of the high power pulsed magnetron sputtering (HiPIMS) technology so that HiPIMS provides sufficient energy to deposit TiAl x -C coating to form a Ti-C lattice, and then through the lower 600-700 ℃ heat treatment temperature, the TiAl x -C coating, Al ions diffuse into the Ti-C lattice to form a Ti3AlC2 MAX phase coating, so that the Ti3AlC2MAX phase coating can be obtained at a relatively low temperature. Compared with the prior art which requires a temperature above 900°C to form a complete Ti3AlC2312 phase and 413 phase MAX phase coating, the heat treatment temperature of the present invention is relatively low.
[0011] In step (1):
[0012] The Ti-Al element ratio of the Ti-Al composite target is 2:1.2-1.5.
[0013] The flow rate of the hydrocarbon gas is 5-10 sccm. Furthermore, the hydrocarbon gas is methane or acetylene.
[0014] In the above-mentioned method, TiAl is sputtered on the substrate surface to obtain x - Before C coating, the substrate is subjected to plasma glow etching to make the substrate surface cleaner.
[0015] Furthermore, the plasma is any one of argon and nitrogen.
[0016] Furthermore, the plasma glow etching parameters are: plasma flow rate is 30 to 35 sccm, ion source voltage is 1000 to 1200 V, substrate bias voltage is -250 to -150 V, and etching time is 20 to 40 min.
[0017] After the substrate is subjected to plasma glow etching treatment, the reaction source is turned off, the Ti-Al composite target is turned on, and a transition layer is sputtered on the surface of the substrate.
[0018] Furthermore, the transition layer is a TiAl compound.
[0019] The sputtering parameters are: sputtering power 1800-2400W, substrate bias voltage -100-0V.
[0020] Before sputtering a transition layer on the surface of the substrate, a protective gas is introduced, the flow rate of the protective gas is 150-250 sccm, and the chamber pressure is 0.6-1.2 Pa.
[0021] To avoid the substrate layer and TiAl x -C coating elements diffuse each other, so that the final Ti3AlC2 MAX phase coating contains other nanocrystalline particles, which affects the purity of the Ti3AlC2 MAX phase coating. In addition, the addition of the transition layer can make the thermal expansion coefficient between the coating and the substrate over-matched, so that the TiAl x -C coating has increased bonding strength.
[0022] In step (2), the heat treatment time is 60 to 180 minutes.
[0023] According to the low-temperature phase forming preparation method of a Ti-Al-C MAX phase coating, a Ti-Al-C MAX phase coating is prepared, and the thickness of the Ti-Al-C MAX phase coating is 2-4 μm.
[0024] Compared with the prior art, the advantages of the present invention include:
[0025] (1) The Ti-Al composite target is pulsed sputtered by a high-power pulsed magnetron sputtering HiPIMS power supply, which has a lower duty cycle and a higher target peak power density, thereby increasing the ionization rate of the target elements and the reaction gas and the plasma energy during the sputtering process, so that the Ti3AlC2 312 series MAX phase can be prepared at a lower heat treatment temperature in the subsequent process, thereby reducing the phase formation temperature (traditional 900-1200°C) required for preparing the Ti3AlC2 312 series MAX phase by conventional magnetron sputtering or cathode arc plating in the current PVD technology. The present invention generates a relatively pure Ti3AlC2 312 series MAX phase at 600-700°C, providing a reliable idea for the preparation of MAX phase coatings.
[0026] (2) High-power pulsed HiPIMS power sputtering deposition technology combines the advantages of traditional magnetron sputtering, low-temperature deposition, smooth surface, and no particle defects, and cathode arc ion plating, which has high metal ionization rate, strong film bonding, and dense coating. It also improves the problem of target poisoning and arcing, so that there is no particle accumulation on the surface of the prepared coating, the particles are finer, the surface is denser and smoother, and the roughness is as low as 15-19nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is the discharge characteristic of the high power pulsed magnetron sputtering HiPIMS power supply in the coating preparation of the present invention.
[0028] Figure 2 1 and 2 are XRD spectra of the Ti-Al-C MAX phase coatings in the deposited state and the annealed state obtained in Example 1 of the present invention and Comparative Example 1.
[0029] Figure 3 This is a surface morphology of the Ti-Al-C MAX phase coating prepared in Example 1 of the present invention.
[0030] Figure 4 It is a surface morphology picture of the Ti-Al-C MAX phase coating prepared in Comparative Example 1 of the present invention.
[0031] Figure 5 1 and 2 are XRD spectra of the Ti-Al-C MAX phase coatings in the deposited state and the annealed state obtained in Example 2 of the present invention and Comparative Example 2.
[0032] Figure 6 This is a surface morphology of the Ti-Al-C MAX phase coating prepared in Example 2 of the present invention.
[0033] Figure 7 This is a surface morphology of the Ti-Al-C MAX phase coating prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0034] Embodiment 1:
[0035] In this embodiment, the substrate material is 1Cr11Ni2W2MoV stainless steel, and the specific preparation steps of the Ti3AlC2 MAX phase coating on the substrate surface are as follows:
[0036] Step 1: Use 400#~2000# SiC sandpaper to grind the surface of 1Cr11Ni2W2MoV stainless steel in turn, and then use diamond grinding paste to polish for 20 minutes;
[0037] Step 2: Place the ground and polished 1Cr11Ni2W2MoV stainless steel substrate in acetone for ultrasonic cleaning for 10 minutes, then blow dry with cold air and stick it on the sample holder with conductive glue for later use.
[0038] Step 3: Place the sample holder with the substrate attached in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 3×10 -5 Pa, set the chamber temperature to 100°C, introduce 34 sccm of high-purity argon into the vacuum chamber, set the linear anode ion source current to 0.2A, and the substrate bias to -200V, and etch and clean the surface of the 1Cr11Ni2W2MoV stainless steel substrate for 30 minutes.
[0039] Step 4: The deposition conditions of the Ti-Al transition layer are the same as those in step 5, except that the gases introduced are different. Instead of hydrocarbon reaction gases, 200 sccm of high-purity argon gas is introduced into the deposition of the transition layer.
[0040] Step 5: TiAl is deposited using high power pulsed HiPIMS technology x -C coating, 200sccm of high-purity argon gas and 7.5sccm of high-purity methane reaction gas were introduced. The sputtering target was a composite target with a Ti:Al ratio of 2:1.5. The sputtering source HiPIMS power supply was set to a frequency of 500Hz, a period of 2000μs, a duty cycle of 5%, and a pulse time of 100μs. The power was set to a constant of 2000W during the deposition process. The discharge characteristics during the deposition process are as follows Figure 1 As shown, the substrate bias voltage is 0 V, the chamber pressure is 1 Pa, and the deposition time is 120 min.
[0041] Step 6: The deposited TiAl x -C coating is placed in an annealing furnace with a vacuum degree of less than 2×10 -3 Pa, kept at 700℃ for 90min, and Ti3AlC2 MAX phase was obtained.
[0042] Comparative Example 1:
[0043] This embodiment is a comparative embodiment of the above-mentioned embodiment 1.
[0044] In this embodiment, the substrate is exactly the same as in Example 1, and the substrate pretreatment and surface argon ion glow etching are also exactly the same. The difference is that in step (4) and step (5), the Ti-Al transition layer and the TiAl x The deposition of the -C coating adopts the conventional DC magnetron sputtering technology instead of HiPIMS high power pulsed magnetron sputtering, and the DC sputtering source is also set to a constant power of 2000 W during the deposition process. The subsequent heat treatment conditions are also the same as those in Example 1.
[0045] Figure 2 The X-ray diffraction spectra of the coatings prepared in the above-mentioned Example 1 and Comparative Example 1 are as deposited and annealed. Figure 2 It can be seen that the composition of the deposited coating obtained by HiPIMS high-power pulsed magnetron sputtering is TiAl x Compounds, while the deposited coating obtained by DC magnetron sputtering in the comparative example is amorphous. Afterwards, at the same annealing temperature, only the HiPIMS high-power pulsed magnetron sputtering technology obtained the Ti3AlC2 312 series MAX phase during the heat treatment at 700°C, while the comparative DC magnetron sputtering technology only generated the Ti2AlC 211 series MAX phase. There are also some peaks from the substrate and the transition layer in the XRD spectrum.
[0046] Figure 3 and Figure 4 These are the surface morphology pictures of the coatings prepared in the above-mentioned Example 1 and Comparative Example 1 respectively. The coating prepared by HiPIMS high-power pulsed magnetron sputtering has a denser and smoother surface and finer particles than the coating prepared by DC magnetron sputtering.
[0047] Embodiment 2:
[0048] In this embodiment, the substrate material is TC4 titanium alloy, and the specific preparation steps of the Ti3AlC2 MAX phase coating on the substrate surface are as follows:
[0049] Step 1: Use 400#~2000# SiC sandpaper to grind the surface of TC4 titanium alloy in sequence, and then use diamond grinding paste to polish for 20 minutes;
[0050] Step 2: Place the ground and polished TC4 titanium alloy substrate in acetone for ultrasonic cleaning for 10 minutes, then blow dry with cold air and stick it on the sample holder with conductive glue for later use.
[0051] Step 3: Place the sample holder with the substrate attached in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 3×10 -5Pa, set the chamber temperature to 100°C, introduce 34 sccm of high-purity argon into the vacuum chamber, set the linear anode ion source current to 0.2A, and the substrate bias to -200V, and etch and clean the surface of the TC4 titanium alloy substrate for 30 minutes.
[0052] Step 4: The deposition conditions of the Ti-Al transition layer are the same as those in step 5. The difference is that the gases introduced are different. No hydrocarbon reaction gas is introduced into the deposition of the transition layer, but only 200 sccm of high-purity argon gas is introduced.
[0053] Step 5: TiAl is deposited using high power pulsed HiPIMS technology x -C coating, 200sccm of high-purity argon gas and 7.5sccm of high-purity methane reaction gas were introduced. The sputtering target was a composite target with a Ti:Al ratio of 2:1.5. The sputtering source HiPIMS power supply was set to a frequency of 500Hz, a period of 2000μs, a duty cycle of 5%, and a pulse time of 100μs. The power was set to a constant of 2000W during the deposition process. The discharge characteristics during the deposition process are as follows Figure 1 As shown, the substrate bias voltage is 0 V, the chamber pressure is 1 Pa, and the deposition time is 120 min.
[0054] Step 6: The deposited TiAl x -C coating is placed in an annealing furnace with a vacuum degree of less than 2×10 -3 Pa, kept at 700℃ for 90min, and Ti3AlC2 MAX phase was obtained.
[0055] Comparative Example 2:
[0056] This embodiment is a comparative embodiment of the above-mentioned embodiment 2.
[0057] In this embodiment, the substrate is exactly the same as in Example 2, and the substrate pretreatment and surface argon ion glow etching are also exactly the same. The difference is that in step (4) and step (5), the Ti-Al transition layer and the TiAl x The deposition of the -C coating adopts the conventional DC magnetron sputtering technology instead of HiPIMS high power pulsed magnetron sputtering, and the DC sputtering source is also set to a constant power of 2000 W during the deposition process. The subsequent heat treatment conditions are also the same as those in Example 2.
[0058] Figure 5 The X-ray diffraction spectra of the coatings prepared in the above-mentioned Example 2 and Comparative Example 2 are as deposited and annealed. Figure 5 It can be seen that the coating deposited by HiPIMS high-power pulsed magnetron sputtering is composed of titanium-aluminum compound TiAl, which is different from the amorphous coating deposited by DC magnetron sputtering. xIn the subsequent annealing process, only the HiPIMS high-power pulsed magnetron sputtering technology obtained the Ti3AlC2 312 series MAX phase during the heat treatment at 700°C, while the comparative DC magnetron sputtering technology only generated the Ti2AlC 211 series MAX phase. There are also some peaks from the matrix and the transition layer in the XRD spectrum.
[0059] Figure 6 and Figure 7 The surface morphology pictures of the coatings prepared in the above-mentioned Example 2 and Comparative Example 2 respectively show that the coating prepared by DC magnetron sputtering has hill features composed of aggregated spherical particles, while the coating prepared by HiPIMS high-power pulsed magnetron sputtering has significantly improved this agglomeration phenomenon, the coating surface particles are refined, the coating is denser, and the surface is smoother.
[0060] In addition, the inventors also conducted experiments with other matrix materials and conditions listed in this specification with reference to the methods of Examples 1 and 2, and obtained the same results.
[0061] In summary, the HiPIMS high-power pulsed magnetron sputtering technology can reduce the phase formation temperature of the Ti3AlC2 312 series MAX phase, and the quality of the prepared coating is better.
[0062] The above embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the above embodiments.
Claims
1. A low temperature phase preparation method for a Ti3AlC2 MAX phase coating, characterized in that: include: (1) Using Ti-Al composite target as sputtering target, hydrocarbon gas as reaction gas source, high power pulse magnetron sputtering technology, with a frequency of 500-1000 Hz, a duty cycle of 5-10%, and a short pulse of 100-200 μs, TiAl is sputtered on the substrate surface. x -C coating; (2) Heat treatment of the TiAl x -C coating to obtain Ti3AlC2 MAX phase coating, the heat treatment temperature is 600-700°C; The Ti-Al element ratio of the Ti-Al composite target is 2:1.2-1.5; In the above method, TiAl is sputtered on the substrate surface to obtain x - Before C coating, the substrate is subjected to plasma glow etching treatment; After the substrate is subjected to plasma glow etching treatment, the reaction gas source is turned off, the Ti-Al composite target is turned on, and a transition layer is sputtered on the surface of the substrate; The transition layer is a TiAl compound.
2. The low temperature phase forming preparation method of the Ti3AlC2 MAX phase coating according to claim 1, characterized in that: The flow rate of the hydrocarbon gas is 5-10 sccm.
3. The low temperature phase forming preparation method of the Ti3AlC2 MAX phase coating according to claim 1, characterized in that: The plasma is argon or nitrogen.
4. The low temperature phase forming preparation method of the Ti3AlC2 MAX phase coating according to claim 1, characterized in that: The plasma glow etching parameters are: plasma flow rate is 30-35sccm, ion source voltage is 1000-1200V, substrate bias voltage is -250--150V, and etching time is 20-40min.
5. The low temperature phase forming preparation method of the Ti3AlC2 MAX phase coating according to claim 1, characterized in that: The sputtering parameters are: sputtering power is 1800-2400W, and substrate bias is -100-0V.