A chip MOS tube wire welding method
By using thin copper wires instead of thick aluminum wires on the chip mos tubes, and adding guide tubes to the copper wire machine for straightening and softening treatment, the problem of high defective products in the existing technology is solved, and the defective products are achieved rate reduction and energy consumption optimization.
Patent Information
- Application Number
- CN202111295071.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-11-03
AI Technical Summary
The existing chip mos tube wire welding method has the problem of high defect rate, mainly because the welding area of the control electrode is too small, resulting in the aluminum wire welding exceeding the range, and the existing copper wire machine is insufficiently straightened and softened, resulting in the copper wire end Head shift and oxidation increase the defective rate.
Copper wire with a diameter of 35-38um is used instead of aluminum wire with a diameter of 300um is welded on the control electrode, and a guide tube is added to the copper wire machine for straightening and softening treatment. The copper wire stress is eliminated through the heating unit, avoid oxidation, and nitrogen is passed. Protect to prevent copper wire from oxidizing.
It significantly reduces the defective yield rate, improves the product yield rate, and reduces energy consumption, achieving the advantages of low defective yield rate and low energy consumption.
Smart Images

Figure CN114005764B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chip MOS tubes, and in particular relates to a chip MOS tube wire welding method. Background Art
[0002] like Figure 1 As shown, Figure 1 In the figure, S is the control electrode, G is the emitter electrode, and there are two copper wires in the chip MOS tube, one of which is welded on the emitter electrode of the chip. The current wire welding method is to use an aluminum wire machine to weld two aluminum wires on the emitter and the control electrode respectively. One wire on the emitter electrode is two aluminum wires with a diameter of 300um, and the other wire on the control electrode is an aluminum wire with a diameter of 300um. This is an inherent welding method in the industry and has been used for many years. However, it is found in actual use that the defective rate of the welded product is high. Therefore, the existing wire welding method has the defect of a high defective rate. Summary of the invention
[0003] The object of the present invention is to provide a chip MOS tube wire welding method. The present invention has the advantages of low defective rate and low energy consumption.
[0004] The technical solution of the present invention is a chip MOS tube wire welding method, which uses an aluminum wire machine to weld two aluminum wires with a diameter of 280-320um on the emitter of the chip MOS tube, and uses a copper wire machine to weld a copper wire with a diameter of 35-38um on the control electrode of the chip MOS tube.
[0005] In the aforementioned chip MOS tube wire welding method, the diameter of the aluminum wire is 300um, and the diameter of the copper wire is 38um.
[0006] In the aforementioned chip MOS tube wire welding method, the end of the copper wire is straightened.
[0007] In the aforementioned chip MOS tube wire welding method, the device used for the straightening and softening treatment includes a guide tube, a plurality of air holes are provided on the outer peripheral surface of the guide tube, an air pipe is provided on the outside of the guide tube, baffles are provided at both ends of the air pipe, a cavity is formed between the air pipe and the guide tube through the baffle, a heating unit that is in contact with the guide tube is provided in the cavity, a pipe joint connected to the air pipe is provided on one side of the heating unit, and the pipe joint is connected to the nitrogen tank through an air valve.
[0008] In the aforementioned chip MOS tube wire welding method, one end of the guide tube extends out of the air pipe.
[0009] Compared with the prior art, the present invention has found through repeated research and experiments that the main reason for the high defective rate of products is that the welding area of the control electrode is too small, which is only slightly larger than the diameter of the aluminum wire. When the aluminum wire is welded to the control electrode, the end of the aluminum wire is expanded into a pancake shape by ultrasonic extrusion, which can easily exceed the welding area range, which may cause damage to the adjacent circuit, and the control electrode and the adjacent circuit may be short-circuited, resulting in a low yield rate. However, this welding range cannot be directly observed and can only be discovered with the help of a microscope. The phenomenon of the control electrode welding range has not been noticed. In addition, the control electrode welding range is not the only reason for product defects. When inspecting defective products, the defective cause is often attributed to other factors, which also causes the problem of defective products caused by the control electrode welding range to be covered up.
[0010] Based on the above-discovered causes of defective products, combined with the current distribution analysis on the chip MOS tube, it is found that the current passing through the control electrode is much smaller than the current passing through the emitter, and there is no need to use an aluminum wire with a diameter of 300um. Copper wire with a diameter of more than 35um can fully meet the current of the control electrode. Therefore, the present invention uses thin copper wire instead of thick aluminum wire as the conductor on the control electrode, and uses the existing copper wire machine to weld the copper wire to the control electrode. Since the copper wire is thin, it is not easy to weld out of range when welding the copper wire to the control electrode, it is not easy to damage the product, and the defective rate is low.
[0011] In addition, the present invention adds a device for straightening and softening the copper wire on the existing copper wire machine, further reducing the defective rate of the product. The working principle of the existing copper wire machine is to use a coiled copper wire, one end of the copper wire is led to the control electrode, and after welding, it is cut to form a copper wire as a conductor on the control electrode, and then continue to lead, weld, and cut, and the cycle is carried out. The applicant found that due to the different inner diameters and curvatures of the inner and outer circles of the copper wire, the degree of warping of the ends formed after the copper wire is continuously led out and cut is different, and it is difficult to ensure that all the ends are aligned with the control electrode. When the copper wire machine is debugged before production, it can only ensure that the current copper wire end is aligned with the center position of the control electrode. In subsequent production, the newly generated end will gradually deviate from the center of the control electrode, and there is a certain possibility that it will deviate from the welding area of the control electrode (whether it deviates depends on the difference in diameter between the inner and outer circles of the coiled copper wire. The greater the winding thickness, the easier it is to deviate), resulting in an increase in the defective rate. The present invention utilizes a guide tube to straighten the copper wire so that the curvatures of the copper wire at various positions after passing through the guide tube are close or even the same. A heating unit in the guide tube is utilized to eliminate stress on the copper wire to prevent the copper wire from rebounding, thereby ensuring that all ends can be aligned with the center position of the control electrode without deviation, so that welding is not likely to exceed the range and the product yield is high.
[0012] Furthermore, the present invention reduces the heat loss of the heating unit and reduces energy consumption by arranging an air pipe and a baffle on the outside of the guide pipe. Nitrogen is passed into the air pipe through a nitrogen tank, and the nitrogen flow rate is controlled by a gas valve to ensure that nitrogen flows out from both ends of the guide pipe, ensuring that the heated part of the copper wire does not contact with oxygen, avoiding oxidation of the copper wire, and ensuring that the copper wire has good conductivity, which also ensures a high yield rate of the product. According to statistics, the present invention can reduce the defective rate to about 60% of the original level.
[0013] Therefore, the present invention has the advantages of low defective product rate and low energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a schematic diagram of the welding of wires on chip MOS tubes.
[0015] Figure 2 It is a front view of the device.
[0016] The markings in the accompanying drawings are: 1-aluminum wire, 2-copper wire, 3-guide tube, 4-air hole, 5-air pipe, 6-baffle, 7-cavity, 8-heating unit, 9-pipe joint, 10-air valve, 11-nitrogen tank. DETAILED DESCRIPTION
[0017] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0018] Embodiment. A method for welding a chip MOS tube wire, the chip name is PW11N70A, such as Figure 1 As shown, two aluminum wires 1 with a diameter of 300um are welded to the emitter of the chip MOS tube using an aluminum wire 1 machine ( Figure 1 A copper wire 2 with a diameter of 38um is welded to the control electrode ( Figure 1 (shown in G).
[0019] The ends of the copper wires 2 are straightened and softened.
[0020] like Figure 2 As shown, the device used for the straightening and softening treatment includes a guide tube 3, a plurality of air holes 4 are provided on the outer peripheral surface of the guide tube 3, an air pipe 5 is provided on the outer side of the guide tube 3, baffles 6 are provided at both ends of the air pipe 5, a cavity 7 is formed between the air pipe 5 and the guide tube 3 through the baffles 6, a heating unit 8 of electric heating wire type fitted with the guide tube 3 is provided in the cavity 7, a pipe joint 9 connected to the air pipe 5 is provided on one side of the heating unit 8, and the pipe joint 9 is connected to the nitrogen tank 11 through the air valve 10. The air pipe 5 and the guide tube 3 are both made of martensitic stainless steel.
[0021] One end of the guide tube 3 extends out of the air pipe 5, and the extended portion is used to continue to guide the copper wire and increase the cooling speed of the copper wire.
[0022] The structure of the existing copper wire machine mainly includes a wire feeding mechanism, a guide tube, a shearing mechanism, an ultrasonic mechanism, an amplitude transformer and a porcelain nozzle. The wire feeding mechanism is responsible for the forward movement of the copper wire, so that the end of the copper wire passes through the guide tube. The guide tube points to the welding area, so that the copper wire arrives at the welding area after coming out of the guide tube. The ultrasonic mechanism generates ultrasonic energy, and the ultrasonic energy is gathered at the porcelain nozzle through the amplitude transformer. After the porcelain nozzle is pressed down, the end of the copper wire is driven by the porcelain nozzle to vibrate at a high frequency and weld with the control electrode. Then the copper wire is cut by the shearing mechanism, that is, a welded copper wire 2 is formed on the control electrode.
[0023] During use of the existing copper wire machine, it was found that since the copper wire is installed in a coiled shape on the copper wire machine, there is actual stress on the copper wire after it is unfolded under the action of the wire feeding mechanism, and it recovers its bending after extending out of the guide tube. As the copper wire coil is consumed layer by layer, the curvature of the unfolded copper wire gradually changes, which makes it difficult for the copper wire coming out of the guide tube to accurately reach the welding area every time.
[0024] In order to ensure that the copper wire can accurately reach the welding area every time, the present invention adds a device to the existing copper wire machine. The device is fixed between the wire feeding mechanism and the guide tube, close to the guide tube, and is used to eliminate the stress of the copper wire, keep the copper wire straight, and make the copper wire controllable.
[0025] The copper wire coming out of the wire feeding mechanism passes through the guide tube 3 and then enters the guide tube. The heating unit 8 heats the copper wire to 500-600°C to eliminate the stress of the copper wire. The gas valve 10 is opened to allow the nitrogen in the nitrogen tank 11 to enter the cavity 7. The nitrogen speed is adjusted through the gas valve 10, and the nitrogen is required to be discharged from both ends of the guide tube 3 to avoid the presence of oxygen in the guide tube and the oxidation of the copper wire.
Claims
1. A method for welding wires of a chip MOS tube, using an aluminum wire machine to weld two aluminum wires (1) with a diameter of 280-320um on the emitter of the chip MOS tube, characterized in that: A copper wire (2) with a diameter of 35-38 μm is welded to the control electrode of the chip MOS tube by using a copper wire machine; The ends of the copper wires (2) are straightened and softened; The device used for the straightening and softening treatment comprises a guide tube (3), a plurality of air holes (4) are arranged on the outer peripheral surface of the guide tube (3), an air pipe (5) is arranged on the outer side of the guide tube (3), baffles (6) are arranged at both ends of the air pipe (5), a cavity (7) is formed between the air pipe (5) and the guide tube (3) through the baffles (6), a heating unit (8) in contact with the guide tube (3) is arranged in the cavity (7), a pipe joint (9) connected to the air pipe (5) is arranged on one side of the heating unit (8), and the pipe joint (9) is connected to a nitrogen tank (11) through a gas valve (10).
2. The chip MOS tube wire welding method according to claim 1, characterized in that: The diameter of the aluminum wire (1) is 300 um, and the diameter of the copper wire (2) is 38 um.
3. The chip MOS tube wire welding method according to claim 1, characterized in that: One end of the guide tube (3) extends out of the trachea (5).
Citation Information
Patent Citations
Restoration chip, regeneration chip, regeneration ink box, and printer system
CN106240161A
Synchronous rectifier module and rectification method and manufacturing method of synchronous rectifier module
CN108206640A
Three-dimensional packaging structure and packaging method of power device
CN109427707A
Integrated circuit chip packaging structure manufactured by using ultrasonic copper wires
CN110176440A
Production process of brushless motor controller
CN111970854A