Method for protecting Low-E glass plate, method for manufacturing glass unit, laminate, and protective sheet for Low-E glass plate

CN114040952BActive Publication Date: 2024-10-29NITTO DENKO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202080047101.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-23
Publication Date
2024-10-29
Estimated Expiration
2040-06-23

AI Technical Summary

Benefits of technology

[0026] In addition, according to this specification, a protective sheet for Low-E glass plates is provided. This protective sheet is used to protect a Low-E glass plate having a Low-E layer containing a zinc component, and has a structure in which an adhesive layer is formed on a base material. The protective sheet is used by bonding its adhesive layer to the Low-E layer of the Low-E glass plate. Furthermore, the adhesive layer in the protective sheet is formed from a water-dispersed adhesive composition, and the ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg/g relative to the weight of the adhesive layer. . With the protective sheet for Low-E glass plates having the above structure, the ammonia content of the adhesive layer is limited to less than a prescribed amount based on the hot water extraction method, so it is possible to prevent or suppress the presence of the Low-E layer in the Low-E glass plate. of deterioration. In some embodiments, the adhesive layer includes ammonia. The adhesive layer of this aspect contains ammonia in a ratio of less than 850 μg/g.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114040952B_ABST
    Figure CN114040952B_ABST
Patent Text Reader

Abstract

A method for protecting a Low-E glass plate that can prevent or inhibit deterioration of a Low-E layer is provided. A method for protecting a Low-E glass plate is provided. The method is a method for protecting a Low-E glass plate as follows: a protective sheet having a substrate and an adhesive layer provided on at least one surface of the substrate is attached to the Low-E layer of a Low-E glass plate having a Low-E layer containing a zinc component by means of the adhesive layer to protect the Low-E layer. The method is characterized in that, as the protective sheet, a protective sheet is used in which the adhesive layer is formed from a water-dispersible adhesive composition and the ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g relative to the weight of the adhesive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for protecting a Low-E glass plate, a method for producing a glass unit, a laminate, and a protective sheet for a Low-E glass plate.

[0002] This application claims priority based on Japanese Patent Application No. 2019-120483 filed on June 27, 2019, the entire contents of which are incorporated herein by reference. Background Art

[0003] When processing or transporting various items, in order to prevent surface damage (scratches, dirt, corrosion, etc.), it is known that there is a technology that adheres a protective sheet to the surface for protection. The objects of protection are wide-ranging. For example, glass plates with Low-E (Low-Emissivity: low radiation) layers (Low-E glass plates) that have been widely popularized in recent years also use protective sheets. Considering the effect of improving the cooling and heating efficiency of indoor spaces brought about by the Low-E layer, Low-E glass plates are preferably used as building materials such as window glass. When manufacturing Low-E glass plates, a protective sheet is usually attached to the directly exposed surface of the Low-E layer until the Low-E glass plate and other glass plates are made into double-layer glass in a manner such that the side surface of the Low-E layer faces the inside. In this way, the Low-E layer is protected from damage, wear, degradation, corrosion, etc. As prior art documents that disclose prior art related to the manufacturing method of glass units, Patent Documents 1 and 2 can be cited.

[0004] In the application of surface protection, as a peelable bonding means, an adhesive (also called a pressure-sensitive adhesive, the same below) can be preferably used. In general, an adhesive is in a soft solid (viscoelastic) state within a temperature range near room temperature, and has the property of being easily bonded to an adherend under pressure. A surface protection sheet using an adhesive is typically constructed as follows: an adhesive layer is provided on one side of a sheet-like substrate formed of a material such as a resin, and the adhesive layer is bonded to an adherend (protected object), thereby achieving the purpose of protection. As prior art documents that disclose adhesive sheets that can be used as surface protection sheets, Patent Documents 3 to 6 can be cited. Respectively, Patent Document 3 discloses a surface protection sheet that protects the surface of a metal plate during deep drawing of the metal plate, and Patent Document 4 discloses a surface protection sheet for an optical film such as a polarizing plate. Patent Document 5 relates to a surface protection sheet for a hydrophilic coated plate having self-cleaning properties. Patent Document 6 is dedicated to reducing the ease of peeling and contamination of a surface protection sheet for a metal plate to be formed with a coating.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: European Patent No. 2150669

[0008] Patent Document 2: International Publication No. 2016 / 139318

[0009] Patent Document 3: Japanese Patent Application Publication No. 2017-186517

[0010] Patent Document 4: Japanese Patent No. 5719194

[0011] Patent Document 5: Japanese Patent Application Publication No. 2012-131976

[0012] Patent Document 6: Japanese Patent No. 3571460 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] By using a protective sheet to protect the Low-E glass plate, not only can physical damage such as scratches and abrasions be avoided, but also the entry of water and moisture can be blocked. Since the Low-E glass plate is exposed to the external environment under the protection of the protective sheet for processing, cleaning, etc., the protective sheet is required to have the ability to prevent the above-mentioned degradation and corrosion in such an environment. In addition, the Low-E glass plate may be protected by the protective sheet for a long period of time due to transportation and storage, and the protective sheet is required to prevent the above-mentioned degradation and corrosion at a satisfactory level even in such a case.

[0015] Based on the above background, the inventors of the present invention have conducted research on preventing degradation and corrosion of Low-E glass plates, and have confirmed that the Low-E layer can deteriorate despite sufficient protection provided by the protective sheet. As a result of the research, it was found that the deterioration of the Low-E layer can occur due to the protective sheet itself, and the present invention was completed by studying the cause. An object of the present invention is to provide a method for protecting a Low-E glass plate that can prevent or inhibit the deterioration of the Low-E layer. Another object of the present invention includes providing a method for manufacturing a glass unit, providing a laminate, and providing a protective sheet for a Low-E glass plate.

[0016] Solutions for solving problems

[0017] According to the present specification, a method for protecting a Low-E glass plate is provided. The method is a method for protecting a Low-E glass plate as follows: a protective sheet having a substrate and an adhesive layer provided on at least one surface of the substrate is attached to the Low-E layer of a Low-E glass plate having a Low-E layer containing a zinc component via the adhesive layer to protect the Low-E layer. The method is characterized in that, as the protective sheet, a protective sheet is used in which the adhesive layer is formed of a water-dispersible adhesive composition and the ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g relative to the weight of the adhesive layer.

[0018] The results of the research conducted by the inventors of the present invention have confirmed that the ammonia contained in the adhesive reacts with the zinc component constituting the Low-E layer, causing the deterioration of the Low-E layer. For example, in a method in which the Low-E layer has a layer containing a zinc component, the low density of the layer containing the zinc component may cause the deterioration of the Low-E layer. It is believed that this phenomenon is caused by the reaction of the zinc component and ammonia. Based on this understanding, in the present protection method, the content of ammonia contained in the adhesive of the protective sheet for the Low-E glass plate is limited to less than a specified value. That is, according to the above protection method, by using a protective sheet having an adhesive layer whose ammonia content is limited to less than a specified amount based on a hot water extraction method, the deterioration of the Low-E layer in the Low-E glass plate can be prevented or suppressed. It should be noted that in the above method, the adhesive layer constituting the protective sheet may contain ammonia or may not contain it.

[0019] It should be noted that, in this specification, "zinc component" refers to a component containing zinc element, including metallic zinc, compounds containing zinc and other elements (zinc compounds), complexes (zinc complexes) and mixtures (zinc mixtures). Zinc compounds such as zinc oxide are typical examples of zinc components.

[0020] In the technology disclosed herein (including a method for protecting a Low-E glass plate, a method for manufacturing a glass unit, a laminate, and a protective sheet for a Low-E glass plate. The same shall apply hereinafter), some methods further include a step of removing the protective sheet from the Low-E glass plate. In addition, during the period from the attachment of the protective sheet to the Low-E glass plate to the removal thereof, the Low-E glass plate to which the protective sheet is attached is subjected to at least one step selected from the group consisting of transportation, storage, processing, cleaning, and operation. In the above-described method of using the Low-E glass plate, the protection of the Low-E glass plate can be achieved by using the protective sheet.

[0021] In some embodiments of the technology disclosed herein, the Low-E glass plate has a width of more than 1 meter. In addition, the attachment of the protective sheet to the Low-E glass plate includes a step of covering the entire surface of the Low-E glass plate with at least one protective sheet. By using such a wide protective sheet, the purpose of protecting a large-area Low-E glass plate can be achieved with one or a small number of sheets.

[0022] In some embodiments of the technology disclosed herein, the protective sheet is attached to the Low-E glass plate with a 180-degree peel strength of 5N / 20mm or less. Thus, the protective sheet can be removed from the Low-E glass plate with a relatively light peel force after the protection period ends.

[0023] In the technology disclosed herein, the Low-E layer of the Low-E glass plate may include a layer containing a zinc component. The above-mentioned layer containing a zinc component may be, for example, a layer selected from a layer containing zinc oxide and a composite layer containing zinc oxide. By limiting the amount of ammonia derived from the adhesive layer of the protective sheet, it is preferably possible to prevent or suppress the deterioration of the Low-E layer having a layer containing a zinc component (a layer containing zinc oxide, a composite layer containing zinc oxide, etc.).

[0024] In addition, according to the present specification, a method for manufacturing a glass unit is provided. The manufacturing method includes: step (A), preparing a Low-E glass plate having a Low-E layer; step (B), attaching a protective sheet to the surface of the Low-E layer of the Low-E glass plate; an optional step (C), subjecting the Low-E glass plate to which the protective sheet is attached to at least one of the group consisting of transportation, storage, processing, cleaning and operation; step (D), removing the protective sheet from the Low-E glass plate; and step (E), assembling a glass unit using the Low-E glass plate. Here, the Low-E layer contains a zinc component. In addition, the protective sheet includes a substrate and an adhesive layer provided on at least one surface of the substrate. The adhesive layer is attached to the surface of the Low-E layer. Furthermore, the adhesive layer is formed by a water-dispersible adhesive composition. Moreover, the ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g relative to the weight of the adhesive layer. According to the above-mentioned production method, the deterioration of the Low-E layer in the Low-E glass sheet can be prevented or suppressed, so that a high-quality glass unit with few defects such as discoloration can be obtained.

[0025] In addition, according to the present specification, a laminate is provided. The laminate comprises: a Low-E glass plate having a Low-E layer containing a zinc component; and a protective sheet having a substrate and an adhesive layer provided on at least one surface of the substrate. In addition, the protective sheet is attached to the Low-E layer of the Low-E glass plate using the adhesive layer. Moreover, the adhesive layer in the protective sheet is formed from a water-dispersible adhesive composition, and the ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g relative to the weight of the adhesive layer. With a laminate of such a structure, the Low-E layer of the Low-E glass plate constituting the laminate is protected by the protective sheet of the above structure, so that its deterioration is prevented or suppressed. In some embodiments, the adhesive layer contains ammonia. The adhesive layer of this embodiment contains ammonia at a ratio of less than 850 μg / g.

[0026] In addition, according to the present specification, a protective sheet for a Low-E glass plate is provided. The protective sheet is used to protect a Low-E glass plate having a Low-E layer containing a zinc component, and has a structure in which an adhesive layer is formed on a substrate. The protective sheet is used by bonding its adhesive layer to the Low-E layer of the Low-E glass plate. Moreover, the aforementioned adhesive layer in the aforementioned protective sheet is formed from a water-dispersible adhesive composition, and the ammonia content of the adhesive layer measured by hot water extraction is less than 850μg / g relative to the weight of the adhesive layer. Using the protective sheet for a Low-E glass plate having the above-mentioned structure, the ammonia content of the adhesive layer based on the hot water extraction method is limited to less than a specified amount, thereby preventing or inhibiting the deterioration of the Low-E layer present in the Low-E glass plate. In some embodiments, the aforementioned adhesive layer contains ammonia. The adhesive layer of this embodiment contains ammonia at a ratio of less than 850μg / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram for explaining one embodiment of a method for manufacturing a glass unit.

[0028] Figure 2 This is a cross-sectional view schematically showing an example of one embodiment of a protective sheet. DETAILED DESCRIPTION

[0029] The following describes the preferred embodiments of the present invention. Based on the enlightenment of the implementation of the invention recorded in this specification and the technical common sense at the time of application, those skilled in the art can understand the matters required for implementing the present invention other than the matters specifically mentioned in this specification. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the art.

[0030] In this specification, as mentioned above, "adhesive" refers to a material that is in a soft solid (viscoelastic) state in a temperature range near room temperature and has the property of being easily bonded to an adherend under pressure. The adhesive described here is defined in "CADahlquist, "Adhesion: Fundamentals and Practice", McLaren & Sons, (1966) P.143". Generally speaking, it can be a material that satisfies the complex tensile elastic modulus E*(1Hz)<10 7 dyne / cm 2 Materials having the above properties at 25°C.

[0031] In addition, the concept of protective sheet in this specification may include materials called adhesive sheets, adhesive tapes, adhesive labels, adhesive films, etc. It should be noted that the protective sheet disclosed herein may be in the form of a roll or a sheet, or may be a sheet further processed into various shapes.

[0032] <Method for manufacturing glass unit>

[0033] The manufacturing method of the glass unit disclosed herein may include: step (A), preparing a Low-E glass plate having a glass substrate and a Low-E layer laminated on the glass substrate; step (B), attaching a protective sheet to the surface of the Low-E layer of the Low-E glass plate; any step (C), subjecting the Low-E glass plate to which the protective sheet is attached to the Low-E glass plate to at least one of the group consisting of transportation, storage, processing, cleaning and operation; step (D), removing the protective sheet from the Low-E glass plate; and step (E), assembling a glass unit using the above-mentioned Low-E glass plate. In this method, the protective sheet (also called surface protective sheet) disclosed herein is used. Hereinafter, refer to Figure 1 Provide explanation.

[0034] First, in step (A), Figure 1As shown, a Low-E glass plate 100 having a Low-E layer 120 is prepared (S10). Specifically, the Low-E glass plate 100 may include a glass substrate 110 and a Low-E layer 120 laminated on the glass substrate 110. The Low-E glass plate 100 is prepared by forming a Low-E layer 120 on one surface of the glass substrate 110. The Low-E layer includes layers such as a metal layer, an oxide layer such as a metal oxide layer, a nitride layer such as a silicon nitride layer, and generally has a multilayer structure, and can be formed by a known or conventional method such as sputtering. In addition, the size of the glass substrate is not particularly limited, and the length of one side (width) is, for example, about 1 m or more, about 2 m or more, and recently, a large-area glass substrate having a length exceeding 2.6 m, and further about 3 m or more (for example, about 3.3 m or more) is used.

[0035] As materials constituting each layer of the Low-E layer, TiO2, ZrO2, Si X N Y 、ZnO X 、Ag、NiCrO X , SnO2, ZTO (zinc and tin oxides), etc. As the infrared reflection layer, it is preferred to use an Ag layer. The Ag layer can be a layer formed of a single substance of Ag, or a layer formed of an alloy of Ag and other metals (such as Pd). In addition, the Low-E layer 120 of this embodiment includes a zinc oxide layer. Although not particularly limited, in some embodiments of the Low-E layer, the Ag layer can be sandwiched between a TiO2 layer, a ZrO2 layer, a ZnO X Layer, NiCrO X Layer, SnO2 layer, ZTO layer and other oxide layers, Si X N Y The outermost surface of the Low-E layer (the surface to which the protective sheet is attached) is mostly made of TiO2, ZrO2, ZnO X 、NiCrO X , SnO2, ZTO and other oxides, Si X N Y Nitrides such as Ag are usually not metals. The Low-E layer can have a multilayer structure of more than 5 layers, for example, more than 10 layers, or more than 15 layers, depending on the purpose and required characteristics. The thickness of each layer is not particularly limited, but is usually Below, about is appropriate, for example, for about The thickness (total thickness) of the Low-E layer may be about 10 nm to 1000 nm (e.g., about 50 to 500 nm). The Low-E glass plate may be a commercially available product, a modified product thereof, or a product produced by a known and / or customary method.

[0036] In step (B), if Figure 1 As shown, the protective sheet 200 is attached to the surface of the Low-E layer 120 formed on the glass substrate 110 (S20). Typically, the protective sheet 200 is attached to the above-mentioned surface in a removable manner. Here, "attached in a removable manner" means an attachment that is intended or predetermined to be peeled off and removed. In most cases, it means an attachment in which the surface of the adherend after the protective sheet (adhesive sheet) is peeled off can maintain substantially the same state as before attachment. The attachment of the protective sheet 200 to the Low-E glass plate 100 is specifically performed by attaching the surface of the adhesive layer of the protective sheet 200 to the surface of the Low-E layer 120 of the Low-E glass plate 100. As a result, the surface of the Low-E glass plate 100 is protected by the protective sheet 200. From a protective point of view, the size of the protective sheet 200 is preferably set to the same degree as the surface of the Low-E layer 120. It is also possible to cover the surface of the protected object by partially overlapping two or more protective sheets. By covering the surface of the Low-E layer 120 with the protective sheet 200 , deterioration of the Low-E layer 120 can be prevented or suppressed.

[0037] After step (B), as step (C), at least one step (S30) selected from the group consisting of transportation, storage, processing, cleaning and operation can be arbitrarily implemented on the Low-E glass plate 100 with the protective sheet 200 attached thereto. The processing can be cutting, edge seaming, etc. of the Low-E glass plate 100 with the protective sheet 200 attached thereto. The cutting means and the size after cutting are appropriately set according to the purpose and are not particularly limited. The protective sheet 200 can be in a state of being attached to the surface of the Low-E layer 120 even after the Low-E glass plate 100 is cut. The cut Low-E glass plate 100 is typically cleaned by water or the like. In the cleaning step, in addition to water, a detergent (including a surfactant) can also be optionally used. During the above-mentioned processing such as transportation, storage, cutting, cleaning such as water washing, and various operations, such as Figure 1 As shown, the Low-E layer 120 is protected from damage, abrasion, and deterioration by the presence of the protection sheet 200 thereon.

[0038] Next, in step (D), the protective sheet 200 is removed from the Low-E glass plate 100 (S40). After the protective sheet 200 has achieved its protective purpose, it is removed from the Low-E glass plate 100 as an adherend. The Low-E glass plate 100 from which the protective sheet 200 has been removed is usually heat-treated and tempered in a heating furnace. Figure 1As shown, the glass unit 300 is manufactured using the Low-E glass plate 100 (S50). The glass unit 300 is typically a heat-insulating or heat-isolating glass unit, and can be manufactured by preparing a pair of glass plates, at least one of which is a Low-E glass plate 100, and making double-layer glass in a manner such that the surface of the Low-E layer 120 of the Low-E glass plate 100 faces inward. Symbols 320 and 340 in the figure respectively represent other glass plates and spacers constituting the glass unit 300. The spacer 340 is arranged between the glass plate 100 and the other glass plate 320 to form a space between the glass plates 100 and 320. It should be noted that in the method disclosed here, in addition to the protective sheet, a known and / or commonly used powder or liquid coating can also be used in combination.

[0039] It should be noted that, in the above embodiment, a Low-E glass plate having a Low-E layer including a zinc oxide layer is used as an example for description, but the Low-E glass plate is not limited to a Low-E glass plate having a Low-E layer including a zinc oxide layer. The deterioration of the Low-E layer prevented or suppressed by the technology disclosed herein is caused by the deterioration of the zinc component contained in the Low-E layer. Therefore, the Low-E layer used in the present technology is not particularly limited as long as it contains a zinc component.

[0040] The Low-E layer of the Low-E glass plate disclosed herein may typically have one or more layers containing a zinc component. The thickness of a layer containing a zinc component is, for example, about 100 nm or less, about 70 nm or less (for example, about 30 nm or less), and is, for example, about 1 nm or more, about 3 nm or more (for example, about 8 nm or more). As a typical example of a layer containing a zinc component, a layer containing zinc oxide can be cited. The layer containing zinc oxide can be a layer containing zinc oxide or a layer containing an oxide of zinc and other elements (for example, tin).

[0041] In addition, the layer containing zinc component can be present on the outer surface (outermost) of the Low-E layer, or it can be present inside the Low-E layer. In the mode where the layer containing zinc component is present inside the Low-E layer, the distance (thickness) from the outer surface of the Low-E layer to the layer containing zinc component is not particularly limited, and for example, it is appropriate to be below about 300nm, and below about 200nm (for example, below about 100nm). In such a configuration, the effect brought by the technology disclosed herein can be preferably exerted. The lower limit of the distance (thickness) from the outer surface of the Low-E layer to the layer containing zinc component is not particularly limited, and for example, it is above about 1nm, and can be above about 10nm.

[0042] <Protection method>

[0043] The protection method disclosed herein is a protection method using the protection sheet disclosed herein (also referred to as a surface protection sheet), and is typically a method for protecting a portion or all of the surface of a Low-E glass plate. The protection method disclosed herein is characterized in that it includes a step of attaching the protection sheet to the surface of the Low-E glass plate (attaching step).

[0044] In addition, the protection method disclosed herein may further include a step of removing the protection sheet from the Low-E glass plate (removal step). Furthermore, between the attachment step and the removal step, at least one step selected from the group consisting of transportation, storage, processing, cleaning and operation may be optionally included for the article to which the protection sheet is attached.

[0045] A suitable example of the protection method disclosed herein is as described in the manufacturing method of the glass unit described above, and the attaching step and the removing step in the present protection method correspond to the steps (B) and (D) in the manufacturing method described above, respectively. There are no special restrictions on other matters in the protection method, and those skilled in the art can understand them by referring to the description of the manufacturing method of the glass unit described above, so the detailed description is omitted here.

[0046] <Constitution of the protective sheet>

[0047] The protective sheet disclosed herein typically has an adhesive layer on a substrate layer (supporting substrate, also referred to as "substrate" for short. The same shall apply hereinafter.). The cross-sectional structure of a protective sheet of an example of a scheme is shown in FIG. Figure 2 . The protective sheet 10 has a structure in which an adhesive layer 2 is provided on one surface 1A of a sheet-like substrate layer 1, and the surface 2A of the adhesive layer 2 is attached to an adherend (protected object) for use. The back side 1B of the substrate layer 1 (the surface opposite to one surface 1A) is also the back side of the protective sheet 10, which constitutes the outer surface of the protective sheet 10. The protective sheet 10 before use (i.e., before being attached to the adherend) may be in a form in which the surface (adhesive surface, i.e., the attachment surface to the adherend) 2A of the adhesive layer 2 is protected by a release liner (not shown) whose at least one side of the adhesive layer serves as a release surface. Alternatively, it may be a protective sheet 10 in which the other side (back side) 1B of the substrate layer 1 serves as a release surface, and the adhesive layer 2 is protected by contacting the back side with the protective sheet 10 by winding the protective sheet 10 into a roll. It should be noted that the protective sheet may also be in a form in which an adhesive layer is provided on both sides of the substrate layer.

[0048] As the release liner, conventional release paper or the like can be used without particular limitation. For example, a release liner having a release treatment layer on the surface of a liner substrate such as a plastic film or paper, or a release liner formed of a low-adhesive material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin-based resin can be used. The release treatment layer can be formed by surface-treating the liner substrate with various release treatment agents such as silicone-based, long-chain alkyl-based, fluorine-based, and molybdenum sulfide-based.

[0049] The width of the protective sheet disclosed here is not particularly limited. By using a protective sheet having a width of, for example, about 1 m or more, and further about 1.5 m or more, the protection of a Low-E glass plate with a relatively large area can be achieved with good efficiency. The width of the protective sheet in some preferred embodiments is about 2 m or more. Such a wide protective sheet can achieve a protective function for a large area of ​​Low-E glass plate with one or a small number of sheets. In the protection of the above-mentioned Low-E glass plate, it is preferred to use a protective sheet having a width of, for example, about 2.5 m or more, and further about 2.6 m or more. The width of the protective sheet can be more than 2.6 m (for example, more than 3 m, and further about 3.3 m or more). The upper limit of the width of the protective sheet is not particularly limited. From the perspective of productivity, handling, etc., about 5 m or less is appropriate, for example, it can be about 4 m or less.

[0050] It should be noted that the protective sheet disclosed here can be, for example, a sheet defined by having a long side and a short side in its plane (sheet surface). The long side is defined as a side longer than the short side, and the short side is defined as a side shorter than the long side. Moreover, for example, the short side can be a side substantially orthogonal to the long side. The length direction of the protective sheet is the direction along the long side, and the width direction is the direction orthogonal to the length direction. Therefore, in this specification, "width" is defined as the length in the direction orthogonal to the length direction. Protective sheets referred to as long strips, bands, and rectangular shapes are typical examples of the protective sheets disclosed here. The long side is a line segment extending in an almost straight line, while the short side is not limited to a straight line, and can be a curve, a broken line, etc. For example, the length (distance in the length direction) of the long strip protective sheet is the same as or longer than the above-mentioned width.

[0051] The thickness of the protective sheet disclosed herein is not particularly limited. From the perspective of handling and lightness, it is appropriate to set it to about 1000 μm or less (typically about 300 μm or less, for example, about 150 μm or less). In some embodiments, the thickness of the protective sheet is preferably about 120 μm or less, more preferably about 100 μm or less, and further preferably about 75 μm or less, for example, it may also be less than 60 μm. In addition, the thickness of the protective sheet is typically more than 20 μm, preferably more than 30 μm, more preferably more than 40 μm, and for example, it may also be more than 45 μm.

[0052] In addition, in this specification, the thickness of a protective sheet includes the thickness of an adhesive layer and a base material layer, but does not include the thickness of a release liner.

[0053] <Adhesive Layer>

[0054] (Ammonia content)

[0055] The adhesive layer constituting the protective sheet disclosed herein is characterized in that the ammonia content measured by hot water extraction is less than 850 μg per 1 g of the adhesive (layer). In other words, the ammonia content of the adhesive layer is less than 850 μg / g relative to the weight of the adhesive layer. This can prevent or inhibit the deterioration of the Low-E glass plate to be protected.

[0056] The following is a detailed description of the mechanism of preventing and inhibiting deterioration of the Low-E layer by limiting the amount of ammonia in the adhesive, but the technology disclosed here is not limited to the following description. The present inventors found that the adhesive used for the protection of the Low-E glass plate will cause deterioration of the Low-E layer after being attached to the surface of the Low-E layer. Therefore, the inventors conducted research from two directions: identification of the deterioration site in the Low-E layer and identification of the causative substance. Regarding the deteriorated parts in the Low-E layer, the cross section of the Low-E layer sample was adjusted by FIB (focused ion beam) microsampling method, and FE-TEM observation was performed at an accelerating voltage of 200 kV using a field emission transmission electron microscope (FE-TEM: model "JEM-2800", manufactured by JEOL). Furthermore, elemental analysis based on EDX was performed using an energy dispersive X-ray spectrometer (EDX: Energy Dispersive X-ray Spectroscopy, product name "NORAN System 7", manufactured by Thermo Fisher Scientific). As a result, changes in the layer containing zinc components (specifically, low density) and a decrease in the detection intensity of zinc elements in the layer containing zinc components were confirmed. On the other hand, regarding the identification of the causal substance, the adhesive constituent materials (polymer, crosslinking agent, emulsifier, etc.) were brought into contact with the Low-E layer surface of the Low-E glass plate according to the material, and the sample was covered with a cover glass to prepare the sample. After being stored in this state, the sample was observed. As a result, ammonia used as a pH adjuster was identified as the cause of deterioration of the Low-E layer. That is, it is known that ammonia in the adhesive penetrates into the Low-E layer and reacts with the zinc component, causing the zinc component to dissolve, which becomes the cause of deterioration of the Low-E layer. It is believed that this phenomenon is caused by the reaction of the zinc component and ammonia. Based on this view, in the technology disclosed here, the content of ammonia contained in the adhesive of the protective sheet for the Low-E glass plate is limited to less than a specified value. By limiting the amount of ammonia, which is a substance causing deterioration of the Low-E layer, to less than a specified amount, deterioration of the Low-E layer in the Low-E glass plate can be prevented or suppressed.

[0057] For the ammonia content per 1g of adhesive (layer), from the perspective of the deterioration prevention of the Low-E layer, it is preferably less than 750μg, more preferably less than 650μg, further preferably less than 550μg, particularly preferably less than about 450μg (for example, less than 400μg), less than 300μg, or less than 100μg (for example, less than 10μg). Some forms of adhesive layers may be substantially free of ammonia. The lower limit of the ammonia content per 1g of adhesive (layer) is 0μg, but considering the convenience of ammonia in pH adjustment and other purposes, it can be about 1μg or more, about 10μg or more, or about 100μg or more. From the perspective of the coating and stability of the adhesive composition, the ammonia content per 1g of adhesive (layer) can be about 300μg or more, about 500μg or more, and further about 700μg or more (for example, about 800μg or more). The amount of ammonia in the adhesive layer can be adjusted by the amount of ammonia added in the adhesive composition, drying conditions, etc. The ammonia content per 1g of adhesive (layer) is measured by the method described in the examples described later. Alternatively, the ammonia content in the protective sheet and the substrate layer constituting the protective sheet is measured by hot water extraction, and the ammonia content from the adhesive layer is calculated based on the difference between the ammonia contents of the two, and the obtained value is converted into a value per unit adhesive (layer) for determination.

[0058] The type of adhesive constituting the adhesive layer disclosed herein is not particularly limited. The above-mentioned adhesive layer can be formed by an adhesive composition, which includes one or more of various polymers (also referred to as polymers as adhesive components or adhesive polymers) selected from, for example, acrylic, polyester, urethane, polyether, rubber, silicone, polyamide, fluorine polymers, etc. as a base polymer (the main component in the polymer component, i.e., the component occupying more than 50% by weight). The technology disclosed herein can be preferably implemented in the form of a protective sheet having, for example, an acrylic adhesive layer and a rubber adhesive layer.

[0059] Here, "acrylic adhesive layer" refers to an adhesive layer using an acrylic polymer as a base polymer. Similarly, "rubber adhesive layer" refers to an adhesive layer using a rubber polymer as a base polymer. "Acrylic polymer" refers to a polymer having a monomer having at least one (meth)acryloyl group in one molecule (hereinafter sometimes referred to as "acrylic monomer") as a main monomer component (the main component of the monomer, i.e., the component that occupies 50% by weight or more of the total amount of monomers constituting the acrylic polymer). In addition, in this specification, "(meth)acryloyl" refers to acryl and methacryloyl. Similarly, "(meth)acrylate" refers to acrylate and methacrylate.

[0060] (Acrylic polymer)

[0061] As the acrylic polymer, for example, a polymer of a monomer raw material containing an alkyl (meth)acrylate (hereinafter also referred to as "monomer A") and further containing another monomer copolymerizable with the alkyl (meth)acrylate (hereinafter also referred to as "monomer B") is preferred. Typically, the acrylic polymer has a copolymerization composition corresponding to the composition of the monomer components contained in the monomer raw material.

[0062] As the monomer A, an alkyl (meth)acrylate represented by the following general formula (1) can be preferably used.

[0063] CH2=C(R 1 )COOR 2 (1)

[0064] Among them, R in the above formula (1) 1 is a hydrogen atom or a methyl group. 2 is an alkyl group having 1 to 20 carbon atoms. Hereinafter, such a range of carbon atoms may be represented as "C 1-20 From the viewpoint of polymerization reactivity, polymerization stability, etc., R 2 C 1-16 Alkyl (meth)acrylate of an alkyl group, more preferably R 2 C 1-12 (Typical is C 1-10 For example, C 1-8 ) alkyl (meth)acrylate.

[0065] As R 2 C 1-20Examples of the alkyl (meth)acrylate having an alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. Such alkyl (meth)acrylates may be used alone or in combination of two or more.

[0066] The technology disclosed herein can be preferably implemented in a manner in which the acrylic acid alkyl ester as the monomer A accounts for about 50% by weight or more (more preferably about 75% by weight or more, further preferably about 90% by weight or more, for example about 95% by weight or more) of the above-mentioned total monomer components. As the above-mentioned acrylic acid alkyl ester, it is preferred that R in the above-mentioned formula (1) 2 C 1-20 Alkyl acrylate of an alkyl group, more preferably R 2 C 1-12 (More preferably C 1-10 , particularly preferably C 1-8 ) alkyl acrylate. The technology disclosed herein can preferably be used in which the above alkyl acrylate is R in the above formula (1) 2 C 2-8 (Typical is C 4-8 ) is implemented in the form of an alkyl acrylate having an alkyl group. The alkyl acrylate may be used alone or in combination of two or more. When two or more alkyl acrylates are used, R may be adjusted to the optimum range for the purpose of adjusting the Tg of the acrylic polymer. 2 C 4-20 (More preferably C 4-10 , more preferably C 4-8 ) alkyl acrylate A1, and C 1-3 (More preferably C 1-2, for example, C2) in combination with an alkyl acrylate A2 having an alkyl group. In this case, the weight ratio of the alkyl acrylate A1 to the alkyl acrylate A2 (A1:A2) is not particularly limited, and is, for example, about 5:95 to 95:5, and is appropriately about 10:90 to 90:10, for example, about 15:85 to 85:15.

[0067] In some preferred embodiments, the monomer component includes one or more alkyl methacrylates as monomer A. By using alkyl methacrylates, a base polymer that can exhibit desired adhesive properties can be preferably designed. As the alkyl methacrylate, R in the above formula (1) is preferably 2 C 1-10 Alkyl methacrylate of an alkyl group, more preferably R 2 C 1-4 (More preferably C1 or C 2-4 ) is an alkyl methacrylate having an alkyl group. The above alkyl methacrylate can be preferably used in combination with an alkyl acrylate. When a methacrylate and an alkyl acrylate are used in combination, one or more methacrylates (e.g., methacrylate C 2-4 The weight of alkyl esters AM and one or more alkyl acrylates by weight C AA The ratio (C AM :C AA ) is not particularly limited. In some embodiments, it is about 1:9 to 9:1, about 2:8 to 8:2 is appropriate, about 3:7 to 7:3 is preferred, and about 4:6 to 6:4 is more preferred. In other embodiments, the total amount of the (meth)acrylic acid alkyl ester (C AM +C AA ) in the alkyl methacrylate (e.g., C1 alkyl methacrylate, i.e., methyl methacrylate (MMA)) by weight C AM The amount of the polyol is preferably about 30% by weight or less, about 20% by weight or less is appropriate, preferably about 10% by weight or less, and more preferably about 7% by weight or less. On the other hand, the lower limit is, for example, about 0.1% by weight or more, about 1% by weight or more is appropriate, and preferably about 2% by weight or more (e.g., about 3% by weight or more).

[0068] It should be noted that the technology disclosed herein can be implemented in a mode in which the monomer component does not substantially contain alkyl methacrylate as monomer A. In a mode in which alkyl methacrylate is used, for example, alkyl methacrylate can be used in a mode in which alkyl methacrylate is not contained. 1-3 The reaction is carried out by means of an alkyl ester (typically MMA).

[0069] In another preferred embodiment, the acrylic polymer is an alkyl acrylate having 4 to 9 carbon atoms in the alkyl group (hereinafter also referred to as monomer mA ), and may contain other monomers as required. The acrylic polymer may be synthesized by polymerizing monomers of corresponding compositions (monomer compositions) by a known method.

[0070] As monomer m A Non-limiting examples of the monomer m include n-butyl acrylate (BA), n-hexyl acrylate, 2-ethylhexyl acrylate (2EHA), n-octyl acrylate, n-nonyl acrylate, and isononyl acrylate (iNA). Preferably, the alkyl acrylate contains a -(CH2)3- structure in the alkyl group, and more preferably, the alkyl acrylate contains a -(CH2)4- structure in the alkyl group. A Preferred examples include 2EHA, BA and iNA. A One type may be used alone, or two or more types may be used in combination.

[0071] Typically, monomer m A The amount of the monomer m used is 40% by weight or more of the total monomer raw material used for the synthesis of the acrylic polymer. From the viewpoint of improving the flexibility and low temperature characteristics of the adhesive layer containing the acrylic polymer, the monomer m is contained in the monomer composition in a ratio of 40% by weight or more. A From this point of view, it is preferred to A The ratio of monomer m in the monomer composition is set to 45% by weight or more, and can be set to 50% by weight or more (for example, more than 50% by weight). A The ratio of 99.9 wt % or less can easily impart moderate agglomeration to the adhesive layer containing the acrylic polymer. A The ratio of is set to 95 wt % or less, more preferably 90 wt % or less, and may be set to 85 wt % or less. In some embodiments, the monomer m A The ratio may be less than 80% by weight, or less than 70% by weight (eg, 65% by weight or less).

[0072] The acrylic polymer in the technology disclosed herein may have a carboxyl group-containing monomer (hereinafter also referred to as monomer m B ) as the monomer composition of monomer B. That is, the acrylic polymer may also be copolymerized with monomer m B . Monomer m B It can help introduce crosslinking points into the acrylic polymer and improve the cohesive force of the adhesive layer containing the acrylic polymer. BBy improving the adhesion (anchoring property) between the adhesive layer containing the acrylic polymer and the substrate layer, it helps to improve the non-residual adhesive property. As carboxyl-containing monomers, for example, acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, (meth) carboxyethyl acrylate, (meth) carboxypentyl acrylate, 1-[2-(methacryloyloxy)ethyl] succinic acid and other ethylenically unsaturated monocarboxylic acids; maleic acid, fumaric acid, itaconic acid, citraconic acid and other ethylenically unsaturated dicarboxylic acids and their anhydrides (such as maleic anhydride, itaconic anhydride), etc. The carboxyl-containing monomers can be used alone or in combination of two or more.

[0073] Use monomer m B In the case of B The ratio of monomer m is not particularly limited. B The ratio of monomer m can be set to 0.05 wt % or more, 0.1 wt % or more is appropriate, and from the viewpoint of polymerization stability and dispersion stability, it is preferably 0.5 wt % or more, and more preferably 1 wt % or more. In addition, from the viewpoint of suppressing excessive increase in peel strength (adhesive force), monomer m B The proportion of about 20 weight % or less (preferably about 10 weight % or less, typically about 7 weight % or less) is appropriate, more preferably about 5 weight % or less, further preferably about 4 weight % or less (e.g., 3 weight % or less). From the viewpoint of inhibiting corrosion of the Low-E glass plate as the object of protection, it is preferred to limit the amount of the carboxyl group-containing monomer.

[0074] For the purpose of adjusting the glass transition temperature (Tg) of the acrylic polymer, the acrylic polymer disclosed in the art may be copolymerized with a (meth)acrylic acid alkyl ester (hereinafter also referred to as monomer m) having an alkyl group with 4 to 20 carbon atoms and a homopolymer Tg of -50°C or higher. C ). Here, the monomer m A The monomer is not included in the monomer m C The monomer m C One type may be used alone, or two or more types may be used in combination. C , preferably a monomer m whose homopolymer Tg is in the range of -40°C to +60°C C , more preferably, the monomer m is in the range of -30°C to +40°C (e.g., -20°C to +30°C) C As the monomer m that can be preferably used C Non-limiting examples of the ester include n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate and lauryl acrylate.

[0075] When using monomer m C In the case ofC The ratio of monomer m is not particularly limited. C The ratio of m is set to, for example, 1 wt % or more, 5 wt % or more, 10 wt % or more, or 15 wt % or more. C From the perspective of the effect of C The ratio of monomer m in the monomer composition can be set to 20% by weight or more, or 25% by weight or more, or 30% by weight or more, or 35% by weight or more (e.g., 40% by weight or more). C The ratio of is set to less than 60% by weight. From the viewpoint of improving flexibility and low temperature properties, it is appropriate to set it to about 55% by weight or less (typically about 50% by weight or less, for example, about 45% by weight or less). C The proportion may be less than 30% by weight, less than 20% by weight, or less than 10% by weight (eg, less than 5% by weight, or further less than 1% by weight).

[0076] In the acrylic polymer disclosed in the art, other monomers other than monomer m may be copolymerized as required. A 、m B 、m C Monomers other than D ) as monomer A. As monomer m D , a single agent that can react with monomer m A Each monomer may be copolymerized or two or more monomers may be used in combination.

[0077] As monomer m D For example, the (meth)acrylic acid alkyl ester (monomer m) represented by the above general formula (1) can be used. D1 )(wherein, equivalent to monomer m A or monomer m C As monomer m D1 Specific examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and the like. D1 One type may be used alone, or two or more types may be used in combination.

[0078] Can be used as monomer m D Examples of the compound may include the functional group-containing monomer (monomer B) described below. Such a functional group-containing monomer can help introduce crosslinking points into the acrylic polymer and improve the cohesive force of the acrylic polymer.

[0079] Hydroxyl-containing monomers: for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl acrylate and other hydroxyalkyl (meth)acrylates; unsaturated alcohols such as vinyl alcohol and allyl alcohol.

[0080] Amide group-containing monomers: for example, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, diacetone(meth)acrylamide.

[0081] Imido group-containing monomers: for example, N-isopropylmaleimide, N-cyclohexylmaleimide, itaconimide.

[0082] Amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate.

[0083] Monomers having an epoxy group: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.

[0084] Cyano-containing monomers: such as acrylonitrile and methacrylonitrile.

[0085] Ketone group-containing monomers: for example, diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, vinyl acetoacetate.

[0086] Monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, N-(meth)acryloylmorpholine, N-(meth)acryloylpyrrolidone.

[0087] Alkoxysilyl group-containing monomers: for example, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane.

[0088] As a monomer m D Other examples of the compound include vinyl ester monomers such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene, substituted styrenes (such as α-methylstyrene), and vinyltoluene; (meth)acrylates containing non-aromatic rings such as cyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclopentyl di(meth)acrylate, and isobornyl (meth)acrylate; aryl (meth)acrylates (such as phenyl (meth)acrylate and benzyl (meth)acrylate), aryloxyalkyl (meth)acrylates (such as (meth)acrylate) (Meth)acrylates containing aromatic rings such as (phenoxyethyl (meth)acrylate), (meth)acrylate arylalkyl esters (such as benzyl (meth)acrylate); olefin monomers such as ethylene, propylene, isoprene, butadiene, isobutylene, etc.; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; isocyanate-containing monomers such as 2-(meth)acryloyloxyethyl isocyanate; alkoxy-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; vinyl ether monomers such as methyl vinyl ether, ethyl vinyl ether, isobutyl vinyl ether, etc.

[0089] As a monomer m D As further other examples of compounds, multifunctional monomers can be cited. As specific examples of multifunctional monomers, compounds having two or more (meth)acryloyl groups in one molecule, such as 1,6-hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and methylenebisacrylamide, can be cited. When such a multifunctional monomer is used, its amount is not particularly limited, and it is appropriate to set it to less than 2% by weight (more preferably less than 1% by weight) of all monomer components.

[0090] Monomer m D The amount of monomer m is preferably set to not more than 40% by weight of the monomer composition, preferably not more than 20% by weight, and more preferably not more than 10% by weight. D The technology disclosed herein can preferably be based on monomer m D The amount of monomer m is 0% by weight or more and less than 5% by weight of the monomer composition. D The amount of 0% by weight of the monomer composition means that at least the monomer m is not intentionally used. D .

[0091] Although not particularly limited, the proportion of monomer A ((meth) alkyl acrylate) in the total monomer components can be set to, for example, about 50% by weight or more, and it is appropriate to set it to about 60% by weight or more, preferably about 70% by weight or more, more preferably about 80% by weight or more, and further preferably about 85% by weight or more. By including more than a specified amount of monomer A, a protective sheet with desired adhesive properties can be suitably achieved. The technology disclosed herein can preferably be implemented in a manner such that the proportion of monomer A in the total monomer components is about 90% by weight or more. In some embodiments, the proportion of monomer A can be about 95% by weight or more, or about 97% by weight or more. From the perspective of the weather resistance of the adhesive layer formed by the composition (further a protective sheet having the adhesive layer), an adhesive composition using such an acrylic polymer as a base polymer can become advantageous. In addition, in the method of using monomer A and monomer B in combination, from the viewpoint of appropriately exerting the effect of monomer B, the proportion of monomer A in all monomer components can be set to, for example, 99.9% by weight or less, preferably 99.5% by weight or less, more preferably 99% by weight or less, or it can also be about 97% by weight or less (for example, 95% by weight or less).

[0092] When the above-mentioned functional group-containing monomer is copolymerized in the acrylic polymer, the proportion of the functional group-containing monomer in the total monomer components constituting the acrylic polymer is preferably set to about 0.1% by weight or more (typically about 0.5% by weight or more, for example, about 1% by weight or more), and preferably about 40% by weight or less (typically about 30% by weight or less, for example, about 20% by weight or less). For example, when a hydroxyl group-containing monomer is copolymerized in the acrylic monomer, from the viewpoint of obtaining the desired cohesive force, the proportion of the hydroxyl group-containing monomer in the total monomer components is appropriately set to about 0.001% by weight or more (typically about 0.01% by weight or more, for example, about 0.1% by weight or more), preferably about 1% by weight or more, more preferably about 3% by weight or more, and preferably about 10% by weight or less (typically about 7% by weight or less, for example, about 5% by weight or less).

[0093] (Rubber polymer)

[0094] In another preferred embodiment, the adhesive layer can be a rubber-based adhesive layer. Examples of the above-mentioned base polymers include natural rubber, styrene-butadiene rubber (SBR), polyisoprene, butene-based polymers with butene (referring to 1-butene, and cis- or trans-2-butene) and / or 2-methylpropylene (isobutylene) as main monomers, ABA-type block copolymer rubbers and hydrogenated products thereof, such as styrene-butadiene-styrene block copolymer rubber (SBS), styrene-isoprene-styrene block copolymer rubber (SIS), styrene-isobutylene-styrene block copolymer rubber (SIBS), styrene-vinyl·isoprene-styrene block copolymer rubber (SVIS), styrene-ethylene-butylene-styrene block copolymer rubber (SEBS) as a hydrogenated product of SBS, styrene-ethylene-propylene-styrene block copolymer rubber (SEPS) as a hydrogenated product of SIS, and various rubber-based polymers. These rubber-based polymers can be used alone or in combination of two or more.

[0095] (Tg of base polymer)

[0096] The Tg of the base polymer of the adhesive layer disclosed here (in the case of an acrylic adhesive layer, an acrylic polymer) is not particularly limited. The Tg of the above-mentioned base polymer can be, for example, below about 0°C. In a preferred embodiment, the Tg of the base polymer of the adhesive layer is below about -5°C. According to the base polymer having the above-mentioned Tg, an adhesive layer with excellent adhesion to the adherend can be suitably formed. When a method is adopted in which the Tg of the base polymer is below about -15°C (more preferably below about -20°C, for example, below about -25°C), a better effect can be achieved. In another preferred embodiment, from the perspective of adhesion to the adherend, the Tg of the base polymer of the adhesive layer is below about -35°C, more preferably below about -40°C, and further preferably below about -45°C (for example, about less than -50°C, further about -52°C or below, or about -55°C or below). In addition, the Tg of the base polymer is preferably -70°C or higher, and is preferably about -65°C or higher, more preferably -60°C or higher, further preferably -55°C or higher (e.g., about -50°C or higher), and may be -35°C or higher from the viewpoint of the cohesiveness of the adhesive. The Tg of the base polymer can be adjusted by appropriately changing the monomer composition (i.e., the type and amount ratio of the monomers used in the synthesis of the polymer).

[0097] In this specification, the Tg of a polymer refers to a value obtained based on the Tg of a homopolymer of each monomer constituting the polymer and the weight fraction (copolymerization ratio based on weight) of the monomer and according to the Fox equation. The Fox equation refers to the relationship between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer formed by homopolymerizing each of the monomers constituting the copolymer, as shown below.

[0098] 1 / Tg=Σ(Wi / Tgi)

[0099] In the above Fox equation, Tg represents the glass transition temperature of the copolymer (unit: K), Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio based on weight), and Tgi represents the glass transition temperature of the homopolymer of monomer i (unit: K).

[0100] As the glass transition temperature of the homopolymer used for calculation of Tg, the value described in the known documents can be used. For example, for the monomers listed below, the following values ​​are used as the glass transition temperature of the homopolymer of the monomer.

[0101]

[0102] For the Tg value of the homopolymer of the monomer other than the above examples, the value recorded in Polymer Handbook (3rd edition, John Wiley & Sons, Inc., 1989) is used. For monomers with multiple values ​​recorded in this document, the highest value is adopted. In the case where the Tg of the homopolymer is not recorded in the above Polymer Handbook, the value obtained by the measurement method described in Japanese Patent Publication No. 2007-51271 is used.

[0103] (Synthesis of base polymer)

[0104] The method for obtaining the base polymer (e.g., acrylic polymer) is not particularly limited. For example, known polymerization methods such as solution polymerization, emulsion polymerization, bulk polymerization, and suspension polymerization can be appropriately used. Alternatively, active energy ray irradiation polymerization such as photopolymerization by irradiation with UV light (typically carried out in the presence of a photopolymerization initiator), radiation polymerization by irradiation with radiation such as β rays and γ rays can also be used. In some preferred methods, the base polymer (e.g., acrylic polymer) is typically obtained by emulsion polymerization of monomer raw materials of the composition described above. For example, as a monomer supply method in the emulsion polymerization method, a one-time input method in which all monomer raw materials are supplied at one time, a continuous supply (drip) method, a batch supply (drip) method, etc. can be appropriately used. It is also possible to pre-mix and emulsify a part or all of the monomer components with water and a surfactant, and supply the emulsion to the polymerization container.

[0105] The polymerization temperature can be appropriately selected according to the types of monomers and solvents used, the types of polymerization initiators, etc. The polymerization temperature is appropriately set to about 20°C or more, preferably about 40°C or more, more preferably about 50°C or more, about 60°C or more, about 65°C or more, and further about 70°C or more. In addition, the polymerization temperature is appropriately set to about 170°C or less (typically about 140°C or less), preferably about 95°C or less (for example, about 85°C or less). In emulsion polymerization, the polymerization temperature is preferably set to about 95°C or less (for example, about 85°C or less).

[0106] Examples of the polymerization initiator include, but are not limited to, azo initiators, peroxide initiators, and redox initiators in which a peroxide and a reducing agent are combined. The polymerization initiator may be used alone or in combination of two or more.

[0107] Examples of the azo initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate, 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, and 2,2'-azobis(N,N'-dimethyleneisobutylamidine) dihydrochloride.

[0108] Examples of peroxide-based initiators include persulfates such as potassium persulfate and ammonium persulfate; benzoyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, di-n-octanoyl peroxide, di(4-methylbenzoyl) peroxide, tert-butyl perbenzoate, tert-butyl peroxyisobutyrate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, di(2-ethylhexyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, tert-butyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, 1,1-bis(tert-butylperoxide)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxide)cyclododecane, 1,1-bis(tert-hexylperoxide)cyclohexane, hydrogen peroxide, and the like.

[0109] Examples of the redox initiator include a combination of a peroxide and ascorbic acid (such as a combination of hydrogen peroxide and ascorbic acid), a combination of a peroxide and an iron (II) salt (such as a combination of hydrogen peroxide and an iron (II) salt), and a combination of a persulfate and sodium bisulfite.

[0110] The amount of the polymerization initiator can be appropriately selected according to the type of the initiator, the type of monomer (composition of monomer components), polymerization conditions, etc. The amount of the polymerization initiator is, for example, about 0.0005 to 1 part by weight, for example, about 0.001 to 0.5 parts by weight, preferably 0.002 to 0.3 parts by weight, more preferably 0.005 to 0.1 parts by weight, relative to 100 parts by weight of the monomer raw material.

[0111] As required, various chain transfer agents known in the art (which may also be regarded as molecular weight regulators or polymerization degree regulators) may be used in emulsion polymerization. Chain transfer agents may be used alone or in combination of two or more. As chain transfer agents, thiols such as n-dodecyl mercaptan, tert-dodecyl mercaptan, glycidyl mercaptan, 2-mercaptoethanol, thioglycolic acid, thioglycolic acid, 2-ethylhexyl thioglycolate, and 2,3-dimercapto-1-propanol may be preferably used. When a chain transfer agent is used, the amount thereof may be set to, for example, about 0.01 to 1 part by weight, preferably 0.02 to 0.1 parts by weight, and more preferably 0.03 to 0.07 parts by weight, relative to 100 parts by weight of all monomer components. The technology disclosed herein may also be preferably implemented without using a chain transfer agent.

[0112] The surfactant (emulsifier) ​​used in the emulsion polymerization is not particularly limited, and known anionic surfactants, nonionic surfactants, etc. can be used. Surfactants having free radical polymerizable functional groups can also be used. Hereinafter, surfactants having free radical polymerizable functional groups are also referred to as reactive (polymerizable) surfactants. In contrast, general surfactants that do not have free radical polymerizable functional groups are sometimes referred to as non-reactive (non-polymerizable) surfactants. Surfactants can be used alone or in combination of two or more.

[0113] Examples of non-reactive surfactants include anionic emulsifiers such as sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzene sulfonate, sodium polyoxyethylene lauryl sulfate, sodium polyoxyethylene alkyl ether sulfate, ammonium polyoxyethylene alkylphenyl ether sulfate, sodium polyoxyethylene alkyl phenyl ether sulfate, and sodium polyoxyethylene alkyl sulfosuccinate; nonionic emulsifiers such as polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene fatty acid esters, and polyoxyethylene polyoxypropylene block polymers; and the like.

[0114] The reactive surfactant is not particularly limited as long as it has a free radical polymerizable functional group. For example, it can be a reactive surfactant having a structure obtained by introducing a free radical polymerizable functional group into the anionic surfactant or nonionic surfactant described above. Examples of the above-mentioned free radical polymerizable functional group include vinyl, propenyl, isopropenyl, vinyl ether (vinyloxy), allyl ether (allyloxy), etc. The concept of propenyl described here includes 1-propenyl (CH3-CH=CH-) and 2-propenyl (CH2=CH-CH2-; also called allyl).

[0115] Examples of anionic reactive surfactants include polyoxyethylene (allyloxymethyl) alkyl ether sulfates (e.g., ammonium salts), polyoxyethylene nonyl propenyl phenyl ether sulfates (e.g., ammonium salts), alkyl allyl sulfosuccinates (e.g., sodium salts), methacryloyloxy polyoxypropylene sulfate salts (e.g., sodium salts), polyoxyalkylene alkenyl ether sulfates (e.g., ammonium salts in which the terminal of the alkenyl group is an isopropenyl group), etc. When the anionic reactive surfactant forms a salt, the salt may be, for example, a metal salt such as a sodium salt, or a non-metallic salt such as an ammonium salt or an amine salt.

[0116] Examples of the nonionic reactive surfactant include polyoxyethylene nonylpropenylphenyl ether and the like.

[0117] Although not particularly limited, in some embodiments, a reactive surfactant having an oxyethylene chain can be preferably used. Here, the oxyethylene chain refers to a repeating structure of an oxyethylene unit, i.e., -(C2H4O) n - represents a structural part. n represents the number of repetitions of the oxyethylene unit. For example, a reactive surfactant having a repetition number n of about 5 to 30 (e.g., 8 to 25) is preferred.

[0118] From the viewpoint of polymerization stability during emulsion polymerization, in some embodiments, a reactive surfactant having a propenyl group can be preferably used. In particular, a reactive surfactant having a propenyl group and an oxyethylene chain is preferably used.

[0119] From the viewpoint of emulsification performance, in some embodiments, an anionic reactive surfactant (e.g., an anionic reactive surfactant having an oxyethylene chain) may be preferably used. When the anionic reactive surfactant forms a salt, the salt is preferably a non-metallic salt, and ammonium salt is preferred.

[0120] When a nonionic reactive surfactant is used, more preferable results can be achieved by using it in combination with other surfactants such as anionic reactive surfactants, anionic non-reactive surfactants, nonionic non-reactive surfactants, and the like.

[0121] By making the monomer raw material emulsion polymerization under the presence of the reactive surfactant with free radical polymerizable functional group, the above-mentioned reactive surfactant can react and be introduced into the base polymer (for example acrylic acid series polymer).The reactive surfactant introduced into the acrylic acid series polymer is restricted in the movement in the adhesive layer, and is therefore not easy to ooze out on the surface of the adhesive layer.Therefore, by using a reactive surfactant, it is possible to suppress the oozing out of low molecular weight compounds to the surface of the adhesive layer.This point is preferably considered from the viewpoint of low pollution.From the viewpoint of realizing more excellent low pollution, it is possible to preferably adopt the mode of the surfactant when only using reactive surfactant as emulsion polymerization.

[0122] The amount of surfactant used is preferably set to about 0.1 weight part or more (e.g., about 0.5 weight part or more) relative to 100 weight parts of all monomer components. In addition, it is appropriate to set the amount of surfactant used to about 10 weight parts or less (e.g., about 5 weight parts or less) relative to 100 weight parts of all monomer components, or it can be about 4 weight parts or less.

[0123] The adhesive layer disclosed herein can include a base polymer in a ratio of about 50% by weight or more. The content ratio of the base polymer in the adhesive layer can be set to about 75% by weight or more, and about 85% by weight or more is appropriate. When using an adhesive with a content ratio of a base polymer of more than a specified ratio, there is a tendency to easily prevent or suppress the pollution of the surface of the protected object, and the stability of the adhesive properties over time is also excellent. In some preferred embodiments, the content ratio of the base polymer in the adhesive layer is about 90% by weight or more, more preferably about 95% by weight or more, further preferably about 97% by weight or more, or about 98% by weight or more (for example, about 99% by weight or more). The upper limit of the content ratio of the base polymer in the adhesive layer is 100% by weight, and in order to achieve target characteristics (such as anti-deterioration, adhesion, etc.), it can be less than 99.5% by weight, can be less than 98.5% by weight, or can be less than 97.5% by weight.

[0124] The adhesive layer of the protective sheet disclosed herein can be an adhesive layer formed by adhesive compositions of various forms. From the viewpoint of reducing environmental burden, it is preferred to adopt a water-dispersible adhesive composition in which at least a part of the adhesive is dispersed in water. As a suitable example of the water-dispersible adhesive composition, a water-dispersible adhesive composition (acrylic acid water-dispersible adhesive composition) containing an acrylic polymer as a base polymer can be cited. It should be noted that, as other forms of the adhesive composition, for example, a composition (solvent-based adhesive composition) in which an adhesive (adhesive component) is contained in an organic solvent can be cited, a composition (active energy ray-cured adhesive composition) prepared by curing to form an adhesive by active energy rays such as ultraviolet rays and radiation, a hot-melt adhesive composition formed by coating in a heated molten state and cooling to near room temperature, etc. It is possible to use a person formed by adding water in the non-aqueous dispersion adhesive composition.

[0125] (Crosslinking agent)

[0126] In the technology disclosed herein, the adhesive composition preferably used to form the adhesive layer contains a crosslinking agent. By using a crosslinking agent, the surface hardness of the adhesive layer can be appropriately adjusted. The type of the crosslinking agent used is not particularly limited and can be appropriately selected from existing known crosslinking agents.

[0127] As the specific example of crosslinking agent, oxazoline crosslinking agent, aziridine crosslinking agent, isocyanate crosslinking agent, epoxy crosslinking agent, melamine crosslinking agent, peroxide crosslinking agent, urea crosslinking agent, metal alkoxide crosslinking agent, metal chelate crosslinking agent, metal salt crosslinking agent, carbodiimide crosslinking agent, hydrazine crosslinking agent, amine crosslinking agent, silane coupling agent etc. can be listed. These crosslinking agents can be used alone or in combination of two or more. For example, preferably one or more selected from oxazoline crosslinking agent, aziridine crosslinking agent, isocyanate crosslinking agent and epoxy crosslinking agent is used. Among them, oxazoline crosslinking agent, isocyanate crosslinking agent, epoxy crosslinking agent are more preferably used. In the mode of using water-dispersible adhesive composition, it is preferred that the crosslinking agent be soluble or dispersed in water, particularly preferably the crosslinking agent (i.e. water-soluble) that can be dissolved in water.

[0128] As the oxazoline crosslinking agent, any crosslinking agent having one or more oxazoline groups in one molecule can be used without particular limitation. It is preferred to use an oxazoline crosslinking agent that is soluble or dispersible in water in the water-dispersible PSA composition.

[0129] Oxazoline radical can be any one in 2-oxazoline radical, 3-oxazoline radical, 4-oxazoline radical.Can preferably use the oxazoline system cross-linking agent with 2-oxazoline radical.For example, can use the water-soluble copolymer or the water-dispersible copolymer that the addition polymerization oxazoline such as 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline and other monomer copolymerization obtains as oxazoline system cross-linking agent.

[0130] Examples of commercially available oxazoline crosslinking agents include trade names “EPOCROS WS-500,” “EPOCROS WS-700,” “EPOCROS K-2010E,” “EPOCROS K-2020E,” and “EPOCROS K-2030E” manufactured by Nippon Shokubai Co., Ltd.

[0131] Examples of aziridine crosslinking agents include trimethylolpropane tris[3-(1-aziridinyl)propionate], trimethylolpropane tris[3-(1-(2-methyl)aziridinylpropionate)], etc. Commercially available aziridine crosslinking agents include, for example, trade names "Chemitite PZ-33" and "Chemitite DZ-22E" manufactured by Nippon Shokubai Co., Ltd.

[0132] As an example of an isocyanate crosslinking agent, a polyfunctional isocyanate compound having two or more functions can be used. Examples include aromatic isocyanates such as toluene diisocyanate, xylene diisocyanate, polymethylene polyphenyl diisocyanate, tris(p-isocyanatophenyl)thiophosphate, and diphenylmethane diisocyanate; alicyclic isocyanates such as isophorone diisocyanate; aliphatic isocyanates such as hexamethylene diisocyanate, etc. As commercially available products, isocyanate adducts such as trimethylolpropane / toluene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, trade name "Coronate HX") can be exemplified. In the water-dispersible adhesive composition, it is preferred to use an isocyanate crosslinking agent that is soluble or dispersible in water. For example, a water-soluble, water-dispersible or self-emulsifying isocyanate crosslinking agent can be preferably used. An isocyanate crosslinking agent of the so-called blocked isocyanate type in which the isocyanate group is blocked can be preferably used.

[0133] As the epoxy crosslinking agent, an epoxy crosslinking agent having two or more epoxy groups in one molecule can be used without particular limitation. An epoxy crosslinking agent having 3 to 5 epoxy groups in one molecule is preferred. In the water-dispersible pressure-sensitive adhesive composition, an epoxy crosslinking agent that is soluble or dispersible in water is preferably used.

[0134] Specific examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylene diamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, and polyglycerol polyglycidyl ether.

[0135] Commercially available products of epoxy crosslinking agents include "TETRAD-X" and "TETRAD-C" manufactured by Mitsubishi Gas Chemical Co., Ltd., "EPICLON CR-5L" manufactured by DIC Corporation, "DENACOL EX-512" manufactured by Nagase Chemtex Co., Ltd., and "TEPIC-G" manufactured by Nissan Chemical Industries, Ltd.

[0136] As a carbodiimide crosslinking agent, a low molecular compound or a high molecular compound having two or more carbodiimide groups can be used. In the water-dispersible adhesive composition, a carbodiimide crosslinking agent that is soluble or dispersible in water is preferably used. Commercially available products of carbodiimide crosslinking agents include, for example, CARBODILITE V series (aqueous solution type) such as "CARBODILITE V-02", "CARBODILITE V-02-L2", and "CARBODILITE V-04" manufactured by Nisshinbo Co., Ltd., and CARBODILITE E series (water dispersion type) such as "CARBODILITE E-01", "CARBODILITE E-02", and "CARBODILITE E-04".

[0137] The content of the cross-linking agent in the adhesive composition disclosed herein (the total amount of the cross-linking agent) is not particularly limited, and it can be considered that the composition and molecular weight of the base polymer are suitably set in a manner to obtain suitable characteristics after cross-linking. Although not particularly limited, the amount of the cross-linking agent relative to 100 parts by weight of the base polymer (typically an acrylic polymer) is, for example, about 0.01 parts by weight or more, about 0.1 parts by weight or more is suitable, preferably about 1 parts by weight or more (for example, about 2 parts by weight or more). In addition, from the viewpoints of adhesion, the amount of the above-mentioned cross-linking agent is set to about 15 parts by weight or less (preferably about 10 parts by weight or less, for example, about 5 parts by weight or less) relative to 100 parts by weight of the base polymer, and from the viewpoint of improving the adhesion with the adherend, preferably about 4 parts by weight or less, more preferably less than 3.5 parts by weight, and further preferably less than 3 parts by weight.

[0138] (Basic Compounds)

[0139] The adhesive composition disclosed herein (and thus the adhesive layer. The same shall apply below unless otherwise specified) may contain a basic compound. In the water-dispersible adhesive composition, the base polymer (e.g., an acrylic polymer) as the main component may be a polymer having an acidic group such as a carboxyl group. By using a basic compound for such a polymer, good coating properties and stability can be obtained through an acid-base neutralization reaction. Therefore, the basic compound can be used as a pH adjuster in the adhesive composition. It should be noted that the "basic compound" in this specification refers to a compound that exhibits alkalinity in the state of an aqueous solution.

[0140] As alkaline compounds, both organic alkaline compounds and inorganic alkaline compounds can be used. Examples of organic alkaline compounds include organic amine compounds such as alkanolamines, alkylamines, and polyalkylene polyamines. As inorganic alkaline compounds, ammonia; hydroxides, carbonates, and bicarbonates of ammonia, alkali metals, or alkaline earth metals; and the like can be listed. As specific examples of the above-mentioned hydroxides, potassium hydroxide and sodium hydroxide can be listed. As specific examples of the above-mentioned carbonates or bicarbonates, ammonium bicarbonate, ammonium carbonate, potassium bicarbonate, potassium carbonate, sodium bicarbonate, and sodium carbonate can be listed. They can be used alone or in combination of two or more. Among them, from the perspective of the ease of viscosity adjustment, dispersion stability, and coating properties of the adhesive composition, ammonia is preferred. As an alkaline compound (non-ammonia alkaline compound) to replace ammonia, there is no particular limitation, and alkali metal hydroxides and alkaline earth metal hydroxides are preferred, among which potassium hydroxide and sodium hydroxide are more preferred. Although not particularly limited, in a typical embodiment, ammonia is added to the adhesive composition in the form of aqueous ammonia, and sodium hydroxide may be added in the form of an aqueous sodium hydroxide solution.

[0141] The adhesive composition disclosed herein may contain ammonia, or may be substantially free of ammonia. In some embodiments, the adhesive composition contains ammonia. In this embodiment, the ammonia content in the adhesive composition can be set in a manner that the ammonia content of the adhesive layer measured by hot water extraction is less than a specified value (limitation of ammonia dosage). The limitation of ammonia dosage can also be implemented by the combined use of ammonia and non-ammonia alkaline compounds. Alternatively, the ammonia can be volatilized by appropriately setting the conditions of the treatment such as the drying process during the formation of the adhesive layer, and the ammonia content of the adhesive layer measured by hot water extraction is adjusted to be less than a specified value (ammonia reduction treatment). The limitation of ammonia dosage and the ammonia reduction treatment can also be used in combination. In other embodiments, the adhesive composition does not contain ammonia. In this embodiment, for example, as a pH adjuster, one or more non-ammonia alkaline compounds can be used. Alternatively, the technology disclosed herein can be implemented in a manner that the above-mentioned adhesive layer does not substantially contain non-ammonia alkaline compounds.

[0142] (pH of adhesive composition)

[0143] The pH of the adhesive composition disclosed herein (specifically, the liquid phase of the adhesive composition) is not particularly limited, and can be set to an appropriate range in consideration of coating properties, stability, storage properties, handling properties, etc. The pH of the adhesive composition can be set to about 11 or less. From the viewpoint of coating properties, about 10 or less is appropriate, and preferably about 9 or less (for example, about 8 or less) is appropriate. In addition, the pH of the adhesive composition can be set to about 5 or more, about 6 or more is appropriate, and from the viewpoint of coating properties, it is preferably 7 or more, and can be a basically neutral region (about 7 to 8). It is preferred that the pH of the adhesive composition is adjusted to within the above-specified range, and an adhesive layer is formed by an adhesive composition having a pH within the range. The pH of the adhesive composition can be set and adjusted based on the molecular design of the base polymer, the content ratio, the addition of a pH adjuster, and the like.

[0144] (Phosphate)

[0145] The adhesive composition (and thus the adhesive layer) disclosed herein may contain a phosphate ester. Examples of the phosphate ester include alkyl phosphates such as lauryl phosphate and lauryl phosphate, phosphates having an oxyethylene chain, and salts thereof. The salts may be, for example, sodium salts, potassium salts, barium salts, triethanolamine salts, and the like of the phosphate esters. Hereinafter, unless otherwise specified, "phosphate ester" is used in the sense of including salts. Among them, a phosphate ester having an oxyethylene chain is more preferably used. The phosphate ester having an oxyethylene chain mainly suppresses the increase in adhesive force over time (i.e., improves the stability of adhesive force) and can prevent corrosion-inducing components such as water, acid, and alkali from entering between the adhesive layer and the surface of the adherend. Here, the oxyethylene chain refers to a chain structure portion containing at least one ethylene oxide (EO) unit and may further contain other oxyethylene units (e.g., oxyethylene units having about 3 to 6 carbon atoms). As a suitable example of a phosphate ester having an oxyethylene chain, a phosphate ester having an EO unit or an oxyethylene chain formed by its repetition can be cited. For example, a phosphoric acid ester represented by the following general formula (a) or a salt thereof can be preferably used.

[0146]

[0147] In the above general formula (a), R 1 Indicates -OH or -(OCH2CH2) n OR 3 , R 2 Represents -(OCH2CH2) m OR 4 . n and m represent the number of moles of EO added. The number of moles of EO added n is an integer of 1 to 30, typically an integer of about 1 to 20, preferably an integer of about 1 to 10, for example, an integer of about 1 to 8. The number of moles of EO added n is preferably an integer of about 1 to 6, and more preferably an integer of about 1 to 4 (for example, 2 to 4). In the general formula (a), the number of moles of EO added m is typically approximately the same as the number of moles of EO added n, and n and m may be the same or different. The above R 3 and R 4 is a monovalent organic group (typically a hydrocarbon group), and may be, for example, independently selected from an alkyl group, a cycloalkyl group, an aryl group, an alkylaryl group, and an arylalkyl group. 3 , R 4 Preferably, it is a linear or branched alkyl group, aryl group or alkylaryl group. 3 , R 4 are each independently an organic group having 1 to 30 carbon atoms, and may be an organic group having 6 or more carbon atoms (preferably 8 or more, for example 11 or more). 3 , R 4The organic group may have a carbon number of 20 or less, preferably 18 or less, for example 15 or less. The salt of the phosphoric acid ester represented by the general formula (a) may be, for example, a sodium salt, potassium salt, barium salt, triethanolamine salt, etc. of these phosphoric acid esters. The phosphoric acid ester may be used alone or in combination of two or more.

[0148] Examples of the above-mentioned phosphate ester include polyoxyethylene tridecyl ether phosphate, polyoxyethylene lauryl ether phosphate, polyoxyethylene octadecyl ether phosphate and the like polyoxyethylene alkyl phosphate esters; polyoxyethylene nonylphenyl ether phosphate, polyoxyethylene octylphenyl ether phosphate, polyoxyethylene dinonylphenyl ether phosphate, polyoxyethylene dioctylphenyl ether phosphate and the like polyoxyethylene alkyl aryl ether phosphate esters; etc. In some embodiments, phosphate esters having a molecular weight of 150 to 5000 can be preferably used.

[0149] The amount of phosphate ester relative to 100 parts by weight of base polymer (e.g., acrylic acid polymer) can be, for example, set to about 0.05 parts by weight or more, preferably set to about 0.1 parts by weight or more, more preferably set to about 0.3 parts by weight or more (e.g., about 0.5 parts by weight or more). In addition, from the viewpoint of low contamination of the adherend surface, it is appropriate to set the amount of phosphate ester relative to 100 parts by weight of base polymer (e.g., acrylic acid polymer) to about 30 parts by weight or less (e.g., 20 parts by weight or less), preferably about 10 parts by weight or less, more preferably about 5 parts by weight or less, further preferably about 3 parts by weight or less, particularly preferably about 2 parts by weight or less (e.g., 1 part by weight or less), for example, it can also be 0.1 parts by weight or less. The technology disclosed herein can be implemented in a manner that the adhesive layer does not substantially contain phosphate ester from the viewpoint of non-contamination of the adherend.

[0150] (Rust Inhibitor)

[0151] The adhesive layer disclosed herein may or may not contain a rust inhibitor. Some preferred adhesive layers may contain a rust inhibitor. As rust inhibitors, there are no particular limitations, and examples thereof include: amine compounds, azole compounds, nitrites, ammonium benzoate, ammonium phthalate, ammonium stearate, ammonium palmitate, ammonium oleate, ammonium carbonate, dicyclohexylamine benzoate, urea, hexamethylenetetramine, thiourea, phenyl carbamate, cyclohexylammonium-N-cyclohexylcarbamate (CHC), etc. These rust inhibitors may be used alone or in combination of two or more. Among them, amine compounds and azole compounds are preferred.

[0152] The content of the rust inhibitor (e.g., amine compounds (amine rust inhibitors), azole compounds (azole rust inhibitors)) is not particularly limited, and can be, for example, 0.01 parts by weight or more (typically 0.05 parts by weight or more) relative to 100 parts by weight of the base polymer. From the viewpoint of obtaining a better effect of preventing corrosion, the above content can be 0.1 parts by weight or more, 0.3 parts by weight or more, or 0.5 parts by weight or more. On the other hand, from the viewpoint of preventing corrosion caused by the contained components and the cohesive force of the adhesive, it is appropriate to generally set the content of the rust inhibitor to less than 8 parts by weight relative to 100 parts by weight of the base polymer, and it can also be 6 parts by weight or less, preferably 5 parts by weight or less, for example, 3 parts by weight or less, or 1 part by weight or less. The technology disclosed herein can also be preferably implemented in a manner that substantially does not use a rust inhibitor.

[0153] (Other ingredients, etc.)

[0154] As required, the adhesive composition may contain a known tackifier such as a rosin-based tackifier, a terpene-based tackifier, a hydrocarbon-based tackifier, etc. From the viewpoint of avoiding excessive peel strength, the amount of the tackifier is preferably set to about 5 parts by weight or less, and more preferably about 1 part by weight or less relative to 100 parts by weight of the base polymer. The protective sheet disclosed herein can be preferably implemented without using a tackifier because the adhesive force can be effectively controlled by the composition of the base polymer, Tg, the gel fraction of the adhesive, etc.

[0155] As required, the above-mentioned adhesive composition can contain various arbitrary additives commonly used in the adhesive composition field such as viscosity modifier (thickener, etc.), crosslinking aid, plasticizer, softener, filler, antistatic agent, anti-aging agent, ultraviolet absorber, antioxidant, light stabilizer, defoamer, etc. In addition, as the above-mentioned arbitrary additive, any polymer component different from the base polymer (such as acrylic polymer) can be used. As the content of such arbitrary polymer, in the adhesive composition, it is usually about 10 weight % or less, for example, about 1 weight % or less, and the adhesive composition disclosed here can also be substantially free of the above-mentioned arbitrary polymer. In addition, for an adhesive composition of one mode, relative to 100 weight parts of the base polymer, the content of plasticizers such as fatty acid esters can be limited to, for example, less than 10 weight parts (for example, less than 1 weight part). Typically, the adhesive composition can be substantially free of plasticizers. In addition, the technology disclosed here can preferably be implemented in a manner that is substantially free of antistatic agents (which can be conductive agents) such as ionic compounds (such as ionic liquids, alkali metal salts). Regarding other matters related to the above-mentioned various optional additives, various conventionally known additives, various methods, etc. can be appropriately adopted based on common technical knowledge, but since they are not the characteristics of the present invention, their detailed description is omitted.

[0156] In the technology disclosed herein, in the form of using a water-dispersed adhesive composition for forming an adhesive layer, the adhesive composition can be prepared by mixing other components (e.g., a cross-linking agent, etc.) used as needed in an aqueous dispersion of an acrylic polymer obtained by emulsion polymerization using a surfactant. For example, a polymerization reaction liquid obtained by emulsion polymerization can be used, and the polymerization reaction liquid can be subjected to treatments such as pH adjustment (e.g., neutralization), adjustment of the non-volatile content, and adjustment of viscosity as needed.

[0157] Although not particularly limited, for example, from the viewpoint of drying efficiency, the nonvolatile content (NV) of the adhesive composition can be set to about 20 weight % or more (typically about 30 weight % or more, preferably about 40 weight % or more). In addition, from the viewpoint of coating properties, it can be set to about 75 weight % or less (typically about 70 weight % or less, preferably about 60 weight % or less).

[0158] (Formation of Adhesive Layer)

[0159] The formation of adhesive layer can be carried out according to the adhesive layer formation method in the known adhesive sheet.Can preferably adopt for example by directly giving (typically coating) adhesive composition on substrate and making it dry and forming the method (direct method) of adhesive layer.In addition, also can adopt to give adhesive composition and make it dry to the surface (peeling surface) with peelability, form adhesive layer on this surface, and this adhesive layer is transferred to the method (transfer method) of substrate.As above-mentioned peeling surface, can utilize the surface of release liner, the substrate back side of having been peeled off etc..Adhesive layer typically is formed continuously, but also can form the rule or irregular pattern such as dot-shaped, stripe-shaped according to purpose, purposes.

[0160] The coating of the adhesive composition can be carried out using a known or commonly used coating machine such as a gravure roll coater, a reverse roll coater, a lick coater, a comma coater, a dip roll coater, a die coater, a rod coater, a knife coater, a spray coater, etc. Alternatively, the adhesive composition can be applied by impregnation, a curtain coating method, etc. From the perspectives of promoting the cross-linking reaction and improving the manufacturing efficiency, it is preferred that the drying of the adhesive composition is carried out under heating. The drying temperature can be set to, for example, about 40°C to 150°C, and is usually preferably set to about 50°C to 130°C (for example, 60°C to 100°C). After the adhesive composition is dried, it can be further aged for the purpose of adjusting the transfer of components in the adhesive layer, carrying out the cross-linking reaction, and relaxing the strain that may be present in the substrate and the adhesive layer.

[0161] (Chloride ion amount)

[0162] In the adhesive layer disclosed here, the amount of chloride ions measured by hot water extraction is not particularly limited. In some embodiments, the amount of chloride ions per 1g of adhesive (layer) can be 350μg or less. By using an adhesive layer that limits the amount of chloride ions in this way, there is a tendency to prevent corrosion in the Low-E glass plate that is the object of protection. It is appropriate that the amount of chloride ions per 1g of adhesive (layer) is about 300μg or less, and can be about 200μg or less (for example, about 150μg or less). By limiting the amount of chloride ions in the adhesive in contact with the Low-E glass plate, a structure that is easy to prevent corrosion in the Low-E glass plate for a long time can be obtained. In some preferred embodiments, the amount of chloride ions per 1g of adhesive (layer) is about 100μg or less, more preferably about 95μg or less, further preferably about 90μg or less, particularly preferably about 85μg or less, and can also be about 75μg or less (about 70μg or less). The lower limit of the amount of chloride ions per 1g of adhesive (layer) is ideally 0μg, but from the perspective of production efficiency, practical permissible levels, etc., it can be about 1μg or more, about 10μg or more, or about 50μg or more. In other embodiments, the amount of chloride ions per 1g of adhesive (layer) can be about 80μg or more, or about 100μg or more (for example, about 120μg or more). According to the technology disclosed herein, it is possible to achieve good corrosion resistance for an adhesive layer containing chloride ions at the above concentration without damaging the adhesive properties. The amount of chloride ions in the adhesive can be adjusted by using a component with a small amount of chloride ions, performing chloride ion removal treatment on components such as water, and the like.

[0163] The chloride ion amount of the adhesive layer can be measured by the following method. Alternatively, the chloride ion amount in the protective sheet and the base material layer constituting the protective sheet can be measured by hot water extraction, and the chloride ion amount from the adhesive layer can be calculated based on the difference between the chloride ion amounts of the two, and the obtained value can be converted into a value per unit adhesive (layer) to obtain the chloride ion amount.

[0164] [Chloride ion content of adhesive (layer)]

[0165] Prepare about 10 mg of the adhesive component of the protective sheet to be measured, put it in a polypropylene (PP) container and weigh it. Then, add 100 mL of ultrapure water and cover it, and perform heating extraction in a 120°C dryer for 1 hour. The amount of chloride ions in the obtained extract is quantified by ion chromatography using a commercially available chloride ion standard solution (obtained from FUJIFILM Wako PureChemical Corporation) to determine the amount of chloride ions per 1 g of adhesive used in the extraction. The ion chromatography measurement conditions are as follows.

[0166] (Measurement conditions)

[0167] Anion analysis:

[0168] Apparatus: "ICS-3000" manufactured by Thermo Fisher Scientific

[0169] Separation column: Dionex IonPac AS18-fast (4mm×250mm)

[0170] Guard column: Dionex IonPac AG18-fast (4mm×50mm)

[0171] Removal system: Dionex AERS-500 (external mode)

[0172] Detector: Conductivity detector

[0173] Eluent: KOH aqueous solution (using eluent generator box)

[0174] Eluent flow rate: 1.0mL / min

[0175] Sample injection volume: 250μL

[0176] Cation analysis:

[0177] Device: "DX-320" manufactured by Thermo Fisher Scientific

[0178] Separation column: Dionex Ion Pac CS16 (5mm×250mm)

[0179] Guard column: Dionex Ion Pac CG16 (5mm×50mm)

[0180] Removal system: Dionex CSRS-500 (recirculation mode)

[0181] Detector: Conductivity detector

[0182] Eluent: Methanesulfonic acid aqueous solution

[0183] Eluent flow rate: 1.0mL / min

[0184] Sample injection volume: 25μL

[0185] (Adhesive layer thickness)

[0186] The thickness of the adhesive layer constituting the protective sheet disclosed herein is not particularly limited. From the viewpoint of preventing residual adhesive on the adherend, the thickness of the above-mentioned adhesive layer is appropriately about 50 μm or less, about 30 μm or less, preferably about 15 μm or less, and more preferably about 8 μm or less (for example, less than 6 μm). In some embodiments, from the viewpoint of peelability, the thickness of the adhesive layer is appropriately about 5 μm or less, and can be about 4 μm or less, for example, 3 μm or less. In addition, from the viewpoint of adhesion, the thickness of the adhesive layer is appropriately about 0.5 μm or more, preferably about 1 μm or more, and more preferably more than 2 μm. The thickness of the adhesive layer may exceed 3 μm, for example, it may exceed 4 μm.

[0187] <Base material layer>

[0188] The protective sheet disclosed herein may include a substrate layer. As the substrate layer, a resin film, a rubber sheet, a foam sheet, a composite thereof, etc. may be used. As examples of rubber sheets, natural rubber sheets, butyl rubber sheets, etc. may be cited. As examples of foam sheets, foamed polyurethane sheets, foamed chloroprene rubber sheets, etc. may be cited.

[0189] The technology disclosed herein can be preferably applied to a protective sheet using a resin film as a substrate layer. The "resin film" mentioned here is typically a film formed by molding a resin composition having a resin component as shown below as the main body into a film shape, which is different from the so-called non-woven fabric and woven fabric (that is, the concept other than non-woven fabric and woven fabric). It is substantially preferably a non-foamed resin film. Here, the non-foamed resin film refers to a resin film that has not been intentionally treated to form a foam body, specifically, it can be a resin film with a foaming ratio of less than about 1.1 times (for example, less than 1.05 times, typically less than 1.01 times).

[0190] As examples of resin components constituting resin films, polyolefin resins (polyethylene, polypropylene, ethylene-propylene copolymers, ethylene-vinyl acetate copolymers, etc.), polyvinyl chloride resins (typically soft polyvinyl chloride resins), polyvinyl acetate resins, polyurethane resins (ether polyurethanes, ester polyurethanes, carbonate polyurethanes, etc.), carbamate (methyl) acrylate resins, thermoplastic elastomers (olefin elastomers, styrene elastomers, acrylic elastomers, etc.), polyester resins (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, etc.), polycarbonate resins, polyamide resins, polyimide resins, fluorine resins, cellophane resins, and other cellulose resins. These resin components can be used alone or in combination. As preferred examples of resin films, polyolefin resin films, polyester resin films, and vinyl chloride resin films can be listed.

[0191] Although not particularly limited, in some forms of the protective sheet, a substrate layer containing one or more resin components selected from the group consisting of polyolefin resins, polyvinyl chloride resins, polyurethane resins, thermoplastic elastomers and polyester resins as the main component (typically a substrate layer containing the resin components in a ratio of more than 50% by weight) can be preferably used. In other forms, considering performance, handling, cost, etc., a substrate layer containing a polyolefin resin layer, a polyester resin layer or a polyvinyl chloride resin layer can be preferably used. Among the above-mentioned resin materials, polyolefin resins, polyurethane resins and olefin elastomers are preferred from the perspectives of thermal stability and lightness, and polyolefin resins and olefin elastomers are particularly preferred from the perspectives of handling.

[0192] The protective sheet disclosed herein can be preferably implemented in a manner that includes a substrate layer containing a polyolefin resin as a main component (containing a proportion of more than 50% by weight), that is, a polyolefin resin film as a substrate layer. For example, a polyolefin resin film in which more than 50% by weight of the entire substrate layer is polyethylene (PE) resin or polypropylene (PP) resin can be preferably used. In other words, the above-mentioned polyolefin resin film can be a polyolefin resin film in which the total amount of PE resin and PP resin occupies more than 50% by weight of the entire substrate layer. The above-mentioned polyolefin resin film can be a blend of PE resin and PP resin.

[0193] The PP resin may be a PP resin having various polymers (propylene-based polymers) containing propylene as a constituent monomer as the main component. It may be a PP resin substantially composed of one or more propylene-based polymers. The concept of the propylene-based polymer described here includes random copolymers (random polypropylene) and block copolymers (block polypropylene) of propylene and other monomers in addition to homopolypropylene. The concept of the propylene-based polymer described here includes, for example, the following propylene-based polymers.

[0194] Homopolymers of propylene (homopolypropylene), for example isotactic polypropylene.

[0195] A random copolymer of propylene and other α-olefins (typically one or more selected from ethylene and α-olefins having 4 to 10 carbon atoms) (random polypropylene), preferably a random polypropylene having propylene as the main monomer (main constituent monomer, i.e., a component accounting for 50% by weight or more of the total monomers).

[0196] A copolymer (block polypropylene) obtained by block copolymerizing propylene with another α-olefin (typically one or more selected from ethylene and α-olefins having 4 to 10 carbon atoms). Preferably, the block polypropylene comprises propylene as the main monomer (main constituent monomer, i.e., the component accounting for 50% by weight or more of the total monomers).

[0197] The PE resin may be a PE resin having various polymers (ethylene polymers) containing ethylene as a constituent monomer as the main component. It may be a PE resin substantially composed of one or more ethylene polymers. The ethylene polymer may be a homopolymer of ethylene, or a copolymer obtained by copolymerizing (random copolymerization, block copolymerization, etc.) other α-olefins as secondary monomers with ethylene as the main monomer. Preferred examples of the α-olefins include α-olefins having 3 to 10 carbon atoms such as propylene, 1-butene (which may be branched 1-butene), 1-hexene, 4-methyl-1-pentene, and 1-octene. For example, it may be preferred to use a PE resin having an ethylene polymer as the main component obtained by copolymerizing the α-olefins as secondary monomers at a ratio of about 10% by weight or less (typically about 5% by weight or less).

[0198] In addition, the PE resin may be a PE resin of a copolymer of a monomer (functional group-containing monomer) and ethylene in addition to a polymerizable functional group, a PE resin obtained by copolymerizing the functional group-containing monomer with an ethylene polymer, etc. As copolymers of ethylene and functional group-containing monomers, for example, ethylene-vinyl acetate copolymers (EVA), ethylene-acrylic acid copolymers (EAA), ethylene-methacrylic acid copolymers (EMAA), ethylene-methyl acrylate copolymers (EMA), ethylene-ethyl acrylate copolymers (EEA), ethylene-methyl methacrylate copolymers (EMMA), copolymers obtained by crosslinking ethylene-(meth)acrylic acid (i.e., acrylic acid and / or methacrylic acid) copolymers with metal ions, etc. may be cited.

[0199] The density of the PE resin is not particularly limited. The concept of the PE resin described herein includes any polyethylene among high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE). In some embodiments, the density of the above PE resin can be, for example, 0.90 to 0.94 g / cm 3As preferred PE resins, LDPE and LLDPE can be cited. The above-mentioned PE resin may contain one or more LDPE and one or more LLDPE. The blending ratio of each LDPE or LLDPE, and the blending ratio of LDPE and LLDPE are not particularly limited, and can be appropriately set in a manner to become a PE resin showing the desired characteristics. As the base material layer of the protective sheet disclosed herein, a polyethylene resin film such as an LLDPE film containing LLDPE at a ratio of more than 50% by weight (preferably about 75% by weight or more, for example, about 90% by weight or more), and an LDPE film containing LDPE at a ratio of more than 50% by weight (preferably about 75% by weight or more, for example, about 90% by weight or more) can be preferably used. A laminated resin film containing the polyethylene resin film as a constituent element may also be used.

[0200] As required, the resin film (e.g., polyolefin resin film) used as the substrate layer of the protective sheet disclosed herein may contain suitable components allowed to be contained in the substrate layer. For example, fillers, colorants (pigments such as inorganic pigments, dyes), antioxidants, light stabilizers (including free radical scavengers, ultraviolet absorbers, etc.), antistatic agents, plasticizers, slip agents, anti-blocking agents and other additives may be appropriately mixed. The mixing amount of each additive may be set to the same degree as the usual mixing amount in the field of resin films used as substrate layers of protective sheets, etc.

[0201] The substrate layer may be a single-layer structure or a multi-layer structure of 2, 3 or more layers. In the case of a multi-layer structure, it is preferred that at least one layer (preferably all layers) is any of the above-mentioned resin films. For example, it is preferred that more than 75% (more preferably more than 90%) of the thickness of the substrate layer is formed by a single layer or multiple layers (typically a single layer) of a polyolefin resin film. It is also possible that the entire substrate layer is formed by a single layer or multiple layers of a polyolefin resin film. From the viewpoint of economy, it is preferred to use a substrate layer formed by a single-layer resin film (for example, LLDPE film, LDPE film, etc.).

[0202] The manufacture method of substrate layer is suitable to adopt existing known method, is not particularly limited.For example, when adopting resin film as substrate layer, the resin film that is suitable to adopt existing known general film forming method making such as inflation molding, extrusion molding, T-die casting molding, calendering roll molding can be used.

[0203] In the configuration in which at least one side of the substrate layer (the side on the adhesive layer side) is the surface of the resin film, the surface of the resin film may be subjected to a known surface treatment such as corona discharge treatment, plasma treatment, ozone exposure, flame exposure, ultraviolet irradiation treatment, acid treatment, alkali treatment, and application of a primer. Such a surface treatment may be a treatment for improving the adhesion between the substrate layer and the adhesive layer, in other words, the anchoring property of the adhesive layer to the substrate layer. In the method of using a polyolefin resin film as the substrate layer, it is particularly meaningful to implement the above-mentioned surface treatment.

[0204] The thickness of the substrate layer constituting the protective sheet disclosed herein is not particularly limited. The thickness of the above-mentioned substrate layer can be, for example, about 800 μm or less (typically about 250 μm or less). In some embodiments, the thickness of the substrate layer (typically a non-foamed resin film) is preferably about 150 μm or less, more preferably about 100 μm or less, further preferably less than 65 μm, for example, less than 55 μm. When the thickness of the substrate layer becomes smaller, the followability of the protective sheet to the shape of the adherend is improved, and there is a tendency to suppress floating and peeling. In addition, from the perspective of protection and operability of the adherend, the thickness of the substrate layer is typically about 10 μm or more, preferably about 25 μm or more, more preferably more than 30 μm, further preferably more than 40 μm, for example, more than 45 μm.

[0205] <Properties of the protective sheet>

[0206] (Initial adhesion to glass)

[0207] The protective sheet disclosed herein is attached to the Low-E glass plate and the initial peel strength (initial adhesion to the glass) measured at a tensile speed of 0.3m / min and a peeling angle of 180 degrees after 30 minutes is about 0.01N / 20mm or more. It is appropriate. In some embodiments, the above-mentioned initial peel strength can be about 0.05N / 20mm or more (for example, about 0.1N / 20mm or more). In some preferred embodiments, the above-mentioned initial peel strength is about 0.5N / 20mm or more (for example, about 1N / 20mm or more), and can also be about 1.5N / 20mm or more. The protective sheet showing the above-mentioned initial peel strength is well bonded to the adherend in a relatively short time after being attached to the adherend, and is not easy to produce floating peeling from the adherend, etc., and can play a good protective performance. The upper limit of the above-mentioned initial peel strength is not particularly limited. From the perspective of light peelability, it is appropriate to be about 5N / 20mm or less, preferably about 2.5N / 20mm or less (for example, about 2N / 20mm or less). The initial peel strength is measured by the following method.

[0208] [Initial peel strength]

[0209] The protective film to be measured was cut into strips with a width of 20 mm and a length of 100 mm to prepare a test piece. Under a standard environment of 23°C and 50% RH, a 2kg rubber roller was reciprocated twice to press the test piece onto a Low-E glass plate as an adherend. After the sample was kept in the above-mentioned standard environment for 30 minutes, a universal tensile testing machine was used in the standard environment to measure the initial peel strength (initial adhesion to glass) [N / 20mm] at a tensile speed of 0.3 m / min and a peeling angle of 180 degrees. As a Low-E glass plate, the model "RSFL6AS" (100mm×100mm) manufactured by Nippon Sheet Glass Co., Ltd. was used. It should be noted that as an adherend, any Low-E glass plate can be used without restriction, and equivalents of the above-mentioned products or other commercially available Low-E glass plates can also be used.

[0210] (Adhesion to glass over time)

[0211] The protective sheet disclosed herein is preferably about 5N / 20mm or less when measured at a tensile speed of 0.3m / min and a peeling angle of 180 degrees after being attached to a Low-E glass plate and stored at 50°C for 7 days. The time-dependent peel strength (time-dependent adhesion to glass) is preferably about 5N / 20mm or less. Even if the protective sheet that meets this characteristic is attached to the adherend for a relatively long period of time, the time-dependent adhesion can be fully suppressed, and the light peelability from the adherend can be maintained. Therefore, the removal operability from the adherend is excellent. When a protective sheet having the above-mentioned time-dependent peel strength of about 4N / 20mm or less (more preferably about 2N / 20mm or less) is used, better peeling operability can be achieved. In addition, from the perspective of suppressing the floating peeling during the protection period of the adherend (for example, when processing the adherend with the protective sheet attached), the above-mentioned time-dependent peel strength is about 0.05N / 20mm or more, preferably about 0.1N / 20mm or more, and more preferably about 0.3N / 20mm or more. The peel strength over time may be about 1 N / 20 mm or more. The peel strength over time is measured by the following method.

[0212] [Peel strength over time]

[0213] The protective film to be measured was cut into strips with a width of 20 mm and a length of 100 mm to prepare a test piece. Under a standard environment of 23°C and 50% RH, a 2kg rubber roller was reciprocated twice to press the test piece onto a Low-E glass plate as an adherend. The sample was stored in an environment of 50°C for 7 days, and then kept in a standard environment of 23°C and 50% RH for 1 hour. In this standard environment, a universal tensile testing machine was used to measure the time-dependent peel strength (time-dependent adhesion to glass) [N / 20mm] at a tensile speed of 0.3 m / min and a peeling angle of 180 degrees. The Low-E glass plate used as an adherend was the same as the initial peel strength measurement mentioned above.

[0214] (Peel strength ratio)

[0215] Although not particularly limited, the ratio of the time-dependent peel strength P2 [N / 20mm] of the protective sheet disclosed herein to the initial peel strength P1 [N / 20mm] (i.e., the P2 / P1 ratio) can be 5 times or less. A small P2 / P1 ratio means that the peel strength increases less over time. Thus, both the initial adhesion and the light peelability during the peeling operation can be well balanced. From this point of view, the P2 / P1 ratio is preferably less than 4, more preferably less than 3, further preferably less than 2, for example, it can be less than 1.8, it can also be less than 1.5, and further can be less than 1.3. In addition, the P2 / P1 ratio is typically greater than 0.8, for example, it can be greater than 1.

[0216] (VOC emission amount)

[0217] From the viewpoint of environmental hygiene, for the protective sheet disclosed herein, the total amount of volatile organic compounds (VOC: volatile organic compounds) emitted from 1 g of the protective sheet (which may include a substrate layer and an adhesive layer, but does not include a release liner) when the protective sheet is heated at 80°C for 30 minutes (hereinafter sometimes referred to as VOC emission) is preferably 1000 μg (hereinafter sometimes recorded as "μg / g") or less. The above-mentioned VOC emission is more preferably 500 μg / g or less (for example, 300 μg / g or less, typically 100 μg / g or less). The VOC emission is measured by the following method.

[0218] [VOC measurement test]

[0219] Cut the protective sheet into the specified size (here the area is about 5cm 2size), peel off the release liner and use it as a sample piece, put the sample piece into a 20mL vial and cover it tightly. Next, heat the vial at 80°C for 30 minutes, and use a headspace autosampler (HSS) to inject 1.0mL of the heated gas (sample gas) into a gas chromatography (GC) measuring device. Based on the obtained gas chromatogram, the amount of gas generated from the sample piece is calculated in terms of n-decane conversion. Based on the obtained value, the VOC emission (μg / g) per 1g of protective sheet (excluding the release liner) is calculated. It should be noted that the n-decane conversion is calculated by setting the detection intensity of the generated gas obtained by GC Mass to the detection intensity of n-decane and applying a pre-made standard curve for n-decane. The settings of HSS and GC are as follows.

[0220] HSS: Model "7694" manufactured by Agilent Technologies

[0221] Heating time: 30 minutes

[0222] Pressurization time: 0.12 minutes

[0223] Cycle filling time: 0.12 minutes

[0224] Cycle equilibration time: 0.05 minutes

[0225] Injection time: 3 minutes

[0226] Sample cycle temperature: 160°C

[0227] Conveyor line temperature: 200°C

[0228] GC device: Model "6890" manufactured by Agilent Technologies

[0229] Column: J&W capillary column manufactured by GL Sciences, trade name "DB-WAP" (inner diameter 0.533 mm×length 30 m, film thickness 1.0 μm)

[0230] Column temperature: 250°C (increased from 40°C to 90°C at 10°C / min, then increased to 250°C at 20°C / min and maintained for 5 minutes)

[0231] Column pressure: 24.3 kPa (constant flow mode)

[0232] Carrier gas: Helium (5.0mL / min)

[0233] Inlet: split (split ratio 12:1)

[0234] Inlet temperature: 250℃

[0235] Detector: FID

[0236] Detector temperature: 250°C

[0237] The protective sheet disclosed herein may be a protective sheet having anti-deterioration properties evaluated as not discoloring in a Low-E glass plate discoloration evaluation test (40°C 92% RH × 2 weeks) performed by the method described in the examples described later. A protective sheet satisfying this property can exhibit excellent anti-deterioration properties in the application of protecting Low-E glass plates.

[0238] <Purpose>

[0239] The protective sheet disclosed herein is suitable as a protective sheet for glass plates used as building materials such as window glass. The glass plate to be attached may be a Low-E glass plate having a Low-E layer on its surface. The Low-E layer disclosed herein contains a zinc component, but is not particularly limited otherwise. For the Low-E layer containing a zinc component that causes deterioration due to ammonia, the effect of preventing and inhibiting deterioration brought about by the technology disclosed herein can be exerted. A typical Low-E layer includes a metal layer, an oxide layer such as a metal oxide layer, a nitride layer such as a silicon nitride layer, and the like, and generally has a multilayer structure, which can be formed by a known or customary method such as sputtering. Examples of the materials constituting each layer of the Low-E layer include TiO2, ZrO2, SiO2, and the like. X N Y 、ZnO X 、Ag、NiCrO X , SnO2, ZTO (zinc and tin oxides), etc. As the infrared reflection layer, it is preferred to use an Ag layer. The Ag layer can be a layer formed by a single substance of Ag, or a layer formed by an alloy of Ag and other metals (such as Pd). The Low-E layer can typically have one or more layers containing zinc components. Although not particularly limited, in some forms of the Low-E layer, the Ag layer can be sandwiched between a TiO2 layer, a ZrO2 layer, a ZnO X Layer, NiCrO X Layer, SnO2 layer, ZTO layer and other oxide layers, Si X N Y The outermost surface of the Low-E layer (the surface to which the protective sheet is attached) is mostly made of TiO2, ZrO2, ZnO X 、NiCrO X , SnO2, ZTO and other oxides, Si X N Y Nitrides such as Ag are usually not metals. The Low-E layer can have a multilayer structure of more than 5 layers, for example, more than 10 layers, or more than 15 layers, depending on the purpose and required characteristics. The thickness of each layer is not particularly limited, but is usually Below, about is appropriate, for example, for about The thickness (total thickness) of the Low-E layer may be approximately 10 nm to 1000 nm (eg, approximately 50 to 500 nm).

[0240] In the embodiment in which the Low-E layer of the Low-E glass plate has a layer containing a zinc component, the thickness of the layer containing a zinc component is, for example, about 100 nm or less, about 70 nm or less (for example, about 30 nm or less), and is, for example, about 1 nm or more, about 3 nm or more (for example, about 8 nm or more). As a typical example of the layer containing a zinc component, a layer containing zinc oxide can be cited. The layer containing zinc oxide can be a layer containing zinc oxide or a layer containing an oxide of zinc and another element (for example, tin).

[0241] The above-mentioned layer containing zinc component can exist on the outer surface (outermost) of the Low-E layer, and can also exist inside the Low-E layer. In the mode that the layer containing zinc component exists inside the Low-E layer, the distance (thickness) from the outer surface of the Low-E layer to the layer containing zinc component is not particularly limited, and for example, it is appropriate to be below about 300nm, and below about 200nm (for example, below about 100nm). Such a structure can preferably exert the effect brought by the technology disclosed herein. The lower limit of the distance (thickness) from the outer surface of the Low-E layer to the layer containing zinc component is not particularly limited, and for example, it is above about 1nm, and can be above about 10nm.

[0242] In the manufacture of the above-mentioned glass plate, the Low-E layer forming surface can be exposed until the two glass plates including the Low-E glass plate are formed into double-layer glass in a manner in which the Low-E layer side surface faces inward. For the purpose of preventing the Low-E layer forming surface from deteriorating, it is preferred to use the protective sheet disclosed herein. That is, the protective sheet can be used as a protective sheet for the Low-E layer forming surface. The Low-E glass plate to which the protective sheet is attached can be in the form of a laminated body formed by laminating the Low-E glass plate and the protective sheet during the protection period. Therefore, according to the technology disclosed herein, a laminated body having a Low-E glass plate and a protective sheet is provided. The details of the Low-E glass plate and the protective sheet are as described above, so they are not repeated.

[0243] In the above-mentioned laminate, the protective sheet is preferably attached to the Low-E glass plate with a 180-degree peel strength of less than 5N / 20mm. From the viewpoint of light peelability, the above-mentioned peel strength is more preferably about 2.5N / 20mm or less (for example, about 2N / 20mm or less). The above-mentioned peel strength is, for example, about 0.01N / 20mm or more, about 0.05N / 20mm or more (for example, about 0.1N / 20mm or more) is appropriate. From the viewpoint of the close adhesion between the Low-E glass plate and the protective sheet, it is preferably about 0.5N / 20mm or more (for example, about 1N / 20mm or more), and can be about 1.5N / 20mm or more. The protective sheet laminated on the Low-E glass plate with the above-mentioned peel strength is not prone to floating and peeling from the Low-E glass plate, and can exert good protective performance. For the measurement conditions of the above-mentioned peel strength, a protective sheet attached to the Low-E glass plate is used as the measurement object, and the peeling conditions basically the same as those for the measurement of the above-mentioned initial peel strength are adopted. The peel strength [N / 20 mm] is determined by dividing the measured value [N] by the actual measurement width [mm] and multiplying the value by 20 [mm].

[0244] In addition, the protective sheet disclosed herein is preferably used for the surface of the adherend of a large area where the peel strength is often limited from the aspect of removal operability. The protective sheet disclosed herein is preferably used in a manner that covers the entire surface of the adherend with a width of about 1m or more, for example, about 1.5m or more, and then about 2m or more (typically about 3m or more, and then about 3.3m or more). The length of the adherend surface is equal to or above the above-mentioned width. In some preferred embodiments, it is preferably used in a manner that covers the entire surface of a large-area flat plate (suitably a flat plate with a smooth surface) as described above. In particular, from the perspective of efficiency such as production and transportation, glass plates for building materials such as window glass are becoming large-area. It can be preferably used in a manner that covers the entire surface of a glass plate with such a large area (for example, a surface width exceeding 2.6m, typically a surface width of about 3m or more, and then about 3.3m or more) (typically the entire Low-E layer forming surface of a Low-E glass plate). According to a preferred embodiment of the technology disclosed herein, it is possible to achieve excellent deterioration resistance while maintaining easy releasability on an adherend having a large area as described above.

[0245] Furthermore, the protective sheet disclosed herein can be a protective sheet whose adhesive force is suppressed over time, so even if the attachment period (or the protection period of the adherend) to the adherend becomes relatively long (typically more than 2 weeks, for example more than 4 weeks), good removal operability can be exerted. Therefore, even if the period from attachment to the adherend (specifically, a Low-E glass plate) to removal from the adherend is more than 2 weeks (for example more than 4 weeks), it can be appropriately used.

[0246] Compared with conventional glass sheets, Low-E glass sheets have higher heat insulation and thermal insulation properties, and can improve the cooling and heating efficiency of indoor spaces, so they are widely used as building materials such as window glass. The technology disclosed herein can indirectly contribute to energy conservation and reduction of greenhouse gas emissions by being used in the manufacture of such materials.

[0247] Matters disclosed by this specification include the following aspects.

[0248] (1) A method for manufacturing a glass unit, comprising:

[0249] Step (A), preparing a Low-E glass plate having a Low-E layer;

[0250] Step (B), attaching a protective sheet to the surface of the Low-E layer of the Low-E glass plate;

[0251] The optional step (C) is to perform at least one selected from the group consisting of transportation, storage, processing, cleaning and operation on the Low-E glass plate to which the protective sheet is attached;

[0252] Step (D), removing the protective sheet from the Low-E glass plate; and

[0253] Step (E), assembling a glass unit using the aforementioned Low-E glass sheet;

[0254] The protective sheet comprises an adhesive layer.

[0255] The aforementioned Low-E layer contains zinc.

[0256] The ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g based on the weight of the adhesive layer.

[0257] (2) The method according to (1) above, wherein the Low-E glass plate has a width of 1 m or more.

[0258] (3) The method according to (1) above, wherein the Low-E glass plate has a width of 2 m or more.

[0259] (4) The method according to (1) above, wherein the Low-E glass plate has a width exceeding 2.6 m.

[0260] (5) The method according to (1) above, wherein the Low-E glass plate has a width of 3 m or more.

[0261] (6) The method according to any one of (1) to (5) above, wherein the Low-E layer includes a layer containing a zinc component.

[0262] (7) The method according to any one of (1) to (5) above, wherein the Low-E layer includes a zinc oxide layer.

[0263] (8) The method according to any one of (1) to (7) above, wherein the thickness of the Low-E layer is 1000 nm or less.

[0264] (9) The method according to any one of (1) to (8) above, wherein the step (B) includes a step of covering the entire surface of one surface of the Low-E glass plate with at least one protective sheet.

[0265] (10) The method according to any one of (1) to (9) above, wherein the step (C) is an essential step, and in the step (C), the Low-E glass plate is cleaned with water.

[0266] (11) A method for protecting a Low-E glass plate, comprising the step of attaching a protective sheet to a surface of a Low-E glass plate having a Low-E layer (attaching step),

[0267] Here, the protective sheet comprises an adhesive layer.

[0268] The aforementioned Low-E layer contains zinc.

[0269] The ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g based on the weight of the adhesive layer.

[0270] (12) The method according to (11) above, further comprising a step of removing the protective sheet from the Low-E glass plate (removal step).

[0271] At least one step selected from the group consisting of conveying, storing, processing, cleaning and handling of the Low-E glass plate to which the protective sheet is attached may be optionally included between the attaching step and the removing step.

[0272] (13) The method according to (11) or (12) above, wherein the Low-E glass sheet has a width of 1 m or more,

[0273] The attaching step includes a step of covering the entire one surface of the Low-E glass plate with at least one protective sheet.

[0274] (14) The method according to any one of (1) to (13) above, wherein the protective sheet is attached to the Low-E glass plate with a 180-degree peel strength of 5 N / 20 mm or less.

[0275] (15) The method according to any one of (1) to (14) above, wherein the PSA layer is a PSA layer formed from a water-dispersible PSA composition.

[0276] (16) The method according to (15) above, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer containing an acrylic polymer or a rubber pressure-sensitive adhesive layer containing a rubber polymer.

[0277] (17) The method according to any one of (1) to (16) above, further comprising a substrate layer.

[0278] (18) The method according to (17) above, wherein the base layer is formed of a resin film.

[0279] (19) The method according to (17) or (18) above, wherein the substrate layer is formed of a polyolefin resin film, a polyester resin film or a vinyl chloride resin film.

[0280] (20) The method according to any one of (1) to (19) above, wherein the Low-E layer includes a layer containing a zinc component (eg, a zinc oxide layer).

[0281] (21) A protective sheet comprising an adhesive layer,

[0282] The ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g based on the weight of the adhesive layer.

[0283] (22) The protective sheet according to (21) above, wherein the PSA layer is a PSA layer formed from a water-dispersible PSA composition.

[0284] (23) The protective sheet according to (21) or (22) above, wherein the adhesive layer contains ammonia.

[0285] (24) The protective sheet according to any one of (21) to (23) above, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer containing an acrylic polymer or a rubber pressure-sensitive adhesive layer containing a rubber polymer.

[0286] (25) The protective sheet according to any one of (21) to (24) above, comprising a substrate layer, wherein the substrate layer is formed of a resin film.

[0287] (26) The protective sheet according to any one of (21) to (25) above, wherein the protective sheet has a 180-degree peel strength with respect to a Low-E glass plate of 5 N / 20 mm or less.

[0288] (27) The protection sheet according to any one of (21) to (26) above, wherein the protection sheet is a Low-E glass plate protection sheet.

[0289] (28) The protective sheet according to any one of (21) to (27) above, which is used to protect a Low-E glass plate having a Low-E layer containing a zinc component.

[0290] (29) The protective sheet according to any one of (21) to (27) above, which is used to protect a Low-E glass plate having a Low-E layer, wherein the Low-E layer has a layer containing a zinc component.

[0291] (30) The protective sheet according to any one of (21) to (27) above, which is used to protect a Low-E glass plate having a Low-E layer, wherein the Low-E layer has a zinc oxide layer.

[0292] (31) A laminate comprising: a Low-E glass plate and a protective sheet for protecting a surface of the Low-E glass plate;

[0293] The Low-E glass plate includes a Low-E layer containing a zinc component.

[0294] The adhesive sheet comprises an adhesive layer.

[0295] The ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g based on the weight of the adhesive layer.

[0296] (32) The laminate according to (31) above, wherein the Low-E layer includes a layer containing a zinc component.

[0297] (33) The laminate according to (31) above, wherein the Low-E layer includes a zinc oxide layer.

[0298] (34) The laminate according to any one of (31) to (33) above, wherein the pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from a water-dispersible pressure-sensitive adhesive composition.

[0299] (35) The laminate according to any one of (31) to (34) above, wherein the adhesive layer contains ammonia.

[0300] (36) The laminate according to any one of (31) to (35) above, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer containing an acrylic polymer or a rubber pressure-sensitive adhesive layer containing a rubber polymer.

[0301] (37) The laminate according to any one of (31) to (36) above, comprising a substrate layer, wherein the substrate layer is formed of a resin film.

[0302] (38) The laminate according to any one of (31) to (37) above, wherein the protective sheet is attached to the Low-E glass plate with a 180-degree peel strength of 5 N / 20 mm or less.

[0303] Example

[0304] Hereinafter, some experimental examples related to the present invention will be described, but the present invention is not intended to be limited to the experimental examples. It should be noted that in the following description, "parts" and "%" are based on weight unless otherwise specified.

[0305] <Evaluation method>

[0306] [Ammonia content of adhesive (layer)]

[0307] Prepare about 10 mg of the adhesive component of the protective sheet to be measured, put it into a polypropylene (PP) container and weigh it. Then, add 100 mL of ultrapure water and cover it with a lid, and perform heating extraction in a 120°C dryer for 1 hour. The amount of ammonium ions in the obtained extract is quantified by ion chromatography using a commercially available ammonium ion standard solution (obtained from FUJIFILM Wako Pure Chemical Corporation) to determine the amount of ammonia in each 1 g of the adhesive used in the extraction. The ion chromatography measurement conditions are as follows.

[0308] (Measurement conditions)

[0309] Device: "DX-320" manufactured by Thermo Fisher Scientific

[0310] Separation column: Dionex Ion Pac CS16 (5mm×250mm)

[0311] Guard column: Dionex Ion Pac CG16 (5mm×50mm)

[0312] Removal system: Dionex CSRS-500 (recirculation mode)

[0313] Detector: Conductivity detector

[0314] Eluent: Methanesulfonic acid aqueous solution

[0315] Eluent flow rate: 1.0mL / min

[0316] Sample injection volume: 25μL

[0317] [Evaluation of discoloration of Low-E glass plate]

[0318] Cut the protective sheet into strips with a width of 20 mm and a length of 100 mm to prepare a test piece. Under a standard environment of 23°C and 50% RH, a 2kg rubber roller was reciprocated twice to press the test piece onto the surface of the Low-E layer of the test Low-E glass plate as the adherend. After the sample was stored in an environment of 40°C and 92% RH for 2 weeks, the protective sheet was peeled off and the state of the glass plate surface in the area protected by the protective sheet was observed under an optical microscope. The case where no discoloration was observed was judged as "◎", the level where discoloration was slightly observed but there was no problem in practical use was judged as "○", and the case where discoloration was observed was evaluated as "×".

[0319] <Preparation of Low-E Glass Plate for Experiment>

[0320] (Production example A1)

[0321] A titanium oxide layer with a thickness of 10 nm (hereinafter, sometimes abbreviated as "TiO2 layer" for convenience), a zinc oxide layer with a thickness of 10 nm (hereinafter, sometimes abbreviated as "ZnO layer" for convenience), a Ag-Pd alloy layer with a thickness of 15 nm (hereinafter, sometimes abbreviated as "Ag layer" for convenience), a zinc oxide layer with a thickness of 10 nm (ZnO layer) and a titanium oxide layer with a thickness of 10 nm (TiO2 layer) were formed in sequence on one surface of a 3 mm thick float glass (produced by Matsunami Glass Industries, Ltd., with a visible light transmittance of 91%) by a DC magnetron sputtering method. In the formation of the titanium oxide layer, a target made of sintered titanium oxide was used, and the power density was 2.67 W / cm 2 The sputtering was performed under the conditions of 0.4 Pa and a working pressure of 0.4 Pa. At this time, the gas introduction amount in the sputtering film forming chamber was adjusted so that Ar:O2 became 98:2 (volume ratio). The zinc oxide layer was formed using a target made by sintering zinc oxide at a power density of 2.67 W / cm 2 The sputtering was performed under the conditions of 0.4 Pa working pressure. At this time, the gas introduction amount in the sputtering film forming chamber was adjusted so that Ar:O2 became 98:2 (volume ratio). A metal target containing silver:palladium in a weight ratio of 96.4:3.6 was used to form the Ag-Pd alloy layer. The power density was 1.33 W / cm 2 Sputtering was performed under the conditions of 0.4 Pa and a working pressure of 0.4 Pa. In this way, a test Low-E glass plate A1 having a Low-E layer in which a TiO2 layer, a ZnO layer, an Ag layer, a ZnO layer, and a TiO2 layer (outermost layer) were sequentially stacked was produced.

[0322] (Production Example A2)

[0323] For the Low-E layer, a TiO2 layer, a ZTO layer, an Ag layer, a ZTO layer, and a TiO2 layer (outermost layer) were sequentially stacked from the glass plate side, and the same operation as the above-mentioned production example A1 was performed to produce a test Low-E glass plate A2. It should be noted that ZTO (zinc tin oxide) refers to oxides of zinc and tin.

[0324] (Production Example A3)

[0325] A test Low-E glass plate A3 was produced in substantially the same manner as in the above-mentioned Production Example A1 except that a TiO2 layer, an Ag layer, and a TiO2 layer (outermost layer) were sequentially stacked as the Low-E layer from the glass plate side.

[0326] <Production of protective film>

[0327] (Production Example B1)

[0328] A monomer raw material containing 58 parts of 2-ethylhexyl acrylate, 40 parts of n-butyl methacrylate and 2 parts of acrylic acid, 3 parts of a surfactant (trade name "Aqualon KH-1025" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene-1-(allyloxymethyl)alkyl ether ammonium sulfate having an EO addition mole number of 30 or less) and 150 parts of deionized water were mixed and emulsified with an emulsifier (homogeneous mixer) while introducing nitrogen gas to prepare an emulsion of the monomer raw material.

[0329] The emulsion was added to a reaction vessel equipped with a thermometer, a nitrogen inlet tube, a condenser and a stirring device, and heated to a liquid temperature of 50°C while stirring under a nitrogen flow. 0.03 parts of 2,2'-azobis(2-methylpropionamidine) dihydrochloride (manufactured by FUJIFILM Wako Pure Chemical Corporation, trade name "V-50") was added as a polymerization initiator, and the polymerization reaction was carried out for 5 hours while maintaining the liquid temperature at about 50°C. Ammonia water was added to the obtained polymerization reaction liquid to adjust the pH. In this way, an aqueous dispersion of an acrylic polymer was prepared.

[0330] Into this aqueous dispersion, 2 parts of an oxazoline crosslinking agent (trade name "EPOCROS WS-500" manufactured by Nippon Shokubai Co., Ltd.) was mixed with 100 parts of nonvolatile components contained in the aqueous dispersion to prepare a pressure-sensitive adhesive composition of this example.

[0331] The adhesive composition was applied to the corona treated surface (first surface) of a polyethylene film with a thickness of 55 μm and subjected to corona discharge treatment on one side by a rod coater in a manner to a thickness of 6 μm after drying. After drying at 70° C. for 2 minutes, it was aged at 50° C. for 1 day to prepare a single-sided adhesive sheet having an acrylic adhesive layer on one side of a substrate layer formed by a polyethylene film. The adhesive sheet thus obtained was used as the protective sheet B1 of this example.

[0332] (Production Examples B2 to B5)

[0333] Protective sheets B2 to B5 were obtained in the same manner as in Preparation Example B1, except that the amount of ammonia used as a pH adjuster relative to the aqueous dispersion of the acrylic polymer was gradually reduced and the drying time during the formation of the adhesive layer was prolonged.

[0334] (Production Example B6)

[0335] In the preparation of the aqueous dispersion of the acrylic polymer, NaOH was used as a pH adjuster instead of ammonia. A protective sheet B6 was obtained in the same manner as in the above-mentioned Preparation Example B1 except for the above-mentioned.

[0336] <Examples 1 to 8 and Reference Examples 9 to 10>

[0337] As protective sheets for the test Low-E glass plates A1 to A3, protective sheets B1 to B6 were used in the combination shown in Table 1, and the above-mentioned Low-E glass plate discoloration evaluation was carried out. The results are shown in Table 1. Table 1 also shows the summary of each example and the ammonia content (residual ammonia content) [μg / g] per 1g of the adhesive of the protective sheet.

[0338] [Table 1]

[0339]

[0340] As shown in Table 1, from Example 1 to Example 5, as the amount of ammonia used as a pH adjuster decreases, the amount of residual ammonia in the adhesive also decreases. Moreover, for Examples 1 to 2 in which the amount of ammonia in the adhesive layer is large, discoloration was observed in the discoloration evaluation of the Low-E glass plate using a Low-E glass plate containing a zinc component, while in Example 3 in which the ammonia content in the adhesive layer is less than 850μg / g, the discoloration of the Low-E glass plate was suppressed, and in Examples 4 to 5 in which the amount of ammonia is even less, more excellent discoloration prevention was achieved. The same tendency was observed in Examples 6 to 7 in which the Low-E glass plates containing different zinc components were tested. In addition, in Example 8 in which NaOH was used as a pH adjuster instead of ammonia, no discoloration of the Low-E glass plate was observed. In Reference Examples 9 to 10 in which a Low-E glass plate containing no zinc component was used, no discoloration of the Low-E glass plate was observed regardless of the amount of ammonia in the adhesive layer. Based on these results, it is believed that the ammonia in the adhesive layer reacts with the zinc component of the Low-E layer to deteriorate the Low-E layer, causing discoloration of the Low-E glass plate. It is also known that the deterioration of the Low-E glass plate can be prevented or suppressed by using a protective sheet in which the amount of ammonia measured by hot water extraction is less than 850 μg per 1 g of the adhesive.

[0341] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the claims. The technology described in the claims includes various modifications and changes to the specific examples described above.

[0342] Description of Reference Numerals

[0343] 1: Base material layer

[0344] 1A: One side

[0345] 1B: The other side

[0346] 2: Adhesive layer

[0347] 2A: Bonding surface

[0348] 10: Protective sheet

[0349] 100: Low-E glass panel

[0350] 110: Glass substrate

[0351] 120: Low-E layer

[0352] 200: Protective film

[0353] 300: Glass unit

[0354] 320: Other glass panels

[0355] 340: Spacer

Claims

1. A method for protecting a Low-E glass plate, characterized in that: A protective sheet having a substrate and an adhesive layer provided on at least one surface of the substrate is attached to a Low-E layer of a Low-E glass plate having a Low-E layer containing a zinc component via the adhesive layer to protect the Low-E layer. The adhesive layer comprises ammonia, As the protective sheet, the PSA layer is formed from a water-dispersible PSA composition and the ammonia content of the PSA layer measured by hot water extraction is less than 850 μg / g relative to the weight of the PSA layer.

2. The protection method according to claim 1, wherein: The method further includes removing the protective sheet from the Low-E glass plate. The process includes performing at least one step selected from the group consisting of transportation, storage, processing, cleaning, and handling on the Low-E glass plate to which the protection sheet is attached during the period from attachment to removal of the protection sheet.

3. The protection method according to claim 1 or 2, wherein: The Low-E glass plate has a width of 1 m or more, Attaching the protection sheet to the Low-E glass plate includes a step of covering the entire one surface of the Low-E glass plate with at least one protection sheet.

4. The protection method according to claim 1 or 2, wherein: The protective sheet is attached to the Low-E glass plate with a 180-degree peel strength of 5N / 20mm or less.

5. A method for manufacturing a glass unit, comprising: Step (A), preparing a Low-E glass plate having a Low-E layer; Step (B), attaching a protective sheet to the surface of the Low-E layer of the Low-E glass plate; The optional step (C) is to perform at least one selected from the group consisting of transportation, storage, processing, cleaning and operation on the Low-E glass plate to which the protective sheet is attached; Step (D), removing the protective sheet from the Low-E glass plate; and Step (E), assembling a glass unit using the Low-E glass sheet, in, The Low-E layer contains zinc. The protective sheet comprises a substrate and an adhesive layer provided on at least one surface of the substrate. The adhesive layer is attached to the surface of the Low-E layer, The adhesive layer is formed from a water-dispersible adhesive composition, The adhesive layer contains ammonia, and the ammonia content of the adhesive layer measured by hot water extraction is less than 850 μg / g relative to the weight of the adhesive layer.

6. A laminated body, characterized in that: Include: A Low-E glass sheet having a Low-E layer containing a zinc component; and A protective sheet comprising a substrate and an adhesive layer provided on at least one surface of the substrate. The protective sheet is attached to the Low-E layer of the Low-E glass plate by using the adhesive layer. The PSA layer in the protective sheet is formed from a water-dispersible PSA composition, the PSA layer contains ammonia, and the ammonia content of the PSA layer measured by hot water extraction is less than 850 μg / g relative to the weight of the PSA layer.

7. Use of a protective sheet for protecting a Low-E glass plate having a Low-E layer containing a zinc component, characterized in that: The protective sheet has an adhesive layer formed on a substrate, and the adhesive layer is bonded to the Low-E layer for use. The PSA layer in the protective sheet is formed from a water-dispersible PSA composition, and the ammonia content of the PSA layer measured by hot water extraction is less than 850 μg / g based on the weight of the PSA layer.

8. The use according to claim 7, wherein: The adhesive layer contains ammonia.

Citation Information

Patent Citations

  • Working treating machine for molding to be worked

    JP1982019194A

  • Adhesive composition, pressure sensitive adhesive double coated tape, adhesion method and portable electronic device

    JP2007051271A

  • Surface protection sheet

    JP2012131976A

  • Surface protection sheet

    JP2017186517A

  • Simulated gun

    JP2019120483A