A method for synthesizing narrow molecular weight distribution polyamide

By using aminocarboxylates and matching diamines as raw materials, the reaction conditions are controlled to inhibit the decomposition of nylon salts, which solves the problem of nylon salts decomposing at high temperatures in the existing technology and achieves narrow molecular weight distribution and good stability of the polymer. Amide synthesis improves product quality and process safety.

CN114085375BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202010853815.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-24
Publication Date
2024-10-15
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Existing nylon salts are easy to decompose at high temperatures, resulting in a wide molecular weight distribution and poor viscosity stability during the polymerization process. They also need to be carried out under higher pressure, which affects product quality.

Method used

Amino carboxylate and matching diamine are used as raw materials. By controlling the reaction conditions and the amount of diamine added, the decomposition of nylon salt is inhibited, the residual acid is neutralized, the molecular weight distribution is adjusted, the operating pressure is reduced, and a narrow molecular weight distribution and Polyamide synthesis with good stability.

Benefits of technology

It achieves a narrow molecular weight distribution of polyamide, improved viscosity stability, excellent product quality, simple process, easy mass production, and excellent dyeing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002645708960000051
    Figure BDA0002645708960000051
  • Figure BDA0002645708960000061
    Figure BDA0002645708960000061
  • Figure HDA0002645708970000011
    Figure HDA0002645708970000011
Patent Text Reader

Abstract

The invention discloses a method for synthesizing a polyamide with a narrow molecular weight distribution, the method comprising adding raw materials including nylon salt, water and diamine into a reactor, heating to 180-240°C, reacting at a pressure of 0.2-1.8MPa for 1.0-3.0 hours, and releasing the pressure to normal pressure; then heating to 240-265°C, first reacting at normal pressure for 1.0-3.0 hours, and then reacting at a pressure of -0.04-0.08MPa for 0.5-3.0 hours, and obtaining the product. The method uses nylon salt as the main reactant, and by introducing diamine as a regulator, the decomposition of nylon salt at high temperature can be effectively suppressed to reduce the polymerization reaction pressure, and the dibasic acid produced by the decomposition of nylon salt can be neutralized, and the molecular weight regulator can also be used to obtain a polyamide product with a narrower molecular weight distribution, a more stable viscosity, and better quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing polyamide, in particular to a method for obtaining polyamide with narrow molecular weight distribution by using aminocarboxylate as raw material and diamine as regulator, belonging to the technical field of nylon preparation. Background Art

[0002] Polyamide, commonly known as nylon, such as nylon 610, nylon 612, etc., is an important general engineering plastic variety with good comprehensive performance, low density, easy molding, large design freedom, thermal insulation, high tensile strength, excellent impact performance, high heat deformation temperature, heat resistance, low friction coefficient, wear resistance, self-lubrication, oil resistance, excellent chemical resistance, etc. It has a wide range of uses. It is widely used in machinery manufacturing, aerospace, automobile lightweight, spinning, home appliances, biomedicine, electrical and other fields.

[0003] At present, when nylon 610, nylon 612 and other products use diamines and dibasic acid salts as raw materials, nylon salts are easy to decompose at high temperatures. Therefore, the polymerization process needs to be carried out at a higher pressure in the early stage. However, as the system temperature rises, even if the system is under a higher pressure, nylon salts will still partially decompose and turn back into monomers of diamines and dibasic acids. Due to the volatility of diamines, most of these decomposed diamines will be discharged during the subsequent pressure relief and vacuuming process, while the residual dibasic acid in the system will act as a capping agent, inhibiting the growth of the molecular chain, making the product molecular weight distribution wide, the viscosity stability poor, and the final product quality stability poor. For example, the technologies disclosed in (“Synthesis of Nylon 612 and Study on Its Properties”, Synthetic Fiber Industry, Tang Xinhua et al., Vol. 30, No. 5, pp. 8-10, October 2007) and (“Synthesis of Nylon 612”, 612 Special Group of Shanghai Resin Research Institute) both use carboxylic acid molecular weight regulators, such as acetic acid, benzoic acid, etc. The addition of such molecular weight regulators cannot effectively inhibit the decomposition of nylon salts, and the reaction needs to be carried out at a relatively high reaction pressure in the early stage, resulting in a wide molecular weight distribution of the product and poor quality stability. Summary of the invention

[0004] In view of the defects of the prior art in synthesizing polyamide using nylon salt, the purpose of the present invention is to provide a method for synthesizing polyamide with narrow molecular weight distribution, stable viscosity and good quality stability. The method has simple process, is easy to implement, has milder reaction conditions, and is conducive to large-scale production.

[0005] In order to achieve the above technical purpose, the present invention provides a method for synthesizing polyamide with narrow molecular weight distribution, which comprises adding raw materials including nylon salt, water and diamine into a reaction kettle, heating to 180-240° C., reacting at a pressure of 0.2-1.8 MPa for 1.0-3.0 hours, and releasing the pressure to normal pressure; then heating to 240-265° C., first reacting at normal pressure for 1.0-3.0 hours, and then reacting at a pressure of -0.04--0.08 MPa for 0.5-3.0 hours to obtain the polyamide; the diamine is the same as the diamine used to synthesize the nylon salt.

[0006] When nylon salt is used to synthesize polyamide, since nylon salt is easily decomposed into monomers of diamine and dibasic acid at high temperature, and diamine is volatile, in the subsequent pressure relief and vacuum process, the diamine produced by the decomposition of nylon salt will escape, so that the residual dibasic acid will play the role of end-capping agent, inhibiting the growth of molecular chain, making the product molecular weight distribution wide and the viscosity stability poor. The key to the technical solution of the present invention is to introduce diamine as a regulator. On the one hand, the addition of diamine can effectively inhibit the decomposition of nylon salt at high temperature, so that in the high-temperature reaction process of the front section, the operating pressure can be reduced. On the other hand, diamine can neutralize the dibasic acid produced by the decomposition of nylon salt, make up for the diamine lost in the pressure relief and vacuum reaction process, so as to effectively prevent the end-capping effect of carboxylic acid and the role of molecular weight regulator, so as to obtain a polyamide product with narrower molecular weight distribution, more stable viscosity and better product quality. Thirdly, a slightly excessive amount of diamine makes the end of the polyamide mainly amino, so that it has excellent dyeing performance.

[0007] The technical solution of the present invention requires that the diamine unit is the same as the diamine unit in the nylon salt. Since the nylon salt has a reversible equilibrium of decomposition reaction during the high-temperature reaction process, when a diamine matching the diamine in the nylon salt is used, the reversible equilibrium reaction of the decomposition reaction of the nylon salt can be made to proceed in the opposite direction, that is, in the direction of generating nylon salt, to achieve a new equilibrium, thereby inhibiting the decomposition of the nylon salt and achieving the purpose of reducing the operating pressure.

[0008] As a preferred technical solution, the mass of the nylon salt accounts for 60% to 90% of the total mass of the raw materials.

[0009] As a preferred technical solution, the nylon salt is nylon 66 salt, nylon 612 salt, nylon 610 salt, nylon 512 salt, nylon 1010 salt, nylon 1012 salt, nylon 46 salt or MXD6 salt. These nylon salts are common ω-aminocarboxylates in the polyamide synthesis process.

[0010] As a preferred technical solution, the mass of the diamine is 0.05‰ to 5‰ of the mass of the nylon salt. The amount of diamine added is very important for the regulation of molecular weight. Different proportions of diamine are added according to the relative viscosity of the desired product. If the amount of diamine added is too much, it will produce a capping effect, inhibiting the continuation of the reaction and the growth of the molecular chain, and the relative viscosity of the obtained product is low, which does not meet the use requirements. If the amount of diamine used is too little, the decomposition of the nylon salt cannot be effectively inhibited, and the purpose of regulating the molecular weight distribution cannot be achieved.

[0011] As a preferred technical solution, the diamine is pentamethylenediamine, hexamethylenediamine, butanediamine, decanediamine, p-phenylenediamine or m-phenylenediamine.

[0012] As a preferred technical solution, the pressure relief is carried out in a slow pressure relief manner, and the pressure relief time is 0.5 to 2.0 hours.

[0013] The preparation method of polyamide provided by the present invention is specifically as follows: adding raw materials such as nylon salt, water, diamine and the like into a reaction kettle, heating to 180-240°C, and pressure to 0.2-1.8MPa, and reacting for 1.0-3.0 hours at the temperature and pressure; then slowly releasing the pressure to normal pressure for 0.5-2.0 hours, heating to 240-265°C, and reacting at normal pressure for 1.0-3.0 hours; after reacting at normal pressure, evacuating to -0.04--0.08MPa, reacting for 0.5-3.0 hours, and after the reaction, pelletizing the cast strip and drying to obtain polyamide slices.

[0014] The heating, pressurizing, vacuuming, pelletizing and drying involved in the present invention all adopt techniques well known in the art.

[0015] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0016] The polyamide synthesis method provided by the present invention has a simple process, and the operation pressure in the early stage of polymerization is lower than that in the existing polymerization process, and is safer;

[0017] The polyamide synthesis method provided by the present invention uses diamine to effectively inhibit the decomposition of nylon salt and adjust the molecular weight distribution of nylon salt, so that the obtained polyamide material has a narrower molecular weight distribution and a more stable viscosity;

[0018] The polyamide provided by the present invention can play the role of a molecular weight regulator by using diamine, so that the terminal amino group content of the product can be higher and the product has excellent dyeing performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The polyamide dyeing effect diagram of Comparative Example 3;

[0020] Figure 2 The polyamide dyeing effect diagram of Example 3. DETAILED DESCRIPTION

[0021] In order to facilitate the understanding of the present invention, embodiments of the present invention are provided herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0022] Unless otherwise defined, the technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for describing specific embodiments and are not intended to limit the present invention. The term "and" as used herein includes any and all combinations of one or more related listed items.

[0023] Example 1

[0024] 800g of nylon 612 salt, 200g of water and 0.4g of hexamethylenediamine raw materials were added into a reactor, the temperature was raised to 200°C and the pressure was 1.2MPa, and the reaction was maintained at the temperature and pressure for 2.0 hours; then the pressure was slowly released to normal pressure for 1.5 hours, the temperature was raised to 255°C, and the reaction was maintained at normal pressure for 1.0 hour; after the reaction at normal pressure, the pressure was evacuated to -0.06MPa and the reaction was carried out for 1.0 hour. After the reaction was completed, the cast strip was pelletized and dried at 120°C for 48 hours to obtain nylon 612 chips.

[0025] Example 2

[0026] 800g of nylon 512 salt, 200g of water and 0.4g of pentamethylenediamine raw materials were added into a reactor, the temperature was raised to 200°C and the pressure was 1.2MPa, and the reaction was maintained at the temperature and pressure for 2.0 hours; then the pressure was slowly released to normal pressure for 1.5 hours, the temperature was raised to 255°C, and the reaction was maintained at normal pressure for 1.0 hour; after the reaction at normal pressure, the pressure was evacuated to -0.06MPa and the reaction was carried out for 1.0 hour. After the reaction was completed, the cast strip was pelletized and dried at 120°C for 48 hours to obtain nylon 512 chips.

[0027] Example 3

[0028] 800g nylon 612 salt, 200g water and 1.2g hexamethylenediamine raw materials were added to the reactor, heated to 200℃, pressure 1.2MPa, maintained at this temperature and pressure for 2.0 hours; then slowly released the pressure to normal pressure, the pressure release time was 1.5 hours, heated to 240℃, maintained at normal pressure for 1.0 hour; after normal pressure reaction, evacuated to -0.06MPa, reacted for 1.0 hour, after the reaction was completed, cast strip pelletized, dried at 120℃ for 48 hours to obtain nylon 612 slices. The polyamide dyeing effect is shown in the figure below. Figure 2 ,relatively Figure 1The dyeing is more even and the color is deeper.

[0029] Comparative Example 1

[0030] Example 1 was repeated, except that no hexamethylenediamine was added.

[0031] Comparative Example 2

[0032] Example 2 was repeated except that no pentamethylenediamine was added.

[0033] Comparative Example 3

[0034] Example 3 was repeated except that no hexamethylenediamine was added.

[0035] Comparative Example 4

[0036] Example 3 was repeated, except that hexamethylenediamine was replaced with pentamethylenediamine.

[0037] Comparative Example 5

[0038] Example 1 was repeated, except that the amount of hexamethylenediamine added was increased to 1%. The relative viscosity of the product was 1.68, which had no application value.

[0039] Molecular weight and molecular weight distribution data table of prepared chips

[0040]

[0041]

[0042] It can be seen from Comparative Examples 1 to 3 that when a proper amount of diamine is added as a regulator, the molecular weight and molecular weight distribution of nylon can be significantly adjusted. However, it can be seen from Comparative Example 4 that if a diamine that does not match the nylon salt is used as a regulator, it can only play an end-capping role and reduce the molecular weight, but cannot adjust the molecular weight distribution to be narrower. It can be seen from Comparative Example 5 that under the same polymerization conditions, if the proportion of the molecular weight regulator added is too high, the relative viscosity of the nylon product is lower.

[0043] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and it is impossible to list all implementation methods here, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for synthesizing a polyamide with a narrow molecular weight distribution, characterized in that: Add raw materials including nylon salt, water and diamine into a reaction kettle, heat up to 180-240°C, react at a pressure of 0.2-1.8MPa for 1.0-3.0 hours, and release the pressure to normal pressure; then heat up to 240-265°C, first react at normal pressure for 1.0-3.0 hours, and then react at a pressure of -0.04--0.08MPa for 0.5-3.0 hours to obtain the diamine; the diamine is the same as the diamine used to synthesize the nylon salt; the mass of the nylon salt accounts for 60%-90% of the total mass of the raw materials; the mass of the diamine is 0.05‰-5‰ of the mass of the nylon salt.

2. The method for synthesizing a polyamide with a narrow molecular weight distribution according to claim 1, characterized in that: The nylon salt is nylon 66 salt, nylon 612 salt, nylon 610 salt, nylon 512 salt, nylon 1010 salt, nylon 1012 salt, nylon 46 salt or MXD6 salt.

3. The method for synthesizing a polyamide with a narrow molecular weight distribution according to claim 1, characterized in that: The diamine is pentamethylenediamine, hexamethylenediamine, butanediamine, decanediamine, p-xylylenediamine or m-xylylenediamine.

4. The method for synthesizing a polyamide with a narrow molecular weight distribution according to claim 1, characterized in that: The pressure relief adopts a slow pressure relief method, and the pressure relief time is 0.5 to 2.0 hours.

Citation Information

Patent Citations

  • Nylon manufacturing method

    CN104031263A

  • Halogen-free flame-retardant high-temperature nylon

    CN105153417A

  • Polymerization method of nylon

    CN109970968A

  • Continuous production method of high-temperature nylon powder with narrow molecular weight distribution

    CN116874771A

  • Polyamide, polyamide composition and use thereof

    JP1997012714A