Rubber composition for sealing material, and pneumatic tire

By adding zinc oxide and liquid polymer to butyl rubber, combined with specific vulcanization accelerator, the problems of low thermal stability and uneven cross-linking reaction during cross-linking of traditional sealing materials are solved, and good sealing of sealing materials is achieved Excellent sexual and destructive characteristics, inhibiting long-term performance changes.

CN114106637BActive Publication Date: 2024-11-22SUMITOMO RUBBER INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110950912.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-26
Filing Date
2021-08-18
Publication Date
2024-11-22
Estimated Expiration
2041-08-18

AI Technical Summary

Technical Problem

Traditional sealing materials have low thermal stability during crosslinking, resulting in insufficient sealing properties and difficult to control crosslinking reactions, resulting in uneven and slow damage characteristics, affecting the long-term performance of sealing materials.

Method used

Using butyl rubber as the basis, zinc oxide and liquid polymer are added, combined with thiuram vulcanization accelerator and dithiocarbamic vulcanization accelerator to control the crosslinking reaction, form a uniform crosslinking structure, and improve the sealing material destructive properties and thermal stability.

Benefits of technology

The sealing material has excellent sealing properties and excellent damage characteristics after deterioration over the years, suppresses changes in damage characteristics over time, and improves the overall performance of the sealing material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114106637B_ABST
    Figure CN114106637B_ABST
Patent Text Reader

Abstract

The present invention provides a rubber composition for sealing material having excellent destruction characteristics, good sealing performance after years of degradation, and suppressing the change of destruction characteristics over time, and a pneumatic tire (self-repairing tire) using the same. A rubber composition for sealing material, wherein the content of zinc oxide is 2 to 15 parts by mass, the content of liquid polymer is 100 to 300 parts by mass, and the content of thiuram-based vulcanization accelerator, dithiocarbamic acid-based vulcanization accelerator, and sulfur is less than 0.1 parts by mass, respectively, relative to 100 parts by mass of butyl rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rubber composition for a sealant material and a pneumatic tire using the same. Background Art

[0002] As a pneumatic tire with puncture resistance (hereinafter also referred to as a pneumatic tire), a self-repairing tire with a sealing material coated on the inner surface of the tire is known. A self-repairing tire is a tire in which a hole formed by a puncture is automatically sealed by the sealing material, and various studies have been conducted on the sealing material.

[0003] Conventional sealing materials use zinc oxide, a thiuram-based vulcanization accelerator, and sulfur together for crosslinking (for example, Patent Document 1).

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] [Patent Document 1] WO2017 / 094653 Summary of the invention

[0007] [Problems to be Solved by the Invention]

[0008] However, the present inventors' research results have revealed that among the above cross-linking, cross-linking using sulfur has low thermal stability and thus has a problem of insufficient sealing properties after aging.

[0009] In addition, conventional sealing materials also use organic peroxides such as peroxides for crosslinking, but the inventors have made it clear after research that conventional sealing materials that use organic peroxides such as peroxides for crosslinking are difficult to control the crosslinking reaction and the crosslinking structure is uneven, so there is room for improvement in the required failure characteristics of the sealing materials. In addition, it is also clear that since the crosslinking reaction using organic peroxides such as peroxides proceeds slowly, there is the following problem: even during storage or use after manufacturing, the crosslinking reaction is not completed, and the sealing performance after years of deterioration is insufficient.

[0010] The present invention aims to solve the above problems and provide a rubber composition for a sealant having excellent fracture characteristics, good sealing performance after aging degradation, and suppressing the temporal change of fracture characteristics, and a pneumatic tire (self-repairing tire) using the same.

[0011] [Methods for solving the problem]

[0012] The present invention relates to a rubber composition for a sealing material, wherein the content of zinc oxide is 2 to 15 parts by mass, the content of liquid polymer is 100 to 300 parts by mass, and the content of thiuram vulcanization accelerator, dithiocarbamic acid vulcanization accelerator and sulfur is less than 0.1 parts by mass, respectively, relative to 100 parts by mass of butyl rubber.

[0013] Preferably, the liquid polymer is liquid polybutene.

[0014] Preferably, the liquid polymer has a kinematic viscosity of 500 to 6000 cSt measured at 100° C. according to ASTM D445.

[0015] Preferably, in the rubber composition for a sealant, the content of the organic peroxide is 1 part by mass or less relative to 100 parts by mass of the butyl rubber.

[0016] The present invention also relates to a pneumatic tire (self-repairing tire) having a sealing layer made using the rubber composition.

[0017] Preferably, the sealing layer has a complex elastic modulus G measured at 100°C according to ISO13145. * It is 0.75~3.50kPa.

[0018] [Effects of the Invention]

[0019] In the rubber composition for sealing materials of the present invention, the content of zinc oxide is 2 to 15 parts by mass, the content of liquid polymer is 100 to 300 parts by mass, and the content of thiuram-based vulcanization accelerator, dithiocarbamic acid-based vulcanization accelerator, and sulfur is 0.1 parts by mass or less, respectively, relative to 100 parts by mass of butyl-based rubber. Therefore, it is possible to provide a rubber composition for sealing materials having excellent destruction characteristics, good sealing performance after aging, and suppressed time-dependent changes in destruction characteristics, and a pneumatic tire (self-repairing tire) using the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] [ Figure 1 ]A schematic illustration of an example of a coating device used in a method for manufacturing a self-repairing tire.

[0021] [ Figure 2 ]constitute Figure 1 An enlarged view of the vicinity of the front end of the nozzle of the coating device is shown.

[0022] [ Figure 3 ] Schematic illustration of the positional relationship of the nozzle relative to the tire.

[0023] [ Figure 4]A schematic illustration of an example of a state in which a roughly rope-shaped sealing material is continuously and spirally attached to the inner circumferential surface of a tire.

[0024] [ Figure 5 ]constitute Figure 1 An enlarged view of the vicinity of the front end of the nozzle of the coating device is shown.

[0025] [ Figure 6 ] Schematic illustration of an example of a sealing material attached to a self-repairing tire.

[0026] [ Figure 7 ]A schematic illustration of an example of a manufacturing device used in a method for manufacturing a self-repairing tire.

[0027] [ Figure 8 ] Cut with a straight line AA perpendicular to (orthogonal to) the coating direction (length direction) of the sealing material Figure 4 A schematic illustration of an example of a cross section of a sealing material when a sealing material is used.

[0028] [ Fig. 9 ]A schematic illustration of an example cross section of a pneumatic tire.

[0029] [reference numerals]

[0030] 10 Tires

[0031] 11 Inner circumference of the tire

[0032] 14 Tread

[0033] 15 Carcass

[0034] 16 Buffer layer (breaker)

[0035] 17 Band

[0036] 20 Sealing material

[0037] 21 Width

[0038] 30 Nozzle

[0039] 31 Tip of the nozzle

[0040] 40 Non-contact displacement sensor

[0041] 50 Rotary drive

[0042] 60 Twin-shaft compounding extruder

[0043] 61 (61a 61b 61c) Supply port

[0044] 62 Material Feeder

[0045] d, d0, d1, d2 Distance between the inner circumference of the tire and the front end of the nozzle DETAILED DESCRIPTION

[0046] The rubber composition for sealing materials (sealing material) of the present invention contains 2 to 15 parts by mass of zinc oxide and 100 to 300 parts by mass of liquid polymer relative to 100 parts by mass of butyl rubber, and the contents of thiuram vulcanization accelerator, dithiocarbamic acid vulcanization accelerator and sulfur are respectively less than 0.1 parts by mass relative to 100 parts by mass of butyl rubber. As a result, the rubber composition has excellent destructive properties (initial stage), good sealing properties after years of deterioration, and can also suppress the change of destructive properties over time.

[0047] The rubber composition can achieve the above-mentioned effects. Although the reason why such effects are achieved is not clear, it can be inferred as follows.

[0048] For butyl rubber, zinc oxide is used, and thiuram-based vulcanization accelerators, dithiocarbamic acid-based vulcanization accelerators, and sulfur are not substantially used, thereby ensuring good damage characteristics, and further having good sealing properties after aging, and suppressing the change of damage characteristics over time. It is believed that this is because, in the above cross-linking system, the control of the cross-linking reaction becomes simple, and the cross-linked structure is easy to become uniform, thereby ensuring good damage characteristics, and further, because the cross-linking reaction is not slowly progressed, but quickly progresses and is completed, further, a cross-linked chain with high thermal stability is formed, so that it has good sealing properties after aging, and can suppress the change of damage characteristics over time.

[0049] Then, by adding the above-mentioned specific amount of liquid polymer to the butyl rubber, the above-mentioned specific amount of zinc oxide can be more evenly dispersed in the composition, making the cross-linking structure more uniform, and obtaining good destruction characteristics. Furthermore, it has good sealing performance after years of degradation, and at the same time, the change of destruction characteristics over time can be suppressed.

[0050] That is, in the above composition, due to the synergistic effect of the above specific amount of zinc oxide and the above specific amount of liquid polymer, the composition has excellent breaking characteristics, has good sealing properties after aging, and can suppress the change of breaking characteristics over time.

[0051] The rubber composition for sealing material (sealing material) of the present invention is suitable for use in areas of the inner surface of a tire that may be punctured, such as the tread of a self-repairing tire. The sealing material will be described below while describing a suitable example of a method for manufacturing a self-repairing tire.

[0052] The self-repairing tire can be manufactured, for example, by mixing the components constituting the sealing material, preparing the sealing material, and then applying the obtained sealing material to the inner circumference of the tire by coating, etc. to form a sealing layer. The self-repairing tire has a sealing layer on the inner side of the inner liner in the tire radial direction.

[0053] A preferred example of a method for producing a self-repairing tire will be described below.

[0054] The self-repairing tire can be manufactured, for example, by mixing the components constituting the sealing material, preparing the sealing material, and then applying the obtained sealing material to the inner circumference of the tire by coating, etc. to form a sealing layer. The self-repairing tire has a sealing layer on the inner side of the inner liner in the tire radial direction.

[0055] As a sealing material, as long as it has adhesion, there is no particular limitation, and the conventional rubber composition used in the puncture seal of the tire can be used. As the rubber component constituting the main component of the rubber composition, butyl rubber can be used. Thus, there is a tendency to obtain appropriate fluidity while ensuring good air permeability resistance and degradation resistance. As butyl rubber, in addition to butyl rubber (IIR), halogenated butyl rubbers (X-IIR) such as brominated butyl rubber (Br-IIR) and chlorinated butyl rubber (Cl-IIR) can also be cited. These can be used alone, or more than 2 kinds can be used. Wherein, based on the reason that compared with unhalogenated butyl rubber, halogenated butyl rubber is easier to carry out cross-linking reaction, easier to increase cross-linking density, and can obtain better effects, preferably halogenated butyl rubber, based on the promotion effect of cross-linking reaction is higher, and the reason that can obtain better effects, more preferably brominated butyl rubber.

[0056] From the viewpoint of better ensuring the fluidity of the sealing material, the Mooney viscosity ML1+8 of the butyl rubber at 125°C is preferably 20 or more, more preferably 40 or more, and preferably 60 or less. When the Mooney viscosity is within the above range, better effects tend to be obtained.

[0057] The Mooney viscosity ML1+8 at 125° C. is measured in accordance with JIS K-6300-1:2001 at a test temperature of 125° C. with the residual heat time of an L-shaped rotor set to 1 minute and the rotation time of the rotor set to 8 minutes.

[0058] The halogen content of the halogenated butyl rubber is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and preferably 5.0% by mass or less, more preferably 4.0% by mass or less. This tends to achieve a better effect of promoting the crosslinking reaction and obtain a better effect.

[0059] The halogen content can be determined by solution NMR.

[0060] As commercially available products of the butyl rubber, for example, products of ExxonMobil Corporation, Nippon Butyl Corporation, JSR Corporation, Cenway Corporation, etc. can be used.

[0061] The content of the butyl rubber in 100% by mass of the rubber component is preferably 80% by mass or more, more preferably 90% by mass or more, and may be 100% by mass. When the content is within the above range, there is a tendency that a better effect can be obtained.

[0062] In addition to the above-mentioned rubber components, other components such as diene rubbers such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR) may be used in combination as the rubber component. These may be used alone or in combination of two or more.

[0063] As the rubber component, for example, a rubber component containing at least one functional group with metal coordination ability in the molecular structure can be suitably used. Here, as the functional group with metal coordination ability, as long as it is a functional group with metal coordination ability, it is not particularly limited, and for example, a functional group containing metal coordination atoms such as oxygen, nitrogen, and sulfur can be cited. Specifically, dithiocarbamate groups, phosphoric acid groups, carboxylic acid groups, carbamate groups, dithiocarboxylic acid groups, aminophosphoric acid groups, thiol groups, etc. can be exemplified. The above-mentioned functional groups can contain only one kind, or can contain two or more kinds.

[0064] In addition, as the coordination metal for the functional group, for example, Fe, Cu, Ag, Co, Mn, Ni, Ti, V, Zn, Mo, W, Os, Mg, Ca, Sr, Ba, Al, Si, etc. can be cited. For example, in a polymer material to which a compound having such a metal atom (M1) is added and which contains a functional group (-COO, etc.) having a metal coordination ability, each -COOM1 is coordinated and bonded, and multiple -COOM1 overlap, thereby forming a cluster of metal atoms agglomerated. In addition, the addition amount of the above-mentioned metal atom (M1) is preferably 0.01 to 200 parts by mass relative to 100 parts by mass of the rubber component.

[0065] As commercially available products of the rubber component, for example, products of Sumitomo Chemical Co., Ltd., Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Corporation, etc. can be used.

[0066] The sealing material contains a liquid polymer. Thus, appropriate fluidity can be better ensured. As described above, by adding the above-mentioned specific amount of liquid polymer to the butyl rubber, the above-mentioned specific amount of zinc oxide can be more evenly dispersed in the composition, and the destructive characteristics are excellent, and the sealing performance after years of degradation is good, and the change of the destructive characteristics over time can be further suppressed.

[0067] As the liquid polymer in the sealing material, liquid polybutene, liquid polyisobutylene, liquid polyisoprene, liquid polybutadiene, liquid poly-α-olefin, liquid isobutylene, liquid ethylene / α-olefin copolymer, liquid ethylene / propylene copolymer, liquid ethylene / butylene copolymer, etc. can be cited. Among them, liquid polybutene is preferred because of its high compatibility with butyl rubber and the ability to obtain better results. As liquid polybutene, copolymers with a molecular structure of long-chain hydrocarbons obtained by further reacting n-butene with isobutylene as the main body can be cited, and hydrogenated liquid polybutene can also be used. As the liquid polymer, only one type can be used, or two or more types can be used in combination.

[0068] The kinematic viscosity of a liquid polymer such as liquid polybutene at 100° C. is preferably 500 cSt or more, more preferably 580 cSt or more, and further preferably 3000 cSt or more. The kinematic viscosity at 100° C. is preferably 6000 cSt or less, more preferably 5500 cSt or less, and further preferably 5000 cSt or less. When the kinematic viscosity at 100° C. is within the above range, there is a tendency that a better effect can be obtained.

[0069] The kinematic viscosity of a liquid polymer such as liquid polybutene at 40°C is preferably 15000 cSt or more, more preferably 20000 cSt or more, further preferably 25000 cSt or more, particularly preferably 50000 cSt or more, and most preferably 100000 cSt or more. The kinematic viscosity at 40°C is preferably 250000 cSt or less, more preferably 200000 cSt or less, and further preferably 180000 cSt or less. When the kinematic viscosity at 40°C is within the above range, there is a tendency that a better effect can be obtained.

[0070] In addition, the kinematic viscosity is a value measured at 40°C or 100°C in accordance with ASTM D445 (2019).

[0071] As commercially available products of the liquid polymer, for example, products of JXTG Energy Corporation, NOF Corporation, DAELIM, KEMAT, INEOS, and the like can be used.

[0072] Relative to 100 parts by mass of butyl rubber, the content of liquid polymer is more than 100 parts by mass, more preferably more than 120 parts by mass, further preferably more than 140 parts by mass, particularly preferably more than 160 parts by mass, and most preferably more than 180 parts by mass. The content is less than 300 parts by mass, more preferably less than 280 parts by mass, further preferably less than 260 parts by mass, particularly preferably less than 240 parts by mass, and most preferably less than 220 parts by mass. When the content of liquid polymer is within the above range, there is a tendency to obtain better effects. When the content of liquid polymer is less than 100 parts by mass, the sealing performance after years of degradation cannot be guaranteed. When the content is more than 300 parts by mass, it is too soft, so the destruction characteristics are low, and in addition, the shape of the sealing material cannot be maintained.

[0073] As the liquid polymer, preferably, only one liquid polymer (preferably liquid polybutene) having a kinematic viscosity at 100°C and a kinematic viscosity at 40°C within the above range is used in the above content. By using such a type and content of liquid polymer, a better effect can be obtained.

[0074] The above composition contains zinc oxide as a cross-linking agent.

[0075] Examples of zinc oxide include conventionally known zinc oxides, and examples of commercially available products include those of Mitsui Mining and Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Shodo Chemical Industry Co., Ltd., and Sakai Chemical Industry Co., Ltd. These may be used alone or in combination of two or more.

[0076] Relative to 100 parts by mass of butyl rubber, the content of zinc oxide is more than 2 parts by mass, preferably more than 4 parts by mass, more preferably more than 6 parts by mass, and further preferably more than 7 parts by mass. In addition, it is less than 15 parts by mass, preferably less than 13 parts by mass, more preferably less than 11 parts by mass, and further preferably less than 10 parts by mass. When the content of zinc oxide is within the above range, there is a tendency to obtain better effects. When the content of zinc oxide is less than 2 parts by mass, the cross-linking reaction cannot be fully carried out, and it is too soft, so the destructive characteristics are low. In addition, the shape of the sealing material cannot be maintained. When the content is more than 15 parts by mass, the sealing performance after years of degradation cannot be guaranteed.

[0077] In the above composition, substantially no thiuram-based vulcanization accelerator, no dithiocarbamic acid-based vulcanization accelerator, and no sulfur are used.

[0078] Examples of the thiuram vulcanization accelerator include tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N), tetramethylthiuram monosulfide, dipentamethylenethiuram tetrasulfide, tetrabutylthiuram disulfide, and tetraethylthiuram disulfide.

[0079] The content of the thiuram vulcanization accelerator is 0.1 parts by mass or less, preferably 0.01 parts by mass or less, and more preferably 0 parts by mass, relative to 100 parts by mass of the butyl rubber. When the content of the thiuram vulcanization accelerator is within the above range, a better effect tends to be obtained.

[0080] Examples of the dithiocarbamic acid-based vulcanization accelerators include zinc dimethyldithiocarbamate (ZnMDC), zinc diethyldithiocarbamate (ZnEDC), zinc dibutyldithiocarbamate (ZnBDC), zinc ethylphenyldithiocarbamate (ZnEPDC), piperidinium pentamethylenedithiocarbamate (PPDC), tellurium diethyldithiocarbamate (TeEDC), sodium dimethyldithiocarbamate (NaMDC), sodium diethyldithiocarbamate (NaEDC), and sodium dibutyldithiocarbamate (NaBDC).

[0081] The content of the dithiocarbamic acid vulcanization accelerator is 0.1 parts by mass or less, preferably 0.01 parts by mass or less, and more preferably 0 parts by mass, relative to 100 parts by mass of the butyl rubber. When the content of the dithiocarbamic acid vulcanization accelerator is within the above range, a better effect tends to be obtained.

[0082] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur.

[0083] As commercially available products of the above sulfur, for example, products of Tsurumi Chemical Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Co., Ltd., Nippon Senryu Kogyo Co., Ltd., Hosoi Chemical Co., Ltd., etc. can be used.

[0084] The sulfur content is 0.1 parts by mass or less, preferably 0.01 parts by mass or less, and more preferably 0 parts by mass, relative to 100 parts by mass of the butyl rubber. When the sulfur content is within the above range, a better effect tends to be obtained.

[0085] Here, the sulfur content refers to the amount of sulfur derived from pure sulfur components such as powdered sulfur, and does not include sulfur derived from sulfur-containing compounds such as phenol-sulfur chloride condensate.

[0086] As the cross-linking agent, it is preferred not to use a conventionally used organic peroxide or the like.

[0087] Examples of the organic peroxide include acyl peroxides such as benzoyl peroxide, dibenzoyl peroxide, and p-chlorobenzoyl peroxide; peroxyesters such as 1-butyl peroxyacetate, tert-butyl peroxybenzoate, and tert-butyl peroxyphthalate; ketone peroxides such as methyl ethyl ketone peroxide; alkyl peroxides such as di-tert-butyl peroxybenzoate and 1,3-bis(1-butylperoxyisopropyl)benzene; hydroperoxides such as tert-butyl peroxide (tert-butyl hydroperoxide); diisopropylbenzene peroxide; and tert-butylisopropylbenzene peroxide.

[0088] As commercially available products of the organic peroxide, for example, products of NOF Corporation, Arkema, Kawaguchi Pharmaceutical Industries, Ltd., Nourion, etc. can be used.

[0089] The content of the organic peroxide is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, further preferably 0.1 parts by mass or less, particularly preferably 0.01 parts by mass or less, and most preferably 0 parts by mass, relative to 100 parts by mass of the butyl rubber. When the content of the organic peroxide is within the above range, there is a tendency that a better effect can be obtained.

[0090] As the crosslinking aid (vulcanization accelerator), a thiazole vulcanization accelerator, a guanidine vulcanization accelerator, or a sulfenamide vulcanization accelerator can be used, and these can be used alone or in combination of two or more.

[0091] As thiazole vulcanization accelerators, for example, 2-mercaptobenzothiazole (MBT), sodium salt, zinc salt, copper salt, cyclohexylamine salt, dibenzothiazole disulfide (MBTS), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl-4-morpholinothio)benzothiazole, 2-(4'-morpholinodithio)benzothiazole, etc. can be mentioned. These can be used alone, or two or more can be used in combination. Among them, dibenzothiazole disulfide (MBTS) and 2-mercaptobenzothiazole (MBT) are preferred, and dibenzothiazole disulfide (MBTS) is more preferred because better effects can be obtained.

[0092] As guanidine vulcanization accelerators, for example, diphenylguanidine, di-o-tolylguanidine, triphenylguanidine, etc. can be mentioned. These can be used alone or in combination of two or more. Among them, diphenylguanidine is preferred because it can obtain better effects.

[0093] As sulfenamide-based vulcanization accelerators, for example, N-tert-butyl-2-benzothiazolyl sulfenamide (TBBS), N-cyclohexyl-2-benzothiazolyl sulfenamide (CBS), N,N'-dicyclohexyl-2-benzothiazolyl sulfenamide (DZ), etc. can be mentioned. These can be used alone, or two or more can be used in combination. Among them, based on the reason that better effects can be obtained, N-tert-butyl-2-benzothiazolyl sulfenamide is preferred.

[0094] As commercially available products of the cross-linking auxiliary agent (vulcanization accelerator), for example, products of Ouchi Shinko Chemical Co., Ltd., Kawaguchi Chemical Industry Co., Ltd., Sanshin Chemical Co., Ltd., etc. can be used.

[0095] Relative to 100 parts by mass of butyl rubber, the content of thiazole vulcanization accelerator and / or guanidine vulcanization accelerator and / or sulfenamide vulcanization accelerator is preferably 1 part by mass or more, more preferably 2 parts by mass or more, further preferably 3 parts by mass or more, particularly preferably 4 parts by mass or more. The content is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, further preferably 7 parts by mass or less, particularly preferably 6 parts by mass or less. When the content is within the above range, there is a tendency to obtain a better effect.

[0096] Here, the content of the thiazole vulcanization accelerator and / or the guanidine vulcanization accelerator and / or the sulfenamide vulcanization accelerator refers to the individual content when the thiazole vulcanization accelerator, the guanidine vulcanization accelerator or the sulfenamide vulcanization accelerator is used alone, and refers to the total content when two or more types are used in combination.

[0097] It is preferred not to use a quinone dioxime compound (quinoid compound) which is a conventionally used crosslinking auxiliary agent (vulcanization accelerator).

[0098] Examples of the quinone dioxime compound include p-benzoquinone dioxime, p-quinone dioxime, p-quinone dioxime diacetate, p-quinone dioxime dicaproate, p-quinone dioxime dilaurate, p-quinone dioxime distearate, p-quinone dioxime dicrotonate, p-quinone dioxime dicycloalkanoate), p-quinone dioxime succinate, p-quinone dioxime adipate, p-quinone dioxime difuroate (p-quinonedioxime difuroate), quinone dioxime dibenzoate, quinone dioxime di(o-chlorobenzoate), quinone dioxime di(p-chlorobenzoate), quinone dioxime di(p-nitrobenzoate), quinone dioxime di(m-nitrobenzoate), quinone dioxime di(3,5-dinitrobenzoate), quinone dioxime di(p-methoxybenzoate), quinone dioxime di(n-pentyloxybenzoate), quinone dioxime di(m-bromobenzoate), etc.

[0099] As commercially available products of the quinone dioxime compound, for example, products of Fujifilm Wako Pure Chemical Industries, Ltd., Junsei Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., LORD Corporation, and the like can be used.

[0100] The content of the quinone dioxime compound is preferably 1 part by mass or less, more preferably 0.5 part by mass or less, further preferably 0.1 part by mass or less, particularly preferably 0.01 part by mass or less, and most preferably 0 part by mass, relative to 100 parts by mass of the butyl rubber. When the content is within the above range, there is a tendency that a better effect can be obtained.

[0101] The rubber composition may contain stearic acid.

[0102] As stearic acid, conventionally known stearic acid can be used, and commercially available products include those of NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., etc. These can be used alone or in combination of two or more.

[0103] The content of stearic acid is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, relative to 100 parts by mass of butyl rubber, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, and further preferably 3 parts by mass or less. When the content is within the above range, there is a tendency that a better effect can be obtained.

[0104] In the rubber composition, inorganic fillers such as carbon black, silica, barium sulfate, talc, mica, mM2·xSiOy·zH2O (wherein M2 represents at least one metal selected from aluminum, calcium, magnesium, titanium and zirconium, or the oxide, hydroxide, hydrate or carbonate of the metal, m represents a value in the range of 1 to 5, x represents 0 to 10, y represents 2 to 5, and z represents a value in the range of 0 to 10) and plasticizers such as aromatic process oil, cycloparaffin process oil and paraffin process oil may be added. These may be used alone or in combination of two or more.

[0105] Specific examples of the filler represented by mM2·xSiOy·zH2O include aluminum hydroxide (Al(OH)3), aluminum oxide (Al2O3, Al2O3·3H2O (hydrate)), clay (Al2O3·2SiO2), kaolin (Al2O3·2SiO2·2H2O), pyrophyllite (Al2O3·4SiO2·H2O), bentonite (Al2O3·4SiO2·2H2O), aluminum silicate (Al2SiO5, Al4(SiO2)3·5H2O, etc. ), calcium aluminum silicate (Al2O3·CaO·2SiO2), calcium hydroxide (Ca(OH)2), calcium oxide (CaO), calcium silicate (Ca2SiO4), calcium magnesium silicate (CaMgSiO4), magnesium hydroxide (Mg(OH)2), magnesium oxide (MgO), talc (MgO·4SiO2·H2O), attapulgite (5MgO·8SiO2·9H2O), magnesium aluminum oxide (MgO·Al2O3), titanium dioxide (TiO2), titanium black (Ti n O 2n-1 ) etc. These may be used alone or in combination of two or more.

[0106] As commercially available products of the above-mentioned inorganic filler, for example, products of Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shin Nichia Carbon Co., Ltd., Columbia Carbon Co., Ltd., Degussa Co., Ltd., Rhodia Co., Ltd., Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd., Tokuyama Co., Ltd., etc. can be used.

[0107] As commercially available products of the above-mentioned plasticizers, for example, products of Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Nippon Energy Co., Ltd., Olisoy Co., Ltd., H&R Co., Ltd., Toyokuni Oil Refining Co., Ltd., Showa Shell Sekiyu Co., Ltd., Fuji Kosan Co., Ltd., Nissin Oillio Group Co., Ltd., and Taoka Chemical Industry Co., Ltd. can be used.

[0108] The content of the inorganic filler is preferably 1 part by mass or more, more preferably 10 parts by mass or more, and further preferably 20 parts by mass or more, relative to 100 parts by mass of the butyl rubber. The content is preferably 50 parts by mass or less, and more preferably 40 parts by mass or less. When the content is within the above range, there is a tendency that a better effect can be obtained.

[0109] Based on the viewpoint of preventing degradation caused by ultraviolet rays and based on the reason that appropriate reinforcement can be better ensured while ensuring good elongation at break, carbon black is preferred as the inorganic filler. At this time, the content of carbon black is preferably 1 part by mass or more, more preferably 10 parts by mass or more, and further preferably 20 parts by mass or more relative to 100 parts by mass of butyl rubber. The content is preferably 50 parts by mass or less, more preferably 40 parts by mass or less. When the content is within the above range, there is a tendency to obtain better effects.

[0110] As carbon black, general carbon black for rubber can be used appropriately. Specifically, N110, N115, N120, N121, N125, N134, N135, N219, N220, N231, N234, N293, N299, N326, N330, N335, N339, N343, N347, N351, N356, N358, N375, N539, N550, N582, N630, N642, N650, N660, N683, N754, N762, N765, N772, N774, N787, N907, N908, N990, N991, etc. can be used appropriately. In addition, our company's own synthetic products can also be used appropriately. These may be used alone or in combination of two or more.

[0111] As the plasticizer (oil), dioctyl phthalate (DOP) is preferred because a plasticizer having a low softening point is preferred in order to maintain a softened state at low temperatures.

[0112] In this specification, the plasticizer does not include the above-mentioned liquid polymer.

[0113] The content of the plasticizer is preferably 15 parts by mass or more, more preferably 20 parts by mass or more, relative to 100 parts by mass of the butyl rubber, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less.

[0114] The rubber composition may contain a thermoplastic resin as a binder.

[0115] As the thermoplastic resin, specific examples include rosin resins such as gum rosin, tall oil rosin, wood rosin, hydrogenated rosin, disproportionated rosin, polymerized rosin, glycerol and pentaerythritol esters of modified rosin; terpene resins such as α-pinene, β-pinene and dipentene terpene resins, aromatic modified terpene resins, terpene phenol resins and hydrogenated terpene resins; aliphatic petroleum resins obtained by polymerizing or copolymerizing C5 fractions obtained by pyrolysis of naphtha; aromatic petroleum resins obtained by polymerizing or copolymerizing C9 fractions obtained by pyrolysis of naphtha; copolymerized petroleum resins obtained by copolymerizing the above C5 fractions with C9 fractions; alicyclic compound petroleum resins such as hydrogenated and dicyclopentadiene-based petroleum resins; petroleum resins such as styrene, substituted styrene and styrene resins of copolymers of styrene and other monomers, etc. These can be used alone or in combination of two or more. Among them, aliphatic petroleum resins are preferred because better effects can be obtained.

[0116] As commercially available products of the above-mentioned thermoplastic resin, for example, products of Nippon Zeon Co., Ltd., Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF Corporation, Arizona Chemical Company, Nippon Paint Chemicals Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Energy Co., Ltd., Arakawa Chemical Industries, Ltd., and Taoka Chemical Industries, Ltd. can be used.

[0117] The content of the thermoplastic resin is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and further preferably 10 parts by mass or more, relative to 100 parts by mass of the butyl rubber. The content is preferably 50 parts by mass or less, more preferably 40 parts by mass or less. When the content is within the above range, there is a tendency that a better effect can be obtained.

[0118] In addition to the above components, the rubber composition may further contain additives generally used in the tire industry, such as silane coupling agents, various antioxidants, etc. The content of these additives is preferably 0.1 to 200 parts by mass relative to 100 parts by mass of the butyl rubber.

[0119] The rubber composition for sealants (sealants) is preferably prepared by mixing butyl rubber, a specific amount of zinc oxide, and a specific amount of liquid polymer, and more preferably prepared by mixing butyl rubber, a specific amount of zinc oxide, and a specific amount of polybutene.

[0120] By mixing the above materials to prepare a sealing material, and applying the prepared sealing material to the inner circumferential surface of the tire (preferably to the inner liner layer in the radial direction of the tire), a self-repairing tire having a sealing layer in the radial direction of the tire inner liner can be manufactured. The mixing of the materials constituting the sealing material can be carried out, for example, using a known mixer. An example of a manufacturing device used in the method for manufacturing a self-repairing tire is Figure 7 shown.

[0121] The inner circumference of the tire is coated with the sealing material, and the coating can be performed on at least the inner circumference of the tire corresponding to the tread portion, and more preferably, on at least the inner circumference of the tire corresponding to the buffer layer. By omitting the coating of the portion that does not need to be coated with the sealing material, a self-repairing tire can be manufactured with better productivity.

[0122] Here, the inner circumference of the tire corresponding to the tread portion refers to the inner circumference of the tire located at the radial inner side of the tread portion in contact with the road surface, and the inner circumference of the tire corresponding to the buffer layer refers to the inner circumference of the tire located at the radial inner side of the buffer layer. In addition, the buffer layer refers to a component arranged inside the tread and located outside the tire body in the radial direction, specifically, Fig. 9 The components shown are the buffer layer 16 and the like.

[0123] Usually, unvulcanized tires are vulcanized using a bladder. The bladder expands during vulcanization and comes into close contact with the inner circumference (inner liner) of the tire. Therefore, at the end of vulcanization, a release agent is usually applied to the inner circumference (inner liner) of the tire so that the bladder and the inner circumference (inner liner) of the tire do not adhere to each other.

[0124] As a release agent, a water-soluble coating or a release rubber is generally used. However, when a release agent is present on the inner circumferential surface of the tire, there is a concern that the adhesion between the sealing material and the inner circumferential surface of the tire will decrease. Therefore, it is preferred to remove the release agent from the inner circumferential surface of the tire in advance. In particular, it is more preferred to remove the release agent in advance from at least the portion of the inner circumferential surface of the tire where the sealing material is initially applied. In addition, it is further preferred to remove the release agent in advance from all portions of the inner circumferential surface of the tire where the sealing material is applied. As a result, the adhesion of the sealing material to the inner circumferential surface of the tire is further improved, and a self-repairing tire with higher sealing performance can be manufactured.

[0125] The method for removing the release agent from the inner circumferential surface of the tire is not particularly limited, and examples thereof include known methods such as buffing, laser treatment, high-pressure water washing, and removal with a detergent (preferably a neutral detergent).

[0126] By continuously and spirally attaching the sealing material to the inner circumference of the tire, the deterioration of the uniformity of the tire can be prevented, and a self-repairing tire with excellent weight balance can be manufactured. In addition, by continuously and spirally attaching the sealing material to the inner circumference of the tire, the sealing material can form a uniform sealing layer in the tire circumferential direction and the tire width direction (especially the tire circumferential direction), so a self-repairing tire with excellent sealing performance can be manufactured stably and productively. In addition, the sealing material is preferably attached without overlapping in the width direction, and more preferably attached seamlessly. In this way, the deterioration of the uniformity of the tire can be further prevented, and a more uniform sealing layer can be formed.

[0127] In addition, the raw materials are sequentially supplied to a continuous kneading machine (particularly a twin-shaft kneading extruder), the sealing material is sequentially prepared by the continuous kneading machine (particularly a twin-shaft kneading extruder), the prepared sealing material is continuously discharged from a nozzle connected to the discharge port of the continuous kneading machine (particularly a twin-shaft kneading extruder), and the sealing material is sequentially directly applied to the inner circumferential surface of the tire. Thus, a self-repairing tire can be manufactured with good productivity.

[0128] Preferably, the sealing layer is formed by continuously and spirally applying a substantially cord-shaped sealing material to the inner circumferential surface of the tire. Thus, a sealing layer composed of a substantially cord-shaped sealing material continuously and spirally arranged along the inner circumferential surface of the tire can be formed on the inner circumferential surface of the tire. The sealing layer can be formed by stacking sealing materials, but is preferably formed by one layer of sealing material.

[0129] When the sealing material is in a roughly cord-shaped form, a sealing layer consisting of one layer of sealing material can be formed by continuously applying the sealing material in a spiral shape to the inner circumference of the tire. When the sealing material is in a roughly cord-shaped form, since the applied sealing material has a certain thickness, even if the sealing layer is formed by one layer of sealing material, the deterioration of the uniformity of the tire can be prevented, and a self-repairing tire with excellent weight balance and good sealing performance can be manufactured. In addition, since only one layer of sealing material is applied without stacking any layers, the self-repairing tire can be manufactured with better productivity.

[0130] In order to prevent the deterioration of tire uniformity and to manufacture self-repairing tires with excellent weight balance and good sealing performance with better productivity, the number of times the sealing material is wound on the inner circumference of the tire is preferably 20 times or more, more preferably 35 times or more, and preferably 70 times or less, more preferably 60 times or less, and further preferably 50 times or less. Here, the number of windings 2 times means that the sealing material is applied to the inner circumference of the tire twice. Figure 4 The sealing material is wound 6 times.

[0131] Next, a method of applying the sealant to the inner peripheral surface of the tire will be described below.

[0132] <First Embodiment>

[0133] In the first embodiment, a self-repairing tire can be manufactured by a method including the following steps: step (1): while rotating the tire and moving at least one of the tire and the nozzle in the width direction of the tire, applying an adhesive sealing material to the inner circumferential surface of the tire through the nozzle, measuring the distance between the inner circumferential surface of the tire and the front end of the nozzle by a non-contact displacement sensor; step (2): based on the measurement result, adjusting the interval between the inner circumferential surface of the tire and the front end of the nozzle to a specified distance by moving at least one of the tire and the nozzle in the radial direction of the tire; step (3): applying the sealing material on the inner circumferential surface of the tire with the adjusted interval.

[0134] By using a non-contact displacement sensor to measure the distance between the inner circumference of the tire and the front end of the nozzle, and feeding back the measurement result, the interval between the inner circumference of the tire and the front end of the nozzle can be kept at a fixed distance. In addition, since the sealing material is applied to the inner circumference of the tire while maintaining the above-mentioned interval at a fixed distance, the thickness of the sealing material can be made uniform without being affected by the deviation of the tire shape or the unevenness of the joint. In addition, since there is no need to input coordinate values ​​for each tire size as in the traditional way, the sealing material can be applied efficiently.

[0135] Figure 1 : is a schematic diagram illustrating an example of a coating device used in a method for manufacturing a self-repairing tire. Figure 2 It is composed Figure 1 An enlarged view of the coating device near the nozzle front end is shown.

[0136] Figure 1 A cross section of a portion of the tire 10 cut along the meridian direction (a cross section cut on a plane including the tire width direction and the radial direction) is shown. Figure 2 A cross section of a portion of the tire 10 cut on a plane including the circumferential direction and the radial direction of the tire is shown. Figure 1 and Figure 2 , the X direction is the width direction (axial direction) of the tire, the Y direction is the circumferential direction of the tire, and the Z direction is the radial direction of the tire.

[0137] The tire 10 is arranged in a rotation drive device (not shown) which fixes and rotates the tire and moves the tire in the width direction and radial direction of the tire. The rotation drive device can independently perform rotation around the axis of the tire, movement in the width direction of the tire, and movement in the radial direction of the tire.

[0138] In addition, the rotation drive device includes a control mechanism (not shown) that can control the amount of movement of the tire in the radial direction. The control mechanism can control the amount of movement of the tire in the width direction and / or the rotation speed of the tire.

[0139] The nozzle 30 is mounted on the front end of an extruder (not shown) and can be inserted into the inner side of the tire 10. Then, the adhesive sealing material 20 extruded from the extruder is discharged from the front end 31 of the nozzle 30.

[0140] The non-contact displacement sensor 40 is mounted on the nozzle 30 , and measures a distance d between the inner peripheral surface 11 of the tire 10 and the front end 31 of the nozzle 30 .

[0141] As described above, the distance d measured by the non-contact displacement sensor is the distance between the inner peripheral surface of the tire and the tip of the nozzle in the radial direction of the tire.

[0142] In the method for manufacturing a self-repairing tire of the present embodiment, first, the tire 10 formed in the vulcanization step is mounted on a rotation drive device, and the nozzle 30 is inserted into the inner side of the tire 10. Then, as shown in FIG. Figure 1 and Figure 2 As shown, the sealing material 20 is continuously applied to the inner circumferential surface 11 of the tire 10 by discharging the sealing material 20 from the nozzle 30 while the tire 10 is rotated and moved in the width direction. The movement of the tire 10 in the width direction is performed along the contour shape of the inner circumferential surface 11 of the tire 10 input in advance.

[0143] As described later, the sealing material 20 is preferably in a roughly rope-shaped shape. More specifically, when the sealing material is applied to the inner circumferential surface of the tire, the sealing material preferably remains in a roughly rope-shaped shape. At this time, the roughly rope-shaped sealing material 20 can be continuously spirally attached to the inner circumferential surface 11 of the tire 10.

[0144] In the present specification, the term "substantially rope-shaped" means a shape having a length longer than a width and a certain degree of width and thickness. Figure 4 An example of a state in which a substantially rope-shaped sealing material is continuously and spirally attached to the inner circumference of a tire is schematically shown. Figure 8 Schematically shows the Figure 4 An example of a cross section of a sealing material when the sealing material is cut at a straight line AA perpendicular to the coating direction (length direction) of the sealing material. In this way, the substantially rope-shaped sealing material has a certain width ( Figure 8 length shown in W) and a certain degree of thickness ( Figure 8 Here, the width of the sealing material refers to the width of the sealing material after coating, and the thickness of the sealing material refers to the thickness of the sealing material after coating, more specifically, the thickness of the sealing layer.

[0145] The substantially rope-shaped sealing material, specifically, is a sealing material that satisfies the thickness of the sealing material described below (the thickness of the sealing material after coating, the thickness of the sealing layer, Figure 8 The preferred numerical range of the length shown by D in FIG. 1 ) and the width of the sealing material (the width of the sealing material after coating, Figure 4 The length shown by W, Figure 6 More preferably, it is a sealing material that satisfies the preferred numerical range of the ratio of the thickness of the sealing material to the width of the sealing material (the thickness of the sealing material / the width of the sealing material) described later. In addition, it can also be a sealing material that satisfies the preferred numerical range of the cross-sectional area of ​​the sealing material described later.

[0146] In the method for producing a self-repairing tire according to the present embodiment, a sealant is applied to the inner peripheral surface of the tire through the following steps (1) to (3).

[0147] <Step (1)>

[0148] like Figure 2 As shown, the distance d between the inner circumferential surface 11 of the tire 10 and the front end 31 of the nozzle 30 before the sealing material 20 is applied is measured by the non-contact displacement sensor 40. The distance d is measured each time the sealing material 20 is applied to the inner circumferential surface 11 of each tire 10, from the start of the application of the sealing material 20 to the end of the application.

[0149] <Step (2)>

[0150] The measured data of the distance d is transmitted to the control mechanism of the rotation drive device. The control mechanism adjusts the radial movement of the tire based on the measured data so that the distance between the inner circumference 11 of the tire 10 and the tip 31 of the nozzle 30 becomes a predetermined distance.

[0151] <Step (3)>

[0152] The sealing material 20 is continuously discharged from the front end 31 of the nozzle 30 and is therefore applied to the inner circumferential surface 11 of the tire 10 at the adjusted interval. Through the above steps (1) to (3), the sealing material 20 can be applied to the inner circumferential surface 11 of the tire 10 with a uniform thickness.

[0153] Figure 3 It is a schematic diagram illustrating the positional relationship of the nozzle relative to the tire.

[0154] like Figure 3As shown, the sealing material can be applied while the distance between the inner circumferential surface 11 of the tire 10 and the front end 31 of the nozzle 30 is maintained at a predetermined distance d0 while the nozzle 30 moves relative to the tire 10 to the positions shown in (a) to (d).

[0155] For the reason that a better effect can be obtained, the adjusted interval d0 is preferably 0.3 mm or more, more preferably 1.0 mm or more. In addition, the adjusted interval d0 is preferably 3.0 mm or less, more preferably 2.0 mm or less.

[0156] Here, the adjusted interval d0 refers to the distance between the inner peripheral surface of the tire and the tip of the nozzle in the radial direction of the tire after adjustment in the above step (2).

[0157] In order to obtain better effects, the adjusted interval d0 is preferably 30% or less, more preferably 20% or less of the thickness of the sealing material after coating, and is preferably 5% or more, more preferably 10% or more of the thickness of the sealing material after coating.

[0158] Based on the reason that better effects can be obtained, the thickness of the sealing material (the thickness of the sealing material after coating, the thickness of the sealing layer, Figure 8 The length (length shown in D) is not particularly limited, but based on the reason that better effects can be obtained, it is preferably 1.0 mm or more, more preferably 1.5 mm or more, further preferably 2.0 mm or more, and particularly preferably 2.5 mm or more. In addition, it is preferably 10 mm or less, more preferably 8.0 mm or less, and further preferably 5.0 mm or less. In addition, the thickness of the sealing material can be adjusted by adjusting the rotation speed of the tire, the moving speed in the width direction of the tire, the distance between the nozzle tip and the inner circumference of the tire, etc.

[0159] The thickness of the sealing material (the thickness of the sealing material after coating, the thickness of the sealing layer) is preferably substantially constant. This can further prevent deterioration of tire uniformity and produce a self-repairing tire with better weight balance.

[0160] Here, in this specification, the thickness being substantially constant means that the thickness fluctuation is controlled to be 90 to 110% (preferably 95 to 105%, more preferably 98 to 102%, and even more preferably 99 to 101%).

[0161] For reasons of less nozzle clogging, excellent operational stability, and better effects, it is preferred to use a substantially cord-shaped sealing material, and it is more preferred to attach the substantially cord-shaped sealing material spirally to the inner circumference of the tire. However, a sealing material that is not substantially cord-shaped may be used and applied to the inner circumference of the tire by spraying.

[0162] When using a substantially rope-shaped sealing material, the width of the sealing material (the width of the sealing material after application, Figure 4 The length (indicated by W) is not particularly limited, but is preferably 0.8 mm or more, more preferably 1.3 mm or more, and further preferably 1.5 mm or more for the reason that a better effect can be obtained. In addition, the width of the sealing material is preferably 18 mm or less, more preferably 13 mm or less, further preferably 9.0 mm or less, particularly preferably 7.0 mm or less, most preferably 6.0 mm or less, and most preferably 5.0 mm or less.

[0163] The thickness of the sealing material (the thickness of the sealing material after coating, the thickness of the sealing layer, Figure 8 The length shown by D in the figure) and the width of the sealing material (the width of the sealing material after coating, Figure 4 The ratio between the length (indicated by W in FIG. 1 ) and the length (indicated by W in FIG. 2 ) (thickness of the sealing material / width of the sealing material) is preferably 0.6 or more, more preferably 0.7 or more, further preferably 0.8 or more, particularly preferably 0.9 or more, and preferably 1.4 or less, more preferably 1.3 or less, further preferably 1.2 or less, particularly preferably 1.1 or less. The closer this ratio is to 1.0, the more the shape of the sealing material is an ideal rope-shaped shape, and the more productivity can be improved to manufacture a self-repairing tire with high sealing performance.

[0164] The cross-sectional area of ​​the sealing material (the cross-sectional area of ​​the sealing material after coating, Figure 8 The area calculated by D×W in the figure is preferably 0.8 mm because it can achieve better results. 2 More preferably 1.95 mm 2 Above, more preferably 3.0 mm 2 Above, 3.75mm is particularly preferred 2 Above, preferably 180mm 2 Below, more preferably 104mm 2 Below, more preferably 45mm 2 Below, especially preferably 35mm 2 Below, 25mm is most preferred 2 the following.

[0165] The width of the area where the sealing material is attached (hereinafter also referred to as the width of the attached area, the width of the sealing layer, Figure 4 The length shown as 6×W, Figure 6 The length (indicated by W1+6×W0) is not particularly limited, but based on the reason that better effects can be obtained, it is preferably more than 80% of the tread contact width, more preferably more than 90%, further preferably more than 100%. In addition, it is preferably less than 120%, more preferably less than 110%.

[0166] The width of the sealant layer is preferably 85 to 115% of the width of the tire breaker layer (the length of the breaker layer in the tire width direction) because a better effect can be obtained.

[0167] In this specification, when a plurality of breaker layers are provided in a tire, the length of the breaker layer in the tire width direction means the length of the breaker layer in the tire width direction that is the longest among the plurality of breaker layers.

[0168] In this specification, the tread contact width is defined as follows. First, when a tire is mounted on a regular rim and filled with a regular internal pressure and in a normal state without load, a regular load is applied to the tire, and the axially outermost contact position of the tire when the tire contacts the ground with a camber angle of 0 degrees is defined as the "contact end" Te. Then, the distance between the contact ends Te and Te in the tire axial direction is defined as the tread contact width TW. Unless otherwise specified, the dimensions of various parts of the tire are the values ​​measured in the normal state.

[0169] The above-mentioned "regular rim" refers to the rim specified for each tire in the specification system including the specification on which the tire is based, and refers to the "standard rim" in JATMA, the "design rim" in TRA, and the "measuring rim" in ETRTO. In addition, the above-mentioned "regular internal pressure" refers to the air pressure specified for each tire in the specification system including the specification on which the tire is based, and refers to the "maximum air pressure" in JATMA, the maximum value recorded in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES" in TRA, and the "INFLATION PRESSURE" in ETRTO. When the tire is for a passenger car, it is 180 kPa.

[0170] In addition, the above-mentioned "normal load" refers to the load specified for each tire in each specification in the specification system including the specifications on which the tire is based. In JATMA, it refers to the "maximum load capacity", in TRA, it refers to the maximum value recorded in the table "TIRE LOAD LIMITS ATVARIOUS COLD INFLATION PRESSURES (Tire load limits at various cold inflation pressures)", and in ETRTO, it refers to "LOAD CAPACITY (Load capacity)". When the tire is for passenger cars, it is a load equivalent to 88% of the above-mentioned load.

[0171] The rotation speed of the tire during application of the sealant is not particularly limited, but is preferably 5 m / min or more, more preferably 10 m / min or more, and is preferably 30 m / min or less, more preferably 20 m / min or less, for the purpose of obtaining better effects.

[0172] By using a non-contact displacement sensor, the risk of failure caused by the adhesion of sealing materials to the sensor can be reduced. As the non-contact displacement sensor used, there is no particular limitation as long as it can measure the distance between the inner circumference of the tire and the front end of the nozzle, and examples thereof include laser sensors, optical sensors, and electrostatic capacitance sensors. These sensors can be used alone, or two or more can be used in combination. Among them, from the viewpoint of measuring rubber, laser sensors and optical sensors are preferred, and laser sensors are more preferred. When using a laser sensor, the distance between the inner circumference of the tire and the front end of the laser sensor is measured based on the reflection of the laser by irradiating the inner circumference of the tire with a laser, and the distance between the front end of the laser sensor and the front end of the nozzle is subtracted from this value, thereby determining the distance between the inner circumference of the tire and the front end of the nozzle.

[0173] The position of the non-contact displacement sensor is not particularly limited as long as it can measure the distance between the inner circumference of the tire before the sealant is applied and the nozzle tip, but it is preferably mounted on the nozzle, and more preferably set at a position where the sealant is not attached.

[0174] Furthermore, there are no particular limitations on the number, size, etc. of the non-contact type displacement sensors.

[0175] Since the non-contact displacement sensor is not heat-resistant, it is preferable to protect it with a heat insulating material or the like and / or cool it with air or the like in order to prevent the heat influence of the high-temperature sealing material ejected from the nozzle. This can improve the durability of the sensor.

[0176] In the description of the first embodiment, an example in which the nozzle does not move but the tire moves is described as the movement in the width direction and the radial direction of the tire. However, the tire may not move but the nozzle moves, or both the tire and the nozzle may move.

[0177] In addition, the rotary drive device preferably has a means for expanding the width of the tire bead portion. When applying the sealing material to the tire, the sealing material can be easily applied to the tire by expanding the width of the tire bead portion. In particular, after the tire is mounted on the rotary drive device, when the nozzle is introduced near the inner circumference of the tire, the nozzle can be introduced only by parallel movement, which is easy to control and improves productivity.

[0178] As a means for expanding the width of the tire bead portion, as long as the width of the tire bead portion can be expanded, there is no particular limitation, and can include a device using 2 groups of multiple (preferably 2) rollers whose positions are constant, a mechanism moving along the tire width direction, etc. The device is placed in the tire from both sides of the tire opening to widen the width of the tire bead portion.

[0179] In the above manufacturing method, the sealing material mixed by a twin-screw kneading extruder and the cross-linking reaction in the extruder is directly applied to the inner circumference of the tire, so the cross-linking reaction starts from the time of application, not only has good adhesion to the inner circumference of the tire, but also the cross-linking reaction can be more appropriately carried out, and a self-repairing tire with high sealing performance can be manufactured. Therefore, there is no need to further cross-link the self-repairing tire coated with the sealing material, and good productivity can be obtained.

[0180] Furthermore, if necessary, a cross-linking step of further cross-linking the self-repairing tire coated with the sealant may be performed.

[0181] In the cross-linking process, the self-repairing tire is preferably heated. Thereby, the cross-linking speed of the sealing material can be increased, the cross-linking reaction can be better performed, and the self-repairing tire can be manufactured with better productivity. The heating method is not particularly limited, and a known method can be used, but a method using an oven is preferred. In the cross-linking process, for example, the self-repairing tire is placed in an oven at 70°C to 190°C (preferably 150°C to 190°C) for 2 to 15 minutes. In addition, since even the easily flowing sealing material just after coating can be prevented from flowing and the cross-linking reaction will not be deteriorated in uniformity, it is preferred to rotate the tire in the circumferential direction of the tire during cross-linking. The rotation speed is preferably 300 to 1000 rpm. Specifically, for example, as an oven, an oven with a rotating mechanism can be used.

[0182] In addition, even if the cross-linking process is not performed separately, it is preferred to rotate the tire in the tire circumferential direction until the cross-linking reaction of the sealing material is completed. Thus, even if the sealing material is easy to flow just after being applied, the cross-linking reaction can be prevented from flowing and the uniformity will not be deteriorated. The rotation speed is the same as in the case of the cross-linking process.

[0183] In order to increase the cross-linking speed of the sealing material, it is preferred to preheat the tire before applying the sealing material. In this way, self-repairing tires can be manufactured with better productivity. The preheating temperature of the tire is preferably above 40°C, more preferably above 50°C, and preferably below 100°C, more preferably below 70°C. By setting the preheating temperature of the tire within the above range, the cross-linking reaction can be started well from the time of coating, so that the cross-linking reaction proceeds more appropriately, and a self-repairing tire with high sealing performance can be manufactured. In addition, by setting the preheating temperature of the tire within the above range, there is no need to perform a cross-linking process, so that self-repairing tires can be manufactured with good productivity.

[0184] Continuous kneading machines (especially twin-shaft kneading extruders) are generally operated continuously. On the other hand, when manufacturing self-repairing tires, when the coating of one tire is completed, the tire needs to be replaced. In this case, in order to suppress the decline in productivity while manufacturing a higher quality self-repairing tire, the following methods (1) and (2) can be used. Since the method (1) has the disadvantages of reduced quality and the method (2) has the disadvantages of increased cost, it is sufficient to distinguish and use them according to the situation.

[0185] (1) Controlling the supply of sealing material to the inner surface of the tire by operating or stopping the continuous kneading machine and all supply devices simultaneously

[0186] That is, when coating of one tire is finished, the continuous mixer and all supply devices are stopped at the same time, the tire is replaced (preferably within 1 minute), the continuous mixer and all supply devices are started at the same time, and the coating of the tire is restarted. By quickly replacing the tire (preferably within 1 minute), the quality degradation can be suppressed.

[0187] (2) By keeping the continuous kneading machine and all supply devices in operation, the flow path is switched to control the supply of the sealing material to the inner peripheral surface of the tire.

[0188] That is, a flow path different from the nozzle that directly feeds the inner circumference of the tire is pre-set in the continuous mixer, and when the coating of one tire is completed, the prepared sealing material is discharged from another flow path until the tire replacement is completed. In this method, since the continuous mixer and all the supply devices can be kept in operation to manufacture the self-repairing tire, a higher quality self-repairing tire can be manufactured.

[0189] In addition, the carcass cord used in the carcass of the self-repairing tire is not particularly limited, and fiber cords, steel cords, etc. can be cited. Among them, steel cords are preferred. Steel cords formed of hard steel wires as specified in JIS G3506 are particularly desirable. In the self-repairing tire, by using high-strength steel cords instead of the commonly used fiber cords as carcass cords, the sidewall cut resistance (tolerance to sidewall cuts caused by riding on curbs, etc.) can be greatly improved, and the puncture resistance of the entire tire including the sidewall can be further improved.

[0190] The structure of the steel cord is not particularly limited, and examples thereof include single-twisted steel cords of 1×n, layer-twisted steel cords of k+m, bundle-twisted steel cords of 1×n, and multi-twisted steel cords of m×n. Here, the single-twisted steel cord of 1×n refers to a single-layer twisted steel cord obtained by twisting n filaments together. In addition, the layer-twisted steel cord of k+m refers to a steel cord having a two-layer structure with different twist directions and twist pitches, with k filaments in the inner layer and m filaments in the outer layer. In addition, the bundle-twisted steel cord of 1×n refers to a bundle-twisted steel cord obtained by twisting n filaments into a bundle. In addition, the multi-twisted steel cord of m×n refers to a multi-twisted steel cord obtained by twisting m strands obtained by twisting n filaments together. n is an integer of 1 to 27, k is an integer of 1 to 10, and m is an integer of 1 to 3.

[0191] The lay pitch of the steel cord is preferably 13 mm or less, more preferably 11 mm or less, and is preferably 5 mm or more, more preferably 7 mm or more.

[0192] The steel cord preferably includes at least one spirally shaped filament, which can provide a larger gap on the steel cord to improve rubber permeability, while maintaining the elongation at low loads to prevent poor forming during vulcanization.

[0193] In order to improve the initial adhesion to the rubber composition, the surface of the steel cord is preferably plated with brass, Zn or the like.

[0194] The elongation of the steel cord at a load of 50 N is preferably 0.5 to 1.5%, more preferably 0.7% or more, and more preferably 1.3% or less.

[0195] The density (ends) of the steel cord is preferably 20 to 50 (ends / 5 cm).

[0196] <Second Embodiment>

[0197] In the case of the method of the first embodiment alone, when the sealing material is roughly in the shape of a rope, it is sometimes difficult to attach the sealing material to the inner circumference of the tire. In particular, it has been clearly found that the sealing material at the beginning of attachment is easily peeled off. In the second embodiment, it is characterized in that in the method for manufacturing the self-repairing tire, the interval between the inner circumference of the tire and the front end of the nozzle is set to a distance d1, and after attaching the sealing material, the interval is set to a distance d2 greater than the distance d1, and the sealing material is attached. Thus, a self-repairing tire having the following characteristics can be easily manufactured: by making the interval between the inner circumference of the tire and the front end of the nozzle close at the beginning of attachment, the width of the sealing material corresponding to the beginning of attachment can be widened, and at least on the inner circumference of the tire corresponding to the tread portion, the adhesive and roughly rope-shaped sealing material is continuously spirally attached, and at least one of the ends of the sealing material in the length direction is a width portion having a width wider than the width of the adjacent portion in the length direction. In the self-repairing tire, by expanding the width of the sealing material corresponding to the attachment start portion, the bonding force in this portion can be improved, and the peeling of the sealing material in this portion can be prevented.

[0198] In the description of the second embodiment, only the differences from the first embodiment are mainly described, and description of the contents overlapping with the first embodiment is omitted.

[0199] Figure 5 It is composed Figure 1 The enlarged view of the nozzle tip of the coating device shown is a state immediately after the sealing material is attached, and (b) is a state after a predetermined time has passed.

[0200] Figure 5 The cross section of a portion of the tire 10 is shown in a plane including the tire circumferential direction and the radial direction. Figure 5 , the X direction is the width direction (axial direction) of the tire, the Y direction is the circumferential direction of the tire, and the Z direction is the radial direction of the tire.

[0201] In the second embodiment, first, the tire 10 formed in the vulcanization step is placed on the rotation drive device, and the nozzle 30 is inserted into the inner side of the tire 10. Figure 1 and Figure 5 As shown, the sealing material 20 is continuously applied to the inner circumferential surface 11 of the tire 10 by discharging the sealing material 20 from the nozzle 30 while the tire 10 is rotated and moved in the width direction. The movement of the tire 10 in the width direction is performed, for example, along the contour shape of the inner circumferential surface 11 of the tire 10 input in advance.

[0202] The sealing material 20 has adhesiveness and is in a substantially rope-like shape, so it can be continuously spirally attached to the inner peripheral surface 11 of the tire 10 corresponding to the tread surface.

[0203] At this time, within a specified period from the start of attachment, as Figure 5 (a) shows, the distance between the inner peripheral surface 11 of the tire 10 and the tip 31 of the nozzle 30 is set to d1, and the sealing material 20 is attached. Then, after the specified time has passed, as Figure 5 (b) shows, by moving the tire 10 in the radial direction, the above interval is changed to a distance d2 greater than the distance d1, and the sealing material 20 is attached.

[0204] In addition, before the attachment of the sealing material is completed, the above interval can be changed back from the distance d2 to the distance d1, but from the viewpoints of manufacturing efficiency and tire weight balance, it is preferable that the distance is d2 until the attachment of the sealing material is completed.

[0205] Furthermore, although it is preferable to keep the value of the above distance d1 fixed within a specified period from the start of attachment and keep the value of the above distance d2 fixed after the specified time has passed, as long as the relationship d1 < d2 is satisfied, the values of the distances d1 and d2 do not have to be fixed.

[0206] The value of the above distance d1 is not particularly limited. For the reason that better effects can be obtained, it is preferably 0.3 mm or more, more preferably 0.5 mm or more. The value of the above distance d1 is preferably 2 mm or less, more preferably 1 mm or less.

[0207] The value of the above distance d2 is also not particularly limited. For the reason that better effects can be obtained, it is preferably 0.3 mm or more, more preferably 1 mm or more. In addition, it is preferably 3 mm or less, more preferably 2 mm or less. The distance d2 is preferably the same as the above adjusted interval d0.

[0208] In addition, in this specification, the distances d1 and d2 between the inner peripheral surface of the tire and the tip of the nozzle refer to the distances in the radial direction of the tire between the inner peripheral surface of the tire and the tip of the nozzle.

[0209] The rotational speed of the tire when attaching the sealing material is not particularly limited. For the reason that better effects can be obtained, it is preferably 5 m / min or more, more preferably 10 m / min or more. In addition, it is preferably 30 m / min or less, more preferably 20 m / min or less.

[0210] Through the above process, the self-repairing tire of the second embodiment can be manufactured.

[0211] Figure 6 It is a schematic explanatory diagram of an example of the sealing material attached to the self-repairing tire of the second embodiment.

[0212] The sealing material 20, which is roughly in the shape of a rope, is wound around the circumference of the tire and continuously attached thereto in a spiral shape. In addition, one end of the sealing material 20 in the length direction is a width portion 21 having a width wider than the width of the adjacent portion in the length direction. The width portion 21 corresponds to the attachment start portion of the sealing material.

[0213] The width of the width portion of the sealing material (the width of the width portion of the sealing material after coating, Figure 6 The length shown in W1 in the figure is not particularly limited, but the width other than the width portion ( Figure 6 The width of the width portion of the sealing material is preferably less than 210% of the width outside the width portion, more preferably less than 180%, and further preferably less than 160%.

[0214] In addition, the width of the width portion of the sealing material is preferably substantially fixed in the longitudinal direction, but may be substantially not fixed. For example, the width portion may be a shape in which the width is the widest at the beginning of the attachment and the width becomes narrower along the longitudinal direction. Here, in this specification, the width is substantially fixed means that the variation of the width is controlled to be 90 to 110% (preferably 97 to 103%, more preferably 98 to 102%, and further preferably 99 to 101%).

[0215] The length of the width of the sealing material (the length of the width of the sealing material after coating, Figure 6 The length L1 in FIG. 1 is not particularly limited, but is preferably less than 650 mm, more preferably less than 500 mm, further preferably less than 350 mm, and particularly preferably less than 200 mm, for the sake of obtaining better effects. In addition, the shorter the width of the sealing material, the better, but in consideration of controlling the distance between the inner circumference of the tire and the front end of the nozzle, the limit is about 10 mm.

[0216] The width of the sealing material other than the width portion (the width of the sealing material other than the width portion after coating, Figure 6 The length shown in W0 in FIG. 1 is not particularly limited, but is preferably 0.8 mm or more, more preferably 1.3 mm or more, and further preferably 1.5 mm or more, and is preferably 18 mm or less, more preferably 13 mm or less, further preferably 9.0 mm or less, particularly preferably 7.0 mm or less, most preferably 6.0 mm or less, and most preferably 5.0 mm or less, based on the reason that a better effect can be obtained. W0 is preferably the same as W above.

[0217] In addition, the width of the sealing material other than the width portion is preferably substantially constant in the longitudinal direction, but there may be a portion where the width is not substantially constant.

[0218] The width of the area where the sealing material is attached (hereinafter also referred to as the width of the attached area, the width of the sealing layer, Figure 6 The length (represented by W1+6×W0) is not particularly limited, but is preferably 80% or more of the tread contact width, more preferably 90% or more, further preferably 100% or more, and preferably 120% or less, more preferably 110% or less, for better results.

[0219] The width of the sealant layer is preferably 85 to 115% of the width of the tire breaker layer (the length of the breaker layer in the tire width direction) because a better effect can be obtained.

[0220] In the self-repairing tire of the second embodiment, the sealant is preferably affixed so as not to overlap in the width direction, and more preferably affixed seamlessly.

[0221] In the self-repairing tire of the second embodiment, the other end portion of the sealant in the longitudinal direction (the end portion corresponding to the attachment end portion) may be a width portion wider than the width of the adjacent portion in the longitudinal direction.

[0222] The thickness of the sealing material (the thickness of the sealing material after coating, the thickness of the sealing layer, Figure 8 The length (shown as D) is not particularly limited, but is preferably greater than 1.0 mm, more preferably greater than 1.5 mm, further preferably greater than 2.0 mm, and particularly preferably greater than 2.5 mm, and is preferably less than 10 mm, more preferably less than 8.0 mm, and further preferably less than 5.0 mm, based on the reason that better effects can be obtained.

[0223] The thickness of the sealing material (thickness of the sealing material after coating, thickness of the sealing layer) is preferably substantially constant. Thus, deterioration of tire uniformity can be further prevented, and a self-repairing tire with better weight balance can be manufactured.

[0224] The thickness of the sealing material (the thickness of the sealing material after coating, the thickness of the sealing layer, Figure 8 The length indicated by D in the figure) and the width of the sealing material other than the width portion (the width of the sealing material other than the width portion after coating, Figure 6The ratio of the length (length shown in W0) to the thickness of the sealing material (the thickness of the sealing material / the width of the sealing material outside the width portion) is preferably 0.6 or more, more preferably 0.7 or more, further preferably 0.8 or more, and particularly preferably 0.9 or more, and is preferably 1.4 or less, more preferably 1.3 or less, further preferably 1.2 or less, and particularly preferably 1.1 or less. The closer this ratio is to 1.0, the more the shape of the sealing material becomes an ideal cord shape, and the more productively a self-repairing tire with high sealing performance can be manufactured.

[0225] The cross-sectional area of ​​the sealing material (the cross-sectional area of ​​the sealing material after coating, Figure 8 The area calculated by D×W in the figure is preferably 0.8 mm because it can achieve better results. 2 More preferably 1.95 mm 2 Above, more preferably 3.0 mm 2 Above, 3.75mm is particularly preferred 2 Above, preferably 180mm 2 Below, more preferably 104mm 2 Below, more preferably 45mm 2 Below, especially preferably 35mm 2 Below, 25mm is most preferred 2 the following.

[0226] In the second embodiment, even if the viscosity of the sealing material is within the above range, especially even if the viscosity is high, by widening the width of the sealing material corresponding to the attachment start portion, the bonding force in this portion can be improved and the peeling of the sealing material in this portion can be prevented.

[0227] The self-repairing tire of the second embodiment is preferably manufactured by the above-mentioned manufacturing method, but may be manufactured by any other appropriate manufacturing method as long as at least one end portion of the sealing material can be adjusted to a width portion.

[0228] The above description, especially in the description of the first embodiment, describes the case of using a non-contact displacement sensor when applying a sealing material to the inner circumferential surface of a tire. However, the sealing material can be applied to the inner circumferential surface of the tire by controlling the movement of the nozzle and / or the tire according to pre-input coordinate values ​​without performing measurements based on the non-contact displacement sensor.

[0229] According to the above-mentioned manufacturing method, a self-repairing tire having a sealing layer made of the above-mentioned sealing material rubber composition on the inner side of the inner liner in the tire radial direction can be manufactured. Since the sealing layer of the pneumatic tire is made of the above-mentioned sealing material rubber composition, it has excellent destruction characteristics, good sealing performance after years of degradation, and can also suppress the change of destruction characteristics over time.

[0230] The sealing layer is preferably composed of a substantially cord-shaped sealing material continuously arranged in a spiral shape along the inner circumferential surface of the tire. More preferably, the substantially cord-shaped sealing materials arranged in a spiral shape are arranged seamlessly without overlapping each other in the width direction.

[0231] The self-repairing tire of the above structure has excellent sealing performance because the inner circumference of the tire has a sealing layer (a sealing layer composed of a substantially cord-shaped sealing material continuously and spirally arranged along the inner circumference of the tire) with uniform sealing material in the tire circumferential direction and the tire width direction (especially in the tire circumferential direction). In addition, due to the sealing material, the balance of the tire is difficult to collapse, and the deterioration of the uniformity of the tire can be reduced.

[0232] Furthermore, by setting the sealing layer produced using the rubber composition for sealing material to have the above structure, there is a tendency to obtain a better effect. It is presumed that this is because the thickness of the sealing layer is ensured to be uniform, thereby achieving a better effect.

[0233] The sealing layer having the above-mentioned structure can be produced, for example, by continuously and spirally applying a substantially rope-shaped sealing material to the inner peripheral surface of the tire.

[0234] The complex elastic modulus G of the sealing layer measured at 100°C according to ISO13145 (2012) is * Preferably, it is 0.75 to 3.50 kPa. * It is more preferably 1.00 or more, further preferably 1.25 or more, particularly preferably 1.50 or more, most preferably 1.75 or more, still more preferably 2.00 or more, further most preferably 2.20 or more, particularly most preferably 2.30 or more, and more preferably 3.25 kPa or less, further preferably 3.00 kPa or less, particularly preferably 2.80 kPa or less, and most preferably 2.60 kPa or less. When the complex elastic modulus is within the above range, there is a tendency to obtain better effects. In addition, in this specification, the complex elastic modulus G * It is a value measured at 100° C. in accordance with ISO 13145 (2012), specifically, it is a value measured by the method of Examples.

[0235] In the sealing layer, in order to make the complex elastic modulus G * In the above range, the sealant can be produced by using the above rubber composition. In particular, for butyl rubber, a specific amount of zinc oxide and a specific amount of liquid polymer can be added.

[0236] More specifically, for butyl rubber, a specific amount of zinc oxide and a specific amount of liquid polybutene may be added.

[0237] Furthermore, it is preferred not to use a thiuram-based vulcanization accelerator, a dithiocarbamic acid-based vulcanization accelerator, or sulfur.

[0238] The tires described above can be suitably used as tires for passenger cars, tires for large passenger cars, tires for large SUVs, tires for trucks / buses, tires for two-wheeled vehicles, racing tires, winter tires (studless tires, snow tires, stud tires), all-season tires, run flat tires, aircraft tires, mining tires, and the like.

[0239] [Example]

[0240] The present invention will be specifically described based on the examples, but the present invention is not limited to these examples.

[0241] Various chemicals used in the examples are described below.

[0242] Butyl rubber: Bromobutyl 2255 (manufactured by ExxonMobil Corporation, Mooney viscosity at 125° C. ML1+8=46, halogen content: 2.0 mass %)

[0243] Carbon black: DIABLACK H (Mitsubishi Chemical Corporation, N330)

[0244] Liquid polybutene: Nippon Polybutene HV1900 (manufactured by JXTG Energy Co., Ltd., kinematic viscosity at 40°C 160,000 cSt, kinematic viscosity at 100°C 3,710 cSt, number average molecular weight 2,900)

[0245] Tackifier: Quintone A100 (manufactured by Japan Zeon Co., Ltd., aliphatic petroleum resin)

[0246] MBTS: NOCCELER DM-P (manufactured by Ouchi Shinko Chemical Co., Ltd., dibenzothiazolyl disulfide (MBTS))

[0247] DPG: NOCCELER D (manufactured by Ouchi Shinko Chemical Co., Ltd., diphenylguanidine)

[0248] BBS: NOCCELER NS-P (manufactured by Ouchi Shinko Chemical Co., Ltd., N-tert-butyl-2-benzothiazolylsulfenamide)

[0249] TBzTD: Sanceler TBzTD (manufactured by Sanshin Chemical Co., Ltd., tetrabenzylthiuram disulfide (TBzTD))

[0250] PZ: Accel PZ (manufactured by Kawaguchi Chemical Industry Co., Ltd., zinc dimethyldithiocarbamate (ZnMDC))

[0251] Zinc oxide: Zinc oxide No. 2 (manufactured by Mitsui Mining and Smelting Co., Ltd.)

[0252] Stearic acid: Tsubaki (manufactured by NOF Corporation)

[0253] Sulfur: Jinhua Yin micro powder sulfur (produced by Tsurumi Chemical Co., Ltd.)

[0254] <Manufacturing of self-repairing tires>

[0255] According to the formulation shown in Table 1, a sealing material was prepared by kneading the mixture at 170° C. for 60 minutes using a 3 L kneader mixer.

[0256] Next, the prepared sealing material (temperature 170°C, viscosity 35000 Pa·s (40°C), roughly in the shape of a rope, 3mm thick, 4mm wide) was sequentially discharged from a nozzle directly connected to the discharge port of the mixer and disposed on the inner surface of the tire, toward the inner surface of the tire (205 / 55R16, preheated temperature: 40°C) rotating in the circumferential direction. Figures 1 to 4 , the sealing material was continuously applied spirally to the inner circumference of the tire (spiral coating) to a thickness of 3 mm and a width of 180 mm in the attached area to form a sealing layer, thereby manufacturing a self-repairing tire. In addition, the viscosity of the sealing material was measured by a rotary viscometer at 40° C. in accordance with JIS K 6833.

[0257] Here, the crosslinking and curing reaction proceeds by the heat generated during kneading.

[0258] The following evaluations were performed using the obtained test tires. The results are shown in Table 1.

[0259] <Heat aging test>

[0260] The obtained test tires were stored at 60° C. for 20 days to obtain heat-aged test tires.

[0261] <Dynamic complex elastic modulus>

[0262] A test piece was cut from the sealant layer of the self-repairing tire (new, after heat aging). The dynamic complex elastic modulus G of the test piece was measured at 100°C using RPA manufactured by Alpha Technology in accordance with ISO 13145 (2012). * .

[0263] In addition, based on the new product and the G after thermal aging * , calculate the change ratio (G after thermal aging *The closer the change ratio is to 100%, the more the temporal change of the destruction characteristics can be suppressed. When the change ratio is 150% or less, it is judged that the temporal change of the destruction characteristics can be suppressed.

[0264] Complex elastic modulus G * (New) When it is above 0.75 kPa, it is judged that the fracture characteristics are excellent. In particular, when the complex elastic modulus G * (New product) When the pressure is 0.80 kPa or more, the destructive characteristics are judged to be more excellent.

[0265] <Airtightness>

[0266] The self-repairing tire (new product) was subjected to accelerated degradation at 60°C for 20 days, and then 100 nails were driven into the tire in a constant temperature room at -25°C. The success rate of airtightness when pulling out a long nail. The higher the success rate of airtightness, the better the sealing performance after years of degradation, and the more the deterioration of sealing performance over time can be suppressed.

[0267] <Shape Retention>

[0268] The self-repairing tires (new products) were subjected to accelerated degradation at 60° C. for 20 days and then evaluated. The qualified products with seal shape retention were rated as 0, and the unqualified products were rated as ×.

[0269] [Table 1]

[0270]

[0271] As can be seen from Table 1, the examples containing 2 to 15 parts by mass of zinc oxide and 100 to 300 parts by mass of liquid polymer relative to 100 parts by mass of butyl rubber, and containing 0.1 parts by mass or less of thiuram vulcanization accelerator, dithiocarbamic acid vulcanization accelerator, and sulfur, respectively, relative to 100 parts by mass of butyl rubber, have excellent destruction characteristics, good sealing properties after years of degradation, and can also suppress the change in destruction characteristics over time.

Claims

1. A rubber composition for a sealing material, It is characterized in that In the rubber composition, relative to 100 parts by mass of butyl rubber, the content of zinc oxide is 2 to 15 parts by mass, the content of liquid polymer is 100 to 300 parts by mass, the content of thiuram vulcanization accelerator, dithiocarbamic acid vulcanization accelerator and sulfur are respectively less than 0.1 parts by mass, and the content of organic peroxide is less than 0.1 parts by mass.

2. The rubber composition for a sealant according to claim 1, in, The liquid polymer is liquid polybutene.

3. The rubber composition for sealing material according to claim 1 or 2, in, The kinematic viscosity of the liquid polymer measured at 100° C. according to ASTM D445 is 500 to 6000 cSt.

4. A pneumatic tire, It is characterized in that A sealant layer is provided which is produced using the rubber composition according to any one of claims 1 to 3.