A lithium ion battery separator, preparation method and application thereof

By using a mixed coating of polymer resin and ceramic particles and a pore-forming agent in the lithium-ion battery separator, the problem of poor stability of the separator at high temperature is solved, the adhesion and peel strength are improved, and the safety of the battery is ensured. and performance stability.

CN114122623BActive Publication Date: 2024-11-15QINGDAO LANKETU MEMBRANE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010897359.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-31
Publication Date
2024-11-15
Estimated Expiration
2040-08-31

AI Technical Summary

Technical Problem

The existing lithium-ion battery separators have poor stability at high temperatures, insufficient adhesion and peel strength, which pose safety risks, and have high solubility in the electrolyte, which affects the cycling performance of the battery.

Method used

The mixed coating containing polymer resin and ceramic particles is used as the bonding functional layer, and the ceramic particles serve as the skeleton to provide support during the hot pressing process, and the bonding force is improved by copolymerizing vinylidene fluoride and hexafluoropropylene copolymers of different copolymerization ratios. The finger-like pores and honeycomb-like pore structures are formed by combining small molecules and large molecules pores to increase permeability and stability, and at the same time, the addition of a dispersant increases the peeling force.

Benefits of technology

It significantly improves the thermal stability, adhesion and peel strength of the lithium-ion battery separator, ensures the safety of the battery and the stability of the electrolyte, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114122623B_ABST
    Figure CN114122623B_ABST
Patent Text Reader

Abstract

The present invention provides a lithium-ion battery separator, a preparation method thereof and its application. The lithium-ion battery separator comprises a base film, a ceramic layer and an adhesive functional layer, wherein the ceramic layer is coated on one side of the base film, and the adhesive functional layer is coated on the outside of the base film and the ceramic layer; or, the ceramic layer is coated on both sides of the base film, and the adhesive functional layer is coated on the outside of the ceramic layer; the adhesive functional layer is a mixed coating comprising a polymer resin and ceramic particles. The lithium-ion battery separator of the present invention not only has high adhesion and high peel strength, and has no burrs on the end face during the slitting process, but also has high thermal stability, which effectively improves the safety of lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary battery separators, and in particular to a lithium ion battery separator, a preparation method thereof, and a lithium ion battery using the lithium ion battery separator. Background Art

[0002] In recent years, the annual output of lithium-ion batteries, the three major terminal products, has increased in a step-by-step manner. In 2016, the production capacity of consumer and power batteries both reached 20GWh, of which soft-pack batteries accounted for 75% of consumer batteries and 9% of power batteries. Data shows that from 2016 to 2020, the demand for consumer lithium batteries will support the steady growth of soft-pack batteries, and the total amount of power batteries is expected to continue to maintain a high growth rate, among which the proportion of soft-pack power batteries will continue to grow. By 2020, the demand for soft-pack power batteries is expected to reach 67GWh.

[0003] Unlike square, cylindrical, and aluminum-shell batteries, soft-package batteries use aluminum-plastic packaging film as the battery shell. The thickness of the aluminum-plastic film is about 110μm or thinner, and the appearance is soft and easy to deform. When the battery fails, the battery swells and the aluminum-plastic film bulges, which will not cause the shell of the battery to break due to increased pressure inside the battery. In addition, the weight of soft-package batteries is 40% lighter than that of steel-shell batteries of the same capacity, the capacity is 10-15% higher than that of steel-shell batteries of the same specifications, the internal resistance is small, and the design is flexible.

[0004] The disadvantage of soft-pack lithium-ion batteries is that the shell is easily deformed, which poses a safety hazard during transportation and use. The existing technology uses an oily PVDF coating film to heat and bond the diaphragm and the plate together to increase the stiffness of the battery cell, thereby improving the safety of the soft-pack battery. In addition, the oily PVDF diaphragm reduces the distance between the plate and the battery cell, thereby increasing the capacity of the battery under the same specifications and dimensions. In addition, the PVDF coating film has a large amount of electrolyte absorption and retention, which helps the battery's cycle performance. Due to the special contribution of oily PVDF to soft-pack batteries and the increasing demand for soft-pack battery diaphragms, domestic and foreign diaphragm companies are stepping up the layout of the research and development and industrialization of oily PVDF coated diaphragms.

[0005] Although the PVDF functional layer is directly coated on the polyolefin base film, the coating liquid has good compatibility with the base film, the peeling force between the coating layer and the base film of the finished film is large, and there is no poor slitting, but the thermal stability of the polyolefin base film directly coated with the adhesive porous layer diaphragm is poor. In order to improve the high temperature stability of the diaphragm and the safety of the battery, the prior art usually coats a ceramic layer on one or both sides of the polyolefin base film surface, and then coats the adhesive porous layer. At this time, due to the poor compatibility of the ceramic layer with the coating liquid, the peeling force between the adhesive functional layer and the ceramic layer of the finished film is small, there are burrs on the end face during the slitting process, and the product is poorly slid.

[0006] Therefore, there is an urgent need for a battery separator with high peel strength, high adhesion and excellent appearance to solve the above technical problems. Summary of the invention

[0007] One of the purposes of the present invention is to provide a lithium-ion battery separator which not only has high adhesion and high peel strength, and has no burrs on the end surface during the slitting process, but also has high thermal stability, thereby effectively improving the safety of lithium-ion batteries.

[0008] Another object of the present invention is to provide a method for preparing a lithium-ion battery separator. The lithium-ion battery separator prepared by this method has high adhesion, high peel strength, and high thermal stability, and the method is feasible and can be continuously industrialized.

[0009] To achieve the above objectives, the present invention provides a lithium-ion battery separator, comprising a base film, a ceramic layer, and an adhesive functional layer, wherein the ceramic layer is coated on one side of the base film, and the adhesive functional layer is coated on the outside of the base film and the ceramic layer; or, the ceramic layer is coated on both sides of the base film, and the adhesive functional layer is coated on the outside of the ceramic layer; the adhesive functional layer is a mixed coating comprising a polymer resin and ceramic particles. The ceramic particles can serve as the skeleton of the adhesive functional layer, providing compression-resistant support during the hot pressing process of the lithium-ion battery separator.

[0010] Preferably, the polymer resin is PVDF resin, including two copolymers of vinylidene fluoride and hexafluoropropylene in different copolymerization ratios. The use of two copolymers in different copolymerization ratios can not only effectively improve the bonding force of the bonding functional layer, but also ensure that the bonding functional layer is not excessively swollen and dissolved by the electrolyte.

[0011] Preferably, the ceramic particles are treated with lipophilic modification. The ceramic particles are preferably aluminum oxide, and the lipophilic modified ceramic particles can be evenly dispersed in the oily slurry.

[0012] Preferably, the adhesive functional layer is obtained by coating an adhesive functional layer slurry, and the adhesive functional layer slurry includes an oily solvent, a polymer resin, ceramic particles, a pore-forming agent, and a dispersant.

[0013] Preferably, the pore former includes a small molecule pore former and a macromolecular pore former.

[0014] The present invention also provides a method for preparing a lithium ion battery separator, comprising the following steps:

[0015] (1) coating a ceramic layer on one or both sides of a base film;

[0016] (2) after unwinding the film material obtained in step (1), coating both sides of the film material obtained in step (1) with an adhesive functional layer slurry; the adhesive functional layer slurry comprises an oily solvent, a polymer resin, ceramic particles, a pore-forming agent, and a dispersant;

[0017] (3) The film material obtained in step (2) enters the primary coagulation bath system, the secondary coagulation bath system, and the water washing system in sequence for treatment;

[0018] (4) The film material after being processed in step (3) enters into a drying system and a heat setting system in sequence for drying and setting, thereby obtaining the lithium-ion battery separator.

[0019] Preferably, the oily solvent is dimethylacetamide.

[0020] Preferably, the polymer resin is PVDF resin, including two copolymers of vinylidene fluoride and hexafluoropropylene with different copolymerization ratios; preferably, the mass ratio of the two copolymers is 2-10:2-10. The use of two copolymers with different copolymerization ratios can not only effectively improve the bonding force of the bonding functional layer, but also ensure that the bonding functional layer is not excessively swollen and dissolved by the electrolyte.

[0021] Preferably, the pore former includes a small molecule pore former and a macromolecular pore former; preferably, the mass ratio of the small molecule pore former to the macromolecular pore former is 2-10:2-10. By using pore formers of different molecular weights, an adhesive functional layer composed of finger-like pores and honeycomb-like pores can be obtained, which increases the permeability of the adhesive functional layer and ensures the smooth passage of lithium ions.

[0022] Preferably, the ceramic particles are lipophilic modified; preferably, the ceramic particles account for 2-15% by mass of the adhesive functional layer slurry. The ceramic particles can serve as the skeleton of the adhesive functional layer to provide compression-resistant support during the hot pressing process of the lithium-ion battery separator.

[0023] Preferably, the method for preparing the adhesive functional layer slurry comprises:

[0024] Step S1, adding a certain amount of the dispersant to a certain amount of the oily solvent, heating and stirring, so that the dispersant is completely dissolved;

[0025] Step S2, adding a certain amount of the ceramic particles into the mixed solution obtained in step S1, and stirring at high speed to make the ceramic particles evenly dispersed;

[0026] Step S3, adding a certain amount of the polymer resin and the pore-forming agent into the mixed solution obtained in step S2, and stirring them fully until they are completely dissolved, so as to obtain the adhesive functional layer slurry.

[0027] The present invention also provides a lithium ion battery, wherein the lithium ion battery comprises the lithium ion battery separator.

[0028] Preferably, the lithium-ion battery separator is prepared by the method for preparing the lithium-ion battery separator.

[0029] The present invention adopts a mixed coating containing polymer resin and ceramic particles as an adhesive functional layer to be coated on both sides of the base film and / or the ceramic layer, so that the ceramic particles serve as the skeleton of the adhesive functional layer to provide compression-resistant support during the hot pressing process of the lithium-ion battery separator; and by mixing and adopting two copolymers of vinylidene fluoride and hexafluoropropylene with different copolymerization ratios, not only can the adhesive force of the adhesive functional layer be effectively improved, but also the adhesive functional layer can be ensured not to be excessively swollen and dissolved by the electrolyte; thirdly, the present invention adopts a combination of pore-forming agents of different molecular weights to obtain an adhesive functional layer of a combination of finger-like pores and honeycomb-like pores, and the pore distribution is more uniform, which effectively increases the permeability of the adhesive functional layer and ensures the smooth passage of lithium ions; fourthly, the present invention adds a dispersant to the adhesive functional layer slurry, which can be used to eliminate part of the static electricity on the one hand, and on the other hand, the dispersant can be used as a surfactant, one end of which is connected to the ceramic layer and the other end is connected to the adhesive functional layer, thereby effectively increasing the peeling force between the adhesive functional layer and the ceramic layer and improving the cutting end face. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope of the present invention.

[0031] Figure 1 The scanning electron microscope (SEM) images of the adhesive functional layers of Example 1 and Comparative Example 3 of the present invention are shown. DETAILED DESCRIPTION

[0032] As used herein:

[0033] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0034] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0035] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0036] In these examples, parts and percentages are by mass unless otherwise indicated.

[0037] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.

[0038] One embodiment of the present invention provides a lithium-ion battery separator, comprising a base film, a ceramic layer, and an adhesive functional layer, wherein the ceramic layer is coated on one side of the base film, and the adhesive functional layer is coated on the outside of the base film and the ceramic layer; the adhesive functional layer is a mixed coating comprising a polymer resin and ceramic particles.

[0039] As a preferred embodiment, the ceramic layer is coated on both sides of the base film, and the adhesive functional layer is coated on the outer side of the ceramic layer; the adhesive functional layer is a mixed coating containing polymer resin and ceramic particles.

[0040] The present invention first coats a ceramic layer on one side or both sides of the base film surface, and uses the adhesive functional layer as the outermost layer of the lithium ion battery separator, which effectively improves the thermal stability of the lithium ion battery separator. The adhesive functional layer adopts a mixed coating containing a polymer resin and ceramic particles. The ceramic particles can serve as the skeleton of the adhesive functional layer and provide compression-resistant support during the hot pressing process of the lithium ion battery separator.

[0041] The lithium-ion battery separator of the present invention adopts the conventional base film and ceramic layer in the prior art, which will not be described here. Among them, the base film is preferably an ultra-high molecular weight polyethylene separator with a thickness of 5 to 20 μm and a porosity of 35 to 50%. In addition, the thickness of the ceramic coating is preferably 1 to 5 μm on one side and 2 to 10 μm on both sides; the thickness of the adhesive functional layer is preferably 0.5 to 4 μm on one side and 1 to 8 μm on both sides, and the porosity is preferably 40% to 60%. The air permeability value of the lithium-ion battery separator of the present invention can reach 100 to 300 S / 100cc.

[0042] As a preferred embodiment, the polymer resin in the adhesive functional layer is PVDF resin, including two copolymers of vinylidene fluoride and hexafluoropropylene with different copolymerization ratios. The use of two copolymers with different copolymerization ratios can not only effectively improve the adhesive force of the adhesive functional layer, but also ensure that the adhesive functional layer is not excessively swollen and dissolved by the electrolyte.

[0043] As a specific implementation, the PVDF resin in the adhesive functional layer includes a PVDF-A resin with a hexafluoropropylene copolymerization ratio of 0.5%-5% and a PVDF-B resin with a hexafluoropropylene copolymerization ratio of 5%-10%, and the mass ratio of the PVDF-A resin to the PVDF-B resin is 2-10:2-10. The greater the copolymerization ratio of hexafluoropropylene, the better the adhesiveness, but the adhesive functional layer is more easily swollen by the electrolyte, and the probability of the pore structure collapsing during use is higher. Therefore, the use of PVDF-A resin and PVDF-B resin mixed for use can effectively improve the problem of reduced adhesiveness caused by the addition of ceramic particles on the one hand, and on the other hand, it can effectively stabilize the pore structure and ensure that the adhesive functional layer is not easily excessively swollen and dissolved by the electrolyte.

[0044] As a preferred embodiment, the ceramic particles in the adhesive functional layer are treated with lipophilic modification. The ceramic particles are preferably aluminum oxide, preferably submicron-grade ceramic α-crystal; the lipophilic modified ceramic particles can be evenly dispersed in the oily slurry.

[0045] As a preferred embodiment, the adhesive functional layer is obtained by coating an adhesive functional layer slurry, and the adhesive functional layer slurry includes an oily solvent, a polymer resin, ceramic particles, a pore former, and a dispersant.

[0046] As a preferred embodiment, the pore former includes a small molecule pore former and a macromolecular pore former. By using pore formers of different molecular weights, an adhesive functional layer of a combination of finger-like pores and honeycomb-like pores can be obtained, and the pore distribution is more uniform, which effectively increases the permeability of the adhesive functional layer and ensures the smooth passage of lithium ions.

[0047] The lithium ion battery separator of the present invention has a peel strength between the adhesive functional layer and the ceramic layer greater than 30 N / m, and a bonding strength between the adhesive functional layer and the pole plate greater than 15 N / m.

[0048] Another embodiment of the present invention provides a method for preparing a lithium ion battery separator, comprising the following steps:

[0049] (1) coating a ceramic layer on one or both sides of a base film;

[0050] (2) after unwinding the film material obtained in step (1), coating both sides of the film material obtained in step (1) with an adhesive functional layer slurry; the adhesive functional layer slurry comprises an oily solvent, a polymer resin, ceramic particles, a pore-forming agent, and a dispersant;

[0051] (3) The film material obtained in step (2) enters the primary coagulation bath system, the secondary coagulation bath system, and the water washing system in sequence for treatment;

[0052] (4) the film material after the treatment in step (3) enters the drying system and the heat setting system in sequence for drying and setting, thereby obtaining the lithium-ion battery separator;

[0053] (5) Rolling up the lithium-ion battery separator obtained in step (4).

[0054] In the step (1), the base film and the ceramic layer are made of conventional base film materials and ceramic layer materials in the prior art, and the conventional ceramic layer coating process in the prior art is adopted, which will not be described in detail here.

[0055] As a preferred embodiment, in step (2), the coating temperature of the adhesive functional layer slurry is 20-40°C, and the coating tension is ≤30N / m; if the coating temperature is lower than 20°C, the pore-forming agent will settle out in the slurry during the coating process, and delamination will occur during the coating process; if the coating temperature is higher than 40°C, there will be problems such as reduced slurry viscosity and thinning coating thickness, which will affect the performance of the adhesive functional layer; and if the coating tension is greater than 30N / m, the diaphragm will be severely stretched, and appearance defects such as ribs will easily occur after winding.

[0056] As a preferred embodiment, in step (2), in the adhesive functional layer slurry, the oily solvent is dimethylacetamide (DMAC), and the mass fraction of DMAC in the adhesive functional layer slurry is preferably 80%-95%.

[0057] As a preferred embodiment, in step (2), in the adhesive functional layer slurry, the polymer resin is a PVDF resin, preferably comprising two copolymers of vinylidene fluoride and hexafluoropropylene with different copolymerization ratios, and the mass ratio of the two copolymers is preferably 2-10:2-10. The two copolymers of vinylidene fluoride and hexafluoropropylene with different copolymerization ratios are preferably PVDF-A resin with a hexafluoropropylene copolymerization ratio of 0.5%-5% and PVDF-B resin with a hexafluoropropylene copolymerization ratio of 5%-10%, wherein the mass fraction of PVDF-A resin in the adhesive functional layer slurry is preferably 2%-10%, and the mass fraction of PVDF-B resin in the adhesive functional layer slurry is preferably 2%-10%. The greater the copolymerization ratio of hexafluoropropylene, the better the adhesion, but the adhesive functional layer is more easily swollen by the electrolyte. At the same time, during use, the probability of pore structure collapse is higher. Therefore, the use of PVDF-A resin and PVDF-B resin in combination can, on the one hand, effectively improve the problem of reduced adhesion caused by the addition of ceramic particles, and on the other hand, effectively stabilize the pore structure and ensure that the adhesive functional layer is not easily excessively swollen and dissolved by the electrolyte.

[0058] As a preferred embodiment, in step (2), in the adhesive functional layer slurry, the ceramic particles are lipophilically modified, preferably aluminum oxide (Al2O3), and the weight percentage of the adhesive functional layer slurry is preferably 2-15%. The lipophilically modified ceramic particles can be evenly dispersed in DMAC without adding additional dispersants; the ceramic particles serve as the skeleton of the adhesive functional layer, providing compression-resistant support during the hot pressing process of the lithium-ion battery separator.

[0059] As a preferred embodiment, in step (2), in the adhesive functional layer slurry, the pore former includes a small molecule pore former and a macromolecular pore former, and the mass ratio of the small molecule pore former to the macromolecular pore former is preferably 2-10:2-10. Among them, the small molecule pore former is preferably a pore former with a molecular weight less than or equal to 2000, such as: polyvinyl alcohol, polyethylene glycol (PEG400~PEG2000); the macromolecular pore former is preferably a pore former with a molecular weight greater than 20000, such as: polyvinyl pyrrolidone K30 (PVPK30), hydroxymethyl cellulose, polyacrylamide (PAM), hydrolyzed polyacrylamide (HPAM), etc. The small molecule pore former has a small entanglement with the PVDF resin molecular chain and is easily eluted in the coagulation bath during the liquid-liquid phase separation process, thereby forming finger-like pores, while the macromolecular pore former has many entanglement points with the PVDF resin molecular chain and is eluted relatively slowly, thereby forming a honeycomb pore structure together with the small molecule pore former. In the present invention, the mass fraction of the small molecule pore former in the adhesive functional layer slurry is preferably 2%-10%, and the mass fraction of the macromolecular pore former in the adhesive functional layer slurry is preferably 2%-10%. By using pore formers of different molecular weights, an adhesive functional layer with a combination of finger-like pores and honeycomb-like pores can be obtained, and the pore distribution is more uniform, which effectively increases the permeability of the adhesive functional layer and ensures the smooth passage of lithium ions.

[0060] As a preferred embodiment, in step (2), in the adhesive functional layer slurry, the dispersant is an oily dispersant, such as triethylhexyl phosphate, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, fatty acid polyethylene glycol esters, etc., preferably unsaturated polyesters in primary shape. Unlike traditional coupling agents or surfactants, the dispersant of the present invention can first be uniformly dissolved in DMAC, will not cause caking or reaction to the slurry, and will not be eluted during the coagulation bath and water washing process. In the present invention, the mass fraction of the dispersant in the adhesive functional layer slurry is preferably 0.1%-3%. On the one hand, the dispersant can be used to eliminate some static electricity, and on the other hand, the dispersant can be used as a surfactant, one end of which is connected to the ceramic layer and the other end is connected to the adhesive functional layer, thereby effectively increasing the peeling force between the adhesive functional layer and the ceramic layer and improving the cut end face.

[0061] As a preferred embodiment, in step (2), the method for preparing the adhesive functional layer slurry comprises:

[0062] Step S1, adding a certain amount of dispersant to a certain amount of oily solvent, heating and stirring, so that the dispersant is completely dissolved;

[0063] Step S2, adding a certain amount of ceramic particles to the mixed solution obtained in step S1, and stirring at high speed to make the ceramic particles evenly dispersed;

[0064] Step S3, adding a certain amount of polymer resin and pore-forming agent into the mixed solution obtained in step S2, and stirring thoroughly until all of them are dissolved, so as to obtain the adhesive functional layer slurry.

[0065] As a preferred embodiment, in the method for preparing the adhesive functional layer slurry, in step S1, a dispersant is added to DMAC, the temperature is raised to 20-40°C and stirred at a low speed (≤100r / min) until the dispersant is completely dissolved. In the present invention, the dispersant is first added to DMAC, and the amount added is small; if the dispersant is added later, uneven dispersion will occur due to the high viscosity of the overall material.

[0066] As a preferred embodiment, in the method for preparing the adhesive functional layer slurry, in step S2, the ceramic particles after lipophilic modification are added to the mixed solution obtained in step S1, and stirred at high speed (≥500r / min) for 0.5 to 1 hour until the ceramic particles are evenly dispersed.

[0067] In the present invention, the dispersant is first added to DMAC in a small amount; the PVDF resin is added in the last step, which effectively avoids the uneven dispersion of the dispersant and ceramic particles due to the high viscosity of the slurry.

[0068] As a preferred embodiment, in step (3), the membrane material obtained in step (2) enters a primary coagulation bath system for phase separation. In this process, the DMAC in the coating and the DMAC in the primary coagulation bath system undergo double diffusion, and the DMAC concentration in the primary coagulation bath is the driving force for double diffusion. In the primary coagulation bath system of the present invention, the mass fraction of DMAC is preferably 60-90%. By adopting a high-concentration plasticizing bath system (i.e., a primary coagulation bath system), the liquid-liquid phase separation time is delayed, the phase separation speed is controlled, the pore size is adjusted, and a macroporous structure coating is prepared to avoid deformation and pore blocking due to stress on the coating. If the concentration of DMAC in the primary coagulation bath is too low, the DMAC diffusion process is accelerated, and the phase separation time of DMAC and PVDF resin in the coating is short, resulting in a small pore size, easy formation of a cortex, and is not conducive to the preparation of surface pores. After the primary coagulation bath, the DMAC content in the coating is reduced, and the surface layer PVDF is solidified, but the core still needs to continue phase separation, so a secondary coagulation bath is required. In the secondary coagulation bath system, the mass fraction of DMAC is preferably 30-50%. Finally, it enters the water washing system, and the mass fraction of DMAC in the water washing system is ≤3%. Water washing helps to fully clean the residual DMAC on the film material and avoid the generation of a large amount of organic waste gas in the subsequent drying process.

[0069] As a preferred embodiment, in step (4), the drying system adopts two methods: air drying and roller drying, wherein the wind temperature is preferably 50-80°C, the roller temperature is preferably 40-60°C, and the roller surface temperature should not be too high to avoid scalding the diaphragm; the heat setting system adopts rollers and air drying, wherein the wind temperature is preferably 80-120°C.

[0070] As a preferred embodiment, in step (5), the tension during the winding process is controlled to be ≤5N / m. In addition, in step (5), before the winding system is used for winding, a performance test step can be added, such as using an online thickness measurement system to measure the thickness of the lithium-ion battery separator, and / or using a defect detection system to detect whether the lithium-ion battery separator has defects, etc., wherein the performance test adopts existing technologies and will not be repeated here.

[0071] Another embodiment of the present invention further provides a lithium ion battery, which includes the lithium ion battery separator of the present invention.

[0072] As a preferred embodiment, the separator in the lithium ion battery is prepared by the method for preparing the separator of the lithium ion battery of the present invention.

[0073] The embodiments of the present invention will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0074] Example 1

[0075] In this embodiment, the lithium-ion battery separator includes a base film, a ceramic layer, and an adhesive functional layer, wherein the ceramic layer is coated on both sides of the base film, and the adhesive functional layer is coated on the outside of the ceramic layer as the outermost layer of the lithium-ion battery separator. The adhesive functional layer is a mixed coating comprising a polymer resin and ceramic particles, wherein the polymer resin is a PVDF resin, including a PVDF-A resin having a hexafluoropropylene copolymerization ratio of 0.5%-5% and a PVDF-B resin having a hexafluoropropylene copolymerization ratio of 5%-10%, and the mass ratio of the PVDF-A resin to the PVDF-B resin is 4:1; the ceramic particles are α-Al2O3, which has been subjected to lipophilic modification treatment; the mass ratio of α-Al2O3, PVDF-A resin and PVDF-B resin is 4:4:1.

[0076] According to the performance test, the lithium ion battery separator of this embodiment has a thickness of 16.1 μm and a surface density of 12±1.5 g / m 2The air permeability is 200±30S / 100cc. The adhesive functional layer is observed by scanning electron microscope, and it shows a combination of evenly distributed finger-like pores and honeycomb-like pores, such as Figure 1 (A) shown.

[0077] The lithium-ion battery of this embodiment includes the lithium-ion battery separator.

[0078] The preparation method of the lithium-ion battery separator of this embodiment is as follows: after unwinding the base film coated with a ceramic layer on both sides, a micro-concave roller is used to simultaneously coat the adhesive functional layer on both sides, the coating slurry temperature is 30°C, and the coating tension is ≤30N / m. Wherein, the adhesive functional layer slurry composition is: dimethylacetamide (DMAC) accounts for 82% by mass, PVDF-A resin with a hexafluoropropylene copolymerization ratio of 0.5%-5% accounts for 4% by mass, PVDF-B resin with a hexafluoropropylene copolymerization ratio of 5%-10% accounts for 1% by mass, α-Al2O3 accounts for 4% by mass, small molecule pore former PEG2000 accounts for 6% by mass, macromolecular pore former PVPK30 accounts for 2% by mass, and unsaturated polyester in the primary form of a dispersant accounts for 1% by mass; its preparation method is: step S1, 1% by mass of the dispersant primary form The unsaturated polyester is added with 82% by mass of DMAC, the temperature is raised to 30° C. and stirred at a low speed (≤100 r / min) to completely dissolve the dispersant; step S2, 4% by mass of α-Al2O3 is added to the obtained mixed solution, and stirred at a high speed (≥500 r / min) for 0.5 hour to uniformly disperse the ceramic particles; step S3, 4% by mass of PVDF-A resin, 1% by mass of PVDF-B resin, 6% by mass of PEG2000, and 2% by mass of PVPK30 are added to the mixed solution obtained in step S2, and stirred sufficiently until all dissolved. The coated film material enters the primary coagulation bath system for phase separation. The primary coagulation bath is a mixture of DMAC and water, where the mass concentration of DMAC is 70% and the temperature of the primary coagulation bath is 35°C; then it enters the secondary coagulation bath, which has the same composition as the primary coagulation bath, and is also a mixture of DMAC and water, where the mass concentration of DMAC is 40% and the temperature of the secondary coagulation bath is 35°C; then it enters the water washing system, which is still a mixture of DMAC and water, where the mass concentration of DMAC is 3%. The temperature of the water washing system is controlled at 30°C, and all coagulation baths and water washing systems are equipped with ultrasound. Then the film material passes through the drying system and the heat setting system in turn, where the wind temperature in the drying system is 70°C and the roller temperature is 50°C; the wind temperature in the heat setting system is 100°C. After drying and heat setting, the lithium-ion battery separator is obtained and rolled up through the winding system.

[0079] Example 2

[0080] In this embodiment, the lithium-ion battery separator includes a base film, a ceramic layer, and an adhesive functional layer, wherein the ceramic layer is coated on one side of the base film, and the adhesive functional layer is coated on the outside of the base film and the ceramic layer, as the outermost layer of the lithium-ion battery separator. The adhesive functional layer is a mixed coating comprising a polymer resin and ceramic particles, wherein the polymer resin is a PVDF resin, including a PVDF-A resin having a hexafluoropropylene copolymerization ratio of 0.5%-5% and a PVDF-B resin having a hexafluoropropylene copolymerization ratio of 5%-10%, and the mass ratio of the PVDF-A resin to the PVDF-B resin is 1:4; the ceramic particles are α-Al2O3, which has been subjected to lipophilic modification treatment; the mass ratio of α-Al2O3, PVDF-A resin and PVDF-B resin is 4:1:4.

[0081] According to the performance test, the lithium ion battery separator of this embodiment has a thickness of 15.5 μm and a surface density of 11±1.5 g / m 2 , the air permeability value is 180±30S / 100cc.

[0082] The lithium-ion battery of this embodiment includes the lithium-ion battery separator.

[0083] The preparation method of the lithium-ion battery separator of this embodiment is as follows: after unwinding the base film coated with a ceramic layer on one side, a micro-concave roller is used to simultaneously coat the adhesive functional layer on both sides, the coating slurry temperature is 20°C, and the coating tension is ≤30N / m. Wherein, the adhesive functional layer slurry composition is: dimethylacetamide (DMAC) accounts for 78.9% by weight, PVDF-A resin with a hexafluoropropylene copolymerization ratio of 0.5%-5% accounts for 1% by weight, PVDF-B resin with a hexafluoropropylene copolymerization ratio of 5%-10% accounts for 4% by weight, α-Al2O3 accounts for 4% by weight, small molecule pore former PEG400 accounts for 10% by weight, large molecule pore former HPAM accounts for 2% by weight, and dispersant sodium dodecyl sulfate accounts for 0.1% by weight; its preparation method is: step S1, 0.1% by weight of dispersant ten Sodium dialkyl sulfate is added to 78.9% by weight of DMAC, the temperature is raised to 35° C. and stirred at a low speed (≤100 r / min) to completely dissolve the dispersant; step S2, 4% by weight of α-Al2O3 is added to the obtained mixed solution, and stirred at a high speed (≥500 r / min) for 1 hour to evenly disperse the ceramic particles; step S3, 1% by weight of PVDF-A resin, 4% by weight of PVDF-B resin, 10% by weight of PEG400, and 2% by weight of HPAM are added to the mixed solution obtained in step S2, and stirred sufficiently until all dissolved. The coated film material enters the primary coagulation bath system for phase separation. The primary coagulation bath is a mixture of DMAC and water, where the mass concentration of DMAC is 70% and the temperature of the primary coagulation bath is 30°C; then it enters the secondary coagulation bath, which has the same composition as the primary coagulation bath, and is also a mixture of DMAC and water, where the mass concentration of DMAC is 30% and the temperature of the secondary coagulation bath is 30°C; then it enters the water washing system, which is still a mixture of DMAC and water, where the mass concentration of DMAC is 2%. The temperature of the water washing system is controlled at 25°C, and all coagulation baths and water washing systems are equipped with ultrasound. Then the film material passes through the drying system and the heat setting system in turn, where the wind temperature in the drying system is 50°C and the roller temperature is 60°C; the wind temperature in the heat setting system is 120°C. After drying and heat setting, the lithium-ion battery separator is obtained and rolled up through the winding system.

[0084] Example 3

[0085] In this embodiment, the lithium-ion battery separator includes a base film, a ceramic layer, and an adhesive functional layer, wherein the ceramic layer is coated on both sides of the base film, and the adhesive functional layer is coated on the outside of the ceramic layer as the outermost layer of the lithium-ion battery separator. The adhesive functional layer is a mixed coating comprising a polymer resin and ceramic particles, wherein the polymer resin is a PVDF resin, including a PVDF-A resin having a hexafluoropropylene copolymerization ratio of 0.5%-5% and a PVDF-B resin having a hexafluoropropylene copolymerization ratio of 5%-10%, and the mass ratio of the PVDF-A resin to the PVDF-B resin is 2:1; the ceramic particles are α-Al2O3, which has been subjected to lipophilic modification treatment; the mass ratio of α-Al2O3, PVDF-A resin and PVDF-B resin is 1:2:1.

[0086] According to the performance test, the lithium ion battery separator of this embodiment has a thickness of 17 μm and a surface density of 13 ± 1.5 g / m 2 , the air permeability value is 250±30S / 100cc.

[0087] The lithium-ion battery of this embodiment includes the lithium-ion battery separator.

[0088] The preparation method of the lithium-ion battery separator of this embodiment is as follows: after unwinding the base film coated with a ceramic layer on both sides, a micro-concave roller is used to simultaneously coat the adhesive functional layer on both sides, the coating slurry temperature is 40°C, and the coating tension is ≤30N / m. Among them, the adhesive functional layer slurry composition is: dimethylacetamide (DMAC) accounts for 74% by mass, PVDF-A resin with a hexafluoropropylene copolymerization ratio of 0.5%-5% accounts for 6% by mass, PVDF-B resin with a hexafluoropropylene copolymerization ratio of 5%-10% accounts for 3% by mass, α-Al2O3 accounts for 3% by mass, small molecule pore former PEG1000 accounts for 5% by mass, macromolecular pore former PVPK30 accounts for 8% by mass, and dispersant fatty acid polyethylene glycol ester accounts for 1% by mass; its preparation method is: step S1, 1% by mass of dispersant fatty acid 74% by mass of DMAC is added to the polyethylene glycol ester, the temperature is raised to 40°C and stirred at a low speed (≤100r / min) to dissolve all the dispersant; step S2, 3% by mass of α-Al2O3 is added to the obtained mixed solution, and stirred at a high speed (≥500r / min) for 1 hour to evenly disperse the ceramic particles; step S3, 6% by mass of PVDF-A resin, 3% by mass of PVDF-B resin, 5% by mass of PEG1000, and 8% by mass of PVPK30 are added to the mixed solution obtained in step S2, and stirred sufficiently until all are dissolved. The coated film material enters the primary coagulation bath system for phase separation. The primary coagulation bath is a mixture of DMAC and water, where the mass concentration of DMAC is 75% and the temperature of the primary coagulation bath is 40°C; then it enters the secondary coagulation bath, which has the same composition as the primary coagulation bath, and is also a mixture of DMAC and water, where the mass concentration of DMAC is 50% and the temperature of the secondary coagulation bath is 40°C; then it enters the water washing system, which is still a mixture of DMAC and water, where the mass concentration of DMAC is 1%. The temperature of the water washing system is controlled at 35°C, and all coagulation baths and water washing systems are equipped with ultrasound. Then the film material passes through the drying system and the heat setting system in turn, where the wind temperature in the drying system is 80°C and the roller temperature is 40°C; the wind temperature in the heat setting system is 95°C. After drying and heat setting, the lithium-ion battery separator is obtained and rolled up through the winding system.

[0089] Comparative Example 1

[0090] The only difference between this comparative example and Example 1 is that in this comparative example, the slurry used to prepare the adhesive functional layer of the lithium-ion battery separator does not contain PVDF-B resin.

[0091] According to the performance test, the lithium-ion battery separator of this comparative example has a thickness of 15.9 μm and a surface density of 12 ± 1.5 g / m 2 , the air permeability value is 190±30S / 100cc.

[0092] Comparative Example 2

[0093] The only difference between this comparative example and Example 1 is that in this comparative example, the slurry used to prepare the adhesive functional layer of the lithium-ion battery separator does not contain a dispersant.

[0094] According to the performance test, the lithium-ion battery separator of this comparative example has a thickness of 16.2 μm and a surface density of 12 ± 1.5 g / m 2 , the air permeability value is 195±30S / 100cc.

[0095] Comparative Example 3

[0096] The only difference between this comparative example and Example 1 is that in this comparative example, the slurry used to prepare the adhesive functional layer of the lithium-ion battery separator does not contain a macromolecular pore-forming agent.

[0097] According to the performance test, the lithium-ion battery separator of this comparative example has a thickness of 16.2 μm and a surface density of 12 ± 1.5 g / m 2 The air permeability is 230±30S / 100cc. The adhesive functional layer is observed by scanning electron microscope and shows a single finger-shaped hole, such as Figure 1 (B) shown.

[0098] Comparative Example 4

[0099] The only difference between this comparative example and Example 1 is that in this comparative example, the slurry used to prepare the adhesive functional layer of the lithium-ion battery separator does not contain ceramic particles.

[0100] According to the performance test, the lithium-ion battery separator of this comparative example has a thickness of 14 μm and a surface density of 10 ± 1.5 g / m 2 , the air permeability value is 200±30S / 100cc.

[0101] The present invention uses the following method to test the peeling force of the lithium ion battery separators of Examples 1-3 and Comparative Examples 1-3 of the present invention, wherein:

[0102] Test method for the peeling force between the adhesive functional layer and the electrode plate: The lithium-ion battery separators of Examples 1-3 and Comparative Examples 1-4 are respectively prepared into soft-pack lithium-ion batteries for testing, wherein the battery capacity is 1Ah, the positive electrode material is ternary nickel cobalt lithium manganese oxide 523 type, the negative electrode material is artificial graphite, the electrolyte is lithium hexafluorophosphate, and the battery cell adopts a winding type. Dry pressing conditions: 1000kgf hot pressing for 3 seconds, temperature 85°C. Hot pressing conditions after liquid injection: 600kgf hot pressing for 2 minutes, temperature 65°C. Test the peeling force between the adhesive functional layer and the electrode plate after dry pressing and wet pressing respectively. Peeling force test conditions: Cut the disassembled electrode plate (bonded to the separator) into sample strips with a width of 1cm and a length of 10cm, and use a universal tensile testing machine to test the peeling force between the separator and the electrode plate, tensile speed: 100mm / min;

[0103] Test method for the peeling force between the adhesive functional layer and the ceramic layer: a 1 cm wide and 10 cm long 3M tape is adhered to the adhesive functional layer, and the lithium ion battery separators of Examples 1-3 and Comparative Examples 1-4 are cut into sample strips with a width of 1 cm and a length of 10 cm along the edges of both sides of the 3M tape. A universal tensile testing machine is used to test the peeling force between the 3M tape and the separator. The 3M tape sticks down the adhesive functional layer, so the measured result shows the peeling force between the adhesive functional layer and the ceramic layer. The tensile speed is 100 mm / min.

[0104] The test results are shown in Table 1. It can be seen from Table 1 that if the adhesive functional layer slurry includes a single PVDF resin, such as excluding PVDF-B resin, the peeling force between the adhesive functional layer and the plate is significantly reduced, resulting in gaps between the plates after hot pressing of the soft-pack lithium-ion battery, large battery internal resistance, insufficient battery core hardness and other defects; if the adhesive functional layer slurry does not contain a dispersant, the peeling force between the adhesive functional layer and the ceramic layer is significantly reduced, resulting in burrs on the end face during the slitting process and poor product slitting; if the adhesive functional layer slurry includes a single pore former, such as excluding a macromolecular pore former, the pore distribution of the lithium-ion battery separator is uneven, resulting in uneven ion transmission process, resulting in severe polarization internal resistance and low discharge capacity during high-rate discharge; if the adhesive functional layer does not contain ceramic particles, PVDF is a soft phase during the hot pressing process of the battery core, especially during the hot pressing process after liquid injection. Under the action of temperature and pressure, PVDF deforms and causes the pore structure to be destroyed, which in turn leads to an increase in the battery internal resistance.

[0105] Table 1 Basic physical properties of lithium ion battery separators of Examples 1-3 and Comparative Examples 1-3

[0106]

[0107]

[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

[0109] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and to form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present invention and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing a lithium ion battery separator, characterized in that: The following steps are involved: (1) coating ceramic layers on both sides of the base film; (2) after unwinding the film material obtained in step (1), coating both sides of the film material obtained in step (1) with an adhesive functional layer slurry; the adhesive functional layer slurry comprises an oily solvent, a polymer resin, ceramic particles, a pore-forming agent, and a dispersant; (3) The film material obtained in step (2) enters the primary coagulation bath system, the secondary coagulation bath system, and the water washing system in sequence for treatment; (4) the film material after the treatment in step (3) enters the drying system and the heat setting system in sequence for drying and setting, thereby obtaining the lithium-ion battery separator; The preparation method of the adhesive functional layer slurry comprises: Step S1, adding a certain amount of the dispersant to a certain amount of the oily solvent, heating and stirring, so that the dispersant is completely dissolved; Step S2, adding a certain amount of the ceramic particles into the mixed solution obtained in step S1, and stirring at high speed to make the ceramic particles evenly dispersed; Step S3, adding a certain amount of the polymer resin and the pore-forming agent to the mixed solution obtained in step S2, and stirring thoroughly until all of them are dissolved; The dispersant is an oily dispersant; The dispersant accounts for 0.1%-3% of the adhesive functional layer slurry in terms of mass fraction; The pore former includes a small molecule pore former with a molecular weight less than or equal to 2000 and a macromolecular pore former with a molecular weight greater than 20000; the mass ratio of the small molecule pore former to the macromolecular pore former is 2-10:2-10; The small molecule pore formers include polyvinyl alcohol and polyethylene glycol; the macromolecular pore formers include polyvinyl pyrrolidone K30, hydroxymethyl cellulose, polyacrylamide, and hydrolyzed polyacrylamide; The ceramic particles are subjected to lipophilic modification treatment; The ceramic particles account for 2-15% by mass of the adhesive functional layer slurry.

2. The method for preparing a lithium ion battery separator according to claim 1, characterized in that: The oily solvent is dimethylacetamide.

3. The method for preparing a lithium ion battery separator according to claim 1 or 2, characterized in that: The polymer resin is PVDF resin, including two copolymers of vinylidene fluoride and hexafluoropropylene with different copolymerization ratios; The mass ratio of the two copolymers is 2-10:2-10.