A method for manufacturing a conformal radome
Through the manufacturing method of conformal radome, layer-by-layer laying and hot pressing curing technology, the poor reliability problem caused by the split design of antenna and radome is solved, and the connection and stability of the conduction layer and the inner cavity equipment are improved. Ensure communication performance in complex environments.
Patent Information
- Application Number
- CN202111422587.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-11-26
AI Technical Summary
The split design of existing antennas and radomes leads to poor system reliability and is difficult to meet the electrical performance requirements in complex environments. The traditional surface metallized conducting and reflecting layers are prone to scratches and peeling, affecting the stability of the system. .
By using the manufacturing method of conformal radome, high-strength glass fiber prepreg and electrically conductive materials are laid layer by layer in the molding mold, combined with hot pressing curing technology, an electrically conductive layer and a reflective layer are formed, and metal aluminum or Laying nickel-plated carbon felts to connect the electrically conductive layer to the inner cavity equipment, ensuring the accuracy of the position and shape between layers.
The electrical conduction layer and the inner cavity equipment are connected, the reliability and electrical performance of the system are improved, and the conduction layer and reflective layer are not easily scratched or peeled, with stable quality, and meet the communication needs in complex environments.
Smart Images

Figure CN114122709B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite material processing, and in particular to a method for manufacturing a conformal radome. Background Art
[0002] With the development of wireless communication technology, the application of multifunctional communication systems is becoming more and more extensive, and at the same time, higher requirements are placed on the design of antenna covers. In order to meet specific electrical performance requirements, the antenna and cover are sometimes designed as an integrated whole, in order to simplify the system structure, improve system reliability, and achieve electrical performance design requirements.
[0003] Conventional radomes only protect antennas from environmental factors such as rain, snow, wind, and sand. Usually, the antenna and radome are designed separately and then mechanically connected together. This type of design is simple, but the overall system reliability is poor, which seriously affects the reliability of the communication system. With the continuous improvement of system integration, conformal radomes have effectively solved the problem of poor system reliability, saved space, and achieved multifunctional integration. In terms of structure, conformal radomes require that the antenna's outer surface is conformal to the inner wall, outer wall, or interlayer surface of the radome; in terms of electrical performance, the conformal structure can realize signal transmission and reception. At the same time, in terms of protection, it can effectively prevent the impact and damage of harsh environments such as strong winds, salt spray, and heavy rain on the system, thereby extending the service life of the antenna, improving system reliability, and ensuring the antenna's all-weather operation. Summary of the invention
[0004] In view of this, the present invention provides a method for manufacturing a conformal radome. The electrical conductive layer and the reflective layer of the present invention are not easy to be scratched or peeled off, and have stable quality and high reliability.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for manufacturing a conformal radome comprises the following steps:
[0007] Step 1, establishing a radome forming mold; the mold includes a metal floor, a core mold, a reflective layer shaping and positioning tool, an electrical conductive layer shaping and positioning tool, an adjustment baffle and a flange pressing plate;
[0008] Step 2: fix the electrically conductive material on the core mold, and then lay the high-strength glass fiber prepreg layer by layer. After the laying is completed, fold the electrically conductive material to the outer surface of the prepreg, and then wrap the heat shrink tape on the outer surface and evacuate it, and pre-compact it at 60°C for 30 minutes;
[0009] Step 3, placing the preform and the mold assembly in step 2 in an oven, an autoclave or a hot press for heating, pressurizing and curing;
[0010] Step 4, polishing and cleaning the outer surface of the product formed by curing in step 3 to expose the electrically conductive material folded to the outer surface in step 2, and then spraying a metal aluminum layer through a conductive layer shaping and positioning tool, and connecting the aluminum layer with the electrically conductive material in step 2, and then connecting with the inner cavity device to form an electrically conductive layer; spraying a metal aluminum layer through a reflective layer shaping and positioning tool to form a reflective layer that is not connected with the inner cavity device;
[0011] Step 5, impregnating the aluminum layer with resin glue or laying a glue film on the surface of the aluminum layer, and then laying high-strength glass fiber prepreg layer by layer; laying high-strength glass fiber prepreg includes: flange laying, transition arc laying at the flange and overall wrapping laying; after laying, install the flange pressure plate, adjust the retaining edge and compact the flange;
[0012] Step 6, placing the preform and the mold assembly in step 5 in an oven, an autoclave or a hot press for heating, pressurizing and curing;
[0013] Step 7, take out the cured part formed in step 6 and demold it, remove the adjustment rib, flange pressure plate and bottom plate in turn, remove the core mold through the demolding tooling, remove the flash, and complete the preparation of the conformal antenna cover.
[0014] Furthermore, the curing molding process in step 3 and step 6 is: the pressure during the molding process is ≥ 0.1 MPa, first curing at 90° C. for 30 minutes, and then curing at 130° C. for 3 hours.
[0015] A method for manufacturing a conformal radome comprises the following steps:
[0016] Step 1, establishing a radome forming mold; the mold includes a metal floor, a core mold, a reflective layer shaping and positioning tool, an electrical conductive layer shaping and positioning tool, an adjustment baffle and a flange pressing plate;
[0017] Step 2: fix the electrically conductive material on the core mold, and then lay the high-strength glass fiber prepreg layer by layer. After the laying is completed, fold the electrically conductive material to the outer surface of the prepreg, and then wrap the heat shrink tape on the outer surface and evacuate it, and pre-compact it at 60°C for 30 minutes;
[0018] Step 3, laying nickel-plated carbon felt on the high-strength glass fiber prepreg in step 2, wherein the nickel-plated carbon felt is cut into shape and positioned by a shaping and positioning tool; after laying the nickel-plated carbon felt, a film is laid on the surface of the nickel-plated carbon felt and the high-strength glass fiber prepreg is laid layer by layer; laying the high-strength glass fiber prepreg includes: flange laying, transition arc laying at the flange, and overall wrapping laying; after the laying is completed, the flange pressure plate is installed, and the retaining edge is adjusted to compact the flange;
[0019] Step 4, placing the preform and the mold assembly in step 3 in an oven, an autoclave or a hot press for heating, pressurizing and curing;
[0020] Step 5, take out the cured part formed in step 4 and demold it, remove the adjustment rib, flange pressure plate and bottom plate in turn, remove the core mold through the demolding tooling, remove the flash, and complete the preparation of the conformal antenna cover.
[0021] Furthermore, the curing process in step 4 is as follows: the pressure during the molding process is ≥ 0.1 MPa, first curing at 90° C. for 30 minutes, and then curing at 130° C. for 3 hours.
[0022] The beneficial effects of the above technical solution of the present invention are:
[0023] 1. The present invention can form an electrical conductive layer and a reflective layer at any position between layers, and realize the connection between the electrical conductive layer and the inner cavity device, which has better designability. Compared with traditional surface metallization, the conductive layer and the reflective layer are not easy to be scratched or peeled off, and have stable quality and strong reliability.
[0024] 2. According to the requirements of electrical conductivity and reflection index, the present invention can select to prepare conformal radome by thermal spraying aluminum metal secondary curing molding, or by paving nickel-plated carbon felt one-time co-curing molding technology. If the electrical conductivity requirement is high, thermal spraying aluminum metal secondary curing molding technology is selected. If the electrical conductivity requirement is not high and production efficiency is taken into consideration, the one-time co-curing molding technology of paving nickel-plated carbon felt is selected.
[0025] 3. The present invention can better determine the position and shape of the thermally sprayed aluminum metal layer or the nickel-plated carbon felt through layer design combined with tooling design and use, and the thermally sprayed aluminum metal layer, the nickel-plated carbon felt and the prepreg are compositely co-cured using a resin or adhesive film with good bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the integrated structure of the conformal antenna and the cover;
[0027] Figure 2 This is a schematic diagram of the first stage of radome laying and mold assembly;
[0028] Figure 3 This is a schematic diagram of the second stage paving and mold assembly of the radome.
[0029] In the figure: 1. Radome body, 2. Electrically conductive layer, 3. Reflective layer, 4. Conductive connection hole, 5. Metal base plate, 6. Core mold, 7. Reflective layer shaping and positioning tool, 8. Electrically conductive layer shaping and positioning tool, 9. First stage preform paving, 10. Adjusting retaining edge, 11. Flange pressure plate, 12. Second stage preform paving. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] A method for manufacturing a conformal radome, using this processing and manufacturing technology, by accurately forming an electrical conductive layer and a reflective layer in the radome, a complex conformal antenna capable of transmitting and receiving directional beams can be prepared, and the integrated design and processing of the antenna and the radome can be achieved. The specific molding steps are as follows:
[0033] ① Establish a forming mold for the radome. Establish the mold required for the radome according to the product model. The mold includes a metal base plate 5, a core mold 6, a reflective layer shaping and positioning tool 7, a conductive layer shaping and positioning tool 8, an adjustment retaining edge 10, a flange pressing plate 11, etc. Establish the rigid metal base plate and the core mold according to the inner surface of the radome model. The shaping and positioning tools 7 and 8 are designed according to the position and shape of the conductive layer and the reflective layer of the electrical design. Establish a segmented rigid metal flange pressing plate 11 according to the outer surface of the radome flange.
[0034] ② In the first stage, apply 3 to 4 layers of release agent on the mold surface. In order to conduct with the inner cavity equipment, first design and fix strips of aluminum foil, nickel-plated carbon felt and other materials with good conductivity on the core mold. According to the layer design, lay high-strength glass fiber prepreg layer by layer on the core mold 5. The laying angle is 0° and 90° in a cycle. After the laying is completed, the excess aluminum foil or nickel-plated carbon felt is folded to the outer surface of the prepreg. The outer surface is wrapped with heat shrink tape and vacuumed at 60℃ for pre-compaction for 30 minutes.
[0035] ③ If thermal spraying of aluminum is used in the curing and molding step ④, the preform in step ②, i.e. the first stage paving preform 9, the metal base plate 5, the core mold 6, the simple retaining edge, etc. are placed on a device that can be heated and pressurized, such as an oven, an autoclave or a hot press, and the mold is heated to 90°C for 30 minutes, and then heated to 130°C for 180 minutes to cure and mold. The pressure during the molding process is not less than 0.1MPa. According to the product use environment and performance requirements, the appropriate pressure value is selected. If nickel-plated carbon felt is used in step ④, this step is omitted and step ④ is directly performed.
[0036] ④ Spraying metal aluminum (or laying nickel-plated carbon felt) Use hot spraying metal aluminum to form the conductive layer and the reflective layer. After step ③, polish and clean the outer surface of the product, remove the release agent, expose the aluminum foil or nickel-plated carbon felt and other conductive materials folded to the outer surface, and use the conductive layer shaping and positioning tool 8 to thermally spray the metal aluminum layer, so that the aluminum layer is connected to the conductive material in step ②, and then connected to the inner cavity equipment to form an conductive layer; spray the metal aluminum layer through the reflective layer shaping and positioning tool 7 to form a reflective layer that is not connected to the equipment. Use laying nickel-plated carbon felt to form the conductive layer and the reflective layer, then directly lay the nickel-plated carbon felt on the prepreg in step ②, and cut the shape and determine the position through the shaping and positioning tool.
[0037] ⑤ In the second stage, if step ④ of the paving adopts hot-sprayed metal aluminum, the aluminum layer is impregnated with resin glue or the adhesive film is laid on the surface of the aluminum layer, and the high-strength glass fiber prepreg is laid layer by layer according to the layer design; if step ④ adopts the paving of nickel-plated carbon felt, the adhesive film is laid on the surface of the nickel-plated carbon felt, and the high-strength glass fiber prepreg is laid layer by layer according to the layer design, wherein the flange plane is stacked and paved after unloading by a feeder, and the flange arc is wrapped with strips of prepreg with progressive widths in sequence, and finally the remaining prepreg is laid as a whole according to the designed number of layers, and the paving angles are 0° and 90° in a cycle, and after the paving is completed, the flange pressure plate 11 is installed, the retaining edge 10 is adjusted to compact the flange, and the remaining outer surfaces are wrapped with heat shrink tape.
[0038] ⑥ Curing and molding: Place the preform in step ⑤, i.e., the second-stage paving preform 12, and the mold assembly in an oven, autoclave or hot press, etc., which can be heated and pressurized. Heat the mold to 90°C and keep it warm for 30 minutes, then heat it to 130°C and keep it warm for 180 minutes to cure it. The pressure during the molding process is not less than 0.1MPa. According to the product use environment and performance requirements, the appropriate pressure value is selected. The thermal spraying metal aluminum method is the second curing molding, and the paving nickel-plated carbon felt method is the first curing molding.
[0039] ⑦ Demolding: Take out the product solidified in step ⑥ and demold it. Remove the adjustment rib 10, flange plate 11 and metal base plate 5 in sequence. Remove the core mold 6 through the demolding tooling and remove the flash of the product. The preparation of the integrated conformal antenna and cover is completed.
[0040] ⑧ After testing the conduction position of the product, the conduction connection hole 4 is machined according to the model, and a wire screw sleeve is inserted to connect the equipment and test the electrical conduction of the product.
[0041] The method realizes the integrated design and processing of a certain type of complex conformal antenna and cover, simplifies the system structure and improves the system reliability.
[0042] Compared with traditional molding methods, this processing and manufacturing technology, through layer design, combined with tooling design and use, can more accurately form the electrical conductive layer (i.e., conformal antenna) and the reflective layer, so that their position, shape, and thickness uniformity are more in line with theoretical requirements, and can better achieve design indicators, improve the electrical performance of the antenna cover, and realize the transmission and reception of directional beams.
[0043] This method can form an electrically conductive layer and a reflective layer at any position between the layers, and realize the connection between the electrically conductive layer and the inner cavity device, and has better designability. Compared with traditional surface metallization, its conductive layer and reflective layer are not easy to be scratched or peeled off, and have stable quality and strong reliability.
Claims
1. A method for manufacturing a conformal radome, characterized in that: The specific steps include: Step 1, establishing a radome forming mold; the mold includes a metal floor, a core mold, a reflective layer shaping and positioning tool, an electrical conductive layer shaping and positioning tool, an adjustment baffle and a flange pressing plate; Step 2: fix the electrically conductive material on the core mold, and then lay the high-strength glass fiber prepreg layer by layer. After the laying is completed, fold the electrically conductive material to the outer surface of the prepreg, and then wrap the heat shrink tape on the outer surface and evacuate it, and pre-compact it at 60°C for 30 minutes; Step 3, placing the preform and the mold assembly in step 2 in an oven, an autoclave or a hot press for heating, pressurizing and curing; Step 4, polishing and cleaning the outer surface of the product formed by curing in step 3 to expose the electrically conductive material folded to the outer surface in step 2, and then spraying a metal aluminum layer through a conductive layer shaping and positioning tool, and connecting the aluminum layer with the electrically conductive material in step 2, and then connecting with the inner cavity device to form an electrically conductive layer; spraying a metal aluminum layer through a reflective layer shaping and positioning tool to form a reflective layer that is not connected with the inner cavity device; Step 5, impregnating the aluminum layer with resin glue or laying a glue film on the surface of the aluminum layer, and then laying high-strength glass fiber prepreg layer by layer; Laying high-strength glass fiber prepreg includes: flange laying, transition arc laying at flange and overall wrapping laying; after laying, install flange pressing plate, adjust retaining edge and compact flange; Step 6, placing the preform and the mold assembly in step 5 in an oven, an autoclave or a hot press for heating, pressurizing and curing; Step 7, take out the cured part formed in step 6 and demold it, remove the adjustment rib, flange pressure plate and bottom plate in turn, remove the core mold through the demolding tooling, remove the flash, and complete the preparation of the conformal antenna cover.
2. The method for manufacturing a conformal radome according to claim 1, characterized in that: The curing molding process in step 3 and step 6 is as follows: the pressure during the molding process is ≥ 0.1 MPa, first curing at 90° C. for 30 minutes, and then curing at 130° C. for 3 hours.
3. A method for manufacturing a conformal radome, characterized in that: The specific steps include: Step 1, establishing a radome forming mold; the mold includes a metal floor, a core mold, a reflective layer shaping and positioning tool, an electrical conductive layer shaping and positioning tool, an adjustment baffle and a flange pressing plate; Step 2: fix the electrically conductive material on the core mold, and then lay the high-strength glass fiber prepreg layer by layer. After the laying is completed, fold the electrically conductive material to the outer surface of the prepreg, and then wrap the heat shrink tape on the outer surface and evacuate it, and pre-compact it at 60°C for 30 minutes; Step 3, laying nickel-plated carbon felt on the high-strength glass fiber prepreg in step 2, wherein the nickel-plated carbon felt is cut into shape and positioned by a shaping and positioning tool; after laying the nickel-plated carbon felt, laying a film on the surface of the nickel-plated carbon felt and laying the high-strength glass fiber prepreg layer by layer; Laying high-strength glass fiber prepreg includes: flange laying, transition arc laying at flange and overall wrapping laying; after laying, install flange pressing plate, adjust retaining edge and compact flange; Step 4, placing the preform and the mold assembly in step 3 in an oven, an autoclave or a hot press for heating, pressurizing and curing; Step 5, take out the cured part formed in step 4 and demold it, remove the adjustment rib, flange pressure plate and bottom plate in turn, remove the core mold through the demolding tooling, remove the flash, and complete the preparation of the conformal antenna cover.
4. The method for manufacturing a conformal radome according to claim 3, characterized in that: The curing process in step 4 is as follows: the pressure during the molding process is ≥ 0.1 MPa, first curing at 90° C. for 30 minutes, and then curing at 130° C. for 3 hours.