Preparation method and device of ferrous sulfate solution for iron oxide pigment, and iron oxide pigment
Through the displacement reaction and hydrolysis reaction between reduced ilmenite and ferrous sulfate solution, the problem of the impact of impurities in sulfuric acid production is solved, the production cost of iron oxide pigments is reduced, and artificial rutile is used to reduce alkali consumption and improve the pigment quality. performance.
Patent Information
- Application Number
- CN202111666080.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-12-31
AI Technical Summary
In the existing technology, the ferrous sulfate by-product produced during the production of titanium dioxide by the sulfuric acid method contains impurities, such as Ti, Al, etc., which affect the color and performance of the pigment, and the cost of adjusting the pH value with NaOH is high, making it difficult to reduce the cost of iron oxide pigments. production costs.
The substitution reaction between reduced ilmenite and ferrous sulfate solution is used to increase the pH value, promote hydrolysis and remove titanium and Al impurities, and replace sodium hydroxide to adjust the pH and reduce alkali consumption.
It can effectively reduce the cost of iron oxide pigments, improve the color and performance of the pigments, and further utilize it to produce downstream products by obtaining artificial rutile.
Smart Images

Figure CN114162875B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron oxide pigment and waste recycling, and in particular to a method and device for preparing a ferrous sulfate solution for iron oxide pigment and the iron oxide pigment. Background Art
[0002] In recent years, the demand for red iron oxide in my country has continued to increase, with an annual growth rate of up to 107%, far higher than the 36.6% growth rate of the entire iron oxide pigment. It is the iron pigment second only to iron black and iron yellow.
[0003] The sulfuric acid process for producing titanium dioxide is based on ilmenite (FeTiO 3 ) as raw material, sulfuric acid is used to decompose the ore, titanium and iron are dissolved as sulfate, and then iron is dissolved as ferrous sulfate (FeSO 4 7H 2 O) crystallizes and separates from the titanium liquid, becoming the main by-product of titanium dioxide production by this method. Ferrous sulfate, also known as green vitriol, is a solid waste in the production of titanium dioxide by sulfuric acid method. The production of 1 ton of titanium dioxide produces about 3 to 3.2 tons of ferrous sulfate heptahydrate. The value of ferrous sulfate itself is not high, but if it is used as a raw material for the production of iron oxide pigments, it can not only effectively utilize resources and reduce environmental pollution, but also reduce the production cost of iron oxide red. If the by-product ferrous sulfate of titanium dioxide is used as a raw material to synthesize iron oxide pigments, it can further save costs and avoid waste of resources.
[0004] Ferrous sulfate, a byproduct of titanium dioxide, contains about 95% ferrous salts, as well as various impurities such as Ti, Mn, Mg, and Al. These impurities mixed in the finished pigment will affect the color and performance of the pigment, especially Ti and Al.
[0005] After the ferrous sulfate produced as a byproduct of titanium dioxide is dissolved in water, the pH value is low, generally around 0.5, which is not conducive to the hydrolysis of titanium. In the prior art, the pH value of the ferrous sulfate solution is often adjusted by adding NaOH. However, the cost of NaOH is high, which is not conducive to reducing the cost of iron oxide pigments.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The first object of the present invention is to provide a method for preparing a ferrous sulfate solution for an iron oxide pigment. By reducing ilmenite to adjust the pH of the ferrous sulfate solution produced as a byproduct of titanium dioxide, the pH value of the mixture can be increased after the iron in the reduced ilmenite undergoes a substitution reaction with the acid, thereby promoting the conversion of aluminum ions and titanium acyl ions (TiO 2+) is hydrolyzed to remove impurities such as titanium and aluminum, and the use of reduced ilmenite instead of traditional sodium hydroxide can reduce alkali consumption and reduce costs. In addition, the iron in the reduced ilmenite is removed by reacting with hydrogen ions to obtain artificial rutile.
[0008] The second object of the present invention is to provide a device for preparing ferrous sulfate solution for iron oxide pigment, which has the advantages of simple structure, convenient operation, cost saving, etc.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] The present invention provides a method for preparing a ferrous sulfate solution for an iron oxide pigment, comprising the following steps:
[0011] (a) mixing a titanium dioxide by-product ferrous sulfate solution with reduced ilmenite, so that the iron in the reduced ilmenite undergoes a substitution reaction with the hydrogen ions in the ferrous sulfate solution, and the titanyl ions and aluminum ions in the ferrous sulfate solution undergo a hydrolysis reaction;
[0012] (b), after the replacement reaction and the hydrolysis reaction are completed, the mixed material is allowed to stand and separated to obtain a supernatant and a slag respectively, the supernatant is mixed with a flocculant solution for flocculation precipitation, and then after solid-liquid separation, the ferrous sulfate solution for the iron oxide pigment is obtained, and the slag is subjected to solid-liquid separation to obtain artificial rutile;
[0013] Wherein, the titanium dioxide by-product ferrous sulfate solution is obtained by dissolving ferrous sulfate heptahydrate crystals, a by-product of the production of titanium dioxide pigment by sulfuric acid method;
[0014] The cations in the titanium dioxide byproduct ferrous sulfate solution include titanyl ions, aluminum ions, ferrous ions and hydrogen ions.
[0015] Reduced ilmenite refers to the reduced ilmenite obtained by high-temperature reduction of ilmenite, the main component of which is TiO 2 and metallic Fe.
[0016] The titanium dioxide by-product ferrous sulfate is a by-product ferrous sulfate heptahydrate crystal in the process of producing titanium dioxide pigment by sulfuric acid method. The titanium dioxide by-product ferrous sulfate solution is obtained by dissolving the ferrous sulfate heptahydrate crystal in water.
[0017] The pH value of the titanium dioxide byproduct ferrous sulfate solution is relatively low, generally around 0.5, which is not conducive to the hydrolysis of titanium. Therefore, the present invention adds reduced ilmenite, in which the iron will undergo a replacement reaction with the hydrogen ions in the titanium dioxide byproduct ferrous sulfate solution, thereby increasing the pH of the mixture and promoting the decomposition of aluminum ions and titanium acyl ions (TiO 2+ ) is hydrolyzed to remove titanium and aluminum impurities. In addition, using reduced ilmenite instead of sodium hydroxide to adjust pH can reduce alkali consumption, thereby reducing costs.
[0018] In addition, the iron in the reduced ilmenite is removed by reacting with hydrogen ions to obtain artificial rutile, which can be used to produce downstream products.
[0019] The reaction principle of the method for preparing ferrous sulfate solution for iron oxide pigment provided by the present invention is as follows:
[0020] In step (a), the iron in the reduced ilmenite undergoes a replacement reaction with the hydrogen ions in the ferrous sulfate solution, and the titanyl ions and aluminum ions in the ferrous sulfate solution undergo a hydrolysis reaction:
[0021] Fe+2H + =Fe 2+ +H 2 ↑;
[0022] TiO 2+ +3H 2 O=Ti(OH) 4 +2H + ;
[0023] Al 3+ +3H 2 O=Al(OH) 3 +3H + .
[0024] The iron in the reduced ilmenite can react with the hydrogen ions in the ferrous sulfate solution produced as a by-product of titanium dioxide, thereby increasing the pH value of the solution and promoting the hydrolysis of titanium and aluminum ions in the solution. At the same time, the iron can continue to react with the hydrogen ions produced after the hydrolysis of titanium and aluminum, further promoting the hydrolysis of titanium and aluminum ions, thereby better reducing the titanium and aluminum impurities in the solution.
[0025] After the replacement reaction and the hydrolysis reaction are completed, the mixed material is allowed to stand and separated in turn to obtain a supernatant and slag. Since the reduced ilmenite has a large density, the reduced ilmenite in the mixed material will settle to the bottom after the mixed material is allowed to stand for a period of time. At this time, the supernatant is first extracted, and then the remaining slag (the slag contains a portion of liquid) is discharged, that is, the separation of the supernatant and the slag is completed.
[0026] The particles of the hydrolyzed titanium acyl ions and aluminum ions will be suspended in the supernatant, so the supernatant is mixed with a flocculant solution for flocculation precipitation, which can make the hydrolyzed particles settle, and then the ferrous sulfate solution for the iron oxide pigment is obtained by solid-liquid separation.
[0027] At the same time, the slag obtained by the above separation is subjected to solid-liquid separation, and the main component of the slag is the reduced ilmenite after the reaction, and most of the iron in it is removed, that is, artificial rutile is obtained.
[0028] In addition, the ferrous sulfate solution for the iron oxide pigment provided by the present invention has low impurity content, especially titanium and aluminum which have a greater impact on the pigment are removed in large quantities, thus improving the color and performance of the iron oxide pigment.
[0029] Preferably, in step (a), the molar ratio of the iron element in the reduced ilmenite to the hydrogen ions in the titanium dioxide byproduct ferrous sulfate solution is 1.1-1.5 (or 1.2, 1.3 or 1.4): 2. That is, the iron in the reduced ilmenite is slightly excessive.
[0030] Preferably, in step (a), the mass fraction of iron in the titanium dioxide by-product ferrous sulfate solution is 6% to 8%, including but not limited to any one of 6.5%, 7%, and 7.5% or a range between any two of them.
[0031] By adopting the above molar ratio and the above mass fraction, the pH value of the mixed material can be increased to greater than 3, thereby promoting the hydrolysis of aluminum sulfate and titanyl sulfate impurities in the mixed material.
[0032] In some specific embodiments of the present invention, since the iron in the ilmenite is excessive during the reaction, the slag after the first reaction can be left in the reaction device for recycling, which can also further reduce the iron content in the artificial rutile.
[0033] In some specific embodiments of the present invention, the slag separated in step (b) contains a portion of liquid material, so the liquid material obtained after solid-liquid separation of the slag can be transported to the flocculation sedimentation device to further recover the ferrous sulfate solution.
[0034] Preferably, in step (a), the pH value of the titanium dioxide by-product ferrous sulfate solution is 0 to 1.5.
[0035] Preferably, in step (a), the temperature of the mixed material is 80-95°C, including but not limited to any one of 82°C, 85°C, 88°C, 90°C, 93°C or a range between any two of them.
[0036] Preferably, in step (a), the total reaction time is 20 to 40 min, including but not limited to any one of 25 min, 30 min, 35 min or a range between any two of them.
[0037] Preferably, in step (b), the volume of the flocculant solution is 0.1% to 0.3% of the volume of the supernatant; including but not limited to any one of 0.13%, 0.15%, 0.18%, 0.2%, 0.23%, 0.25%, 0.28% or a range between any two of them.
[0038] Preferably, in step (b), the mass fraction of the flocculant solution is 0.05% to 0.15%, including but not limited to any one of 0.06%, 0.08%, 0.1%, 0.12%, 0.14% or a range between any two of them.
[0039] Preferably, in step (b), the flocculation sedimentation time is 3 to 5 hours, including but not limited to any one of 3.5 hours, 4 hours, and 4.5 hours, or a range between any two of them.
[0040] In some specific embodiments of the present invention, the flocculant includes polyacrylamide and / or modified polyacrylamide.
[0041] Polyacrylamide is a linear high molecular polymer. It is a hard glassy solid at room temperature. Its products include glue, latex, white powder, translucent beads and flakes. It has good thermal stability. It can be dissolved in water in any proportion. The aqueous solution is a uniform and transparent liquid.
[0042] In some specific embodiments of the present invention, the solid-liquid separation method includes pressure filtration and / or belt filtration.
[0043] In some specific embodiments of the present invention, in step (b), the standing time is 10 to 30 minutes, and can also be 15 minutes, 20 minutes or 25 minutes.
[0044] The present invention also provides a device for preparing ferrous sulfate solution for iron oxide pigment, which is applicable to the method for preparing ferrous sulfate solution for iron oxide pigment as described above. Figure 1 As shown, it includes a reaction device, a flocculation sedimentation device, a first solid-liquid separation device and a ferrous sulfate solution storage device connected in sequence.
[0045] The reaction device is also connected to a second solid-liquid separation device.
[0046] The second solid-liquid separation device is also connected to an artificial rutile storage device.
[0047] Among them, the reaction device serves as a reaction container for the titanium dioxide by-product ferrous sulfate solution and the reduced ilmenite. After the reaction is completed, it is left to stand for a period of time to separate the supernatant. The flocculation and precipitation device serves as a container for flocculation and precipitation of the supernatant and the flocculant solution. After the flocculation and precipitation are completed, the mixed material enters the first solid-liquid separation device for solid-liquid separation to obtain the ferrous sulfate solution for the iron oxide pigment, which can be flowed into the ferrous sulfate solution storage device for storage.
[0048] At the same time, after the reaction of the titanium dioxide byproduct ferrous sulfate solution and the reduced ilmenite is completed, slag can be separated. Since the reduced ilmenite has a large density, it will settle to the bottom of the reaction device after standing for a period of time. Therefore, the supernatant in the reaction device can be extracted first, and then the remaining slag (the slag contains a part of liquid) can be discharged, that is, the separation of the supernatant and the slag is completed.
[0049] After obtaining the slag, the slag is subjected to solid-liquid separation to obtain artificial rutile (artificial rutile refers to a titanium-rich raw material produced by separating most of the iron components in ilmenite by chemical processing methods, which has the same composition and structural properties as natural rutile. It is a high-quality substitute for natural rutile and can be used to produce chloride-process titanium dioxide and titanium tetrachloride). The artificial rutile can be placed in the artificial rutile storage device.
[0050] Preferably, a first stirring device is also provided in the reaction device.
[0051] The first stirring device can evenly mix the titanium dioxide byproduct ferrous sulfate solution and the reduced ilmenite, thereby facilitating the full reaction.
[0052] Preferably, the top of the reaction device is provided with a feed inlet for titanium dioxide by-product ferrous sulfate, a water inlet and a feed inlet for reduced ilmenite.
[0053] Before the reaction, various raw materials are added into the reaction device, wherein titanium dioxide by-product ferrous sulfate is added through the titanium dioxide by-product ferrous sulfate inlet, and water is added through the water inlet. After the two substances are mixed, a titanium dioxide by-product ferrous sulfate solution is obtained; and reduced ilmenite is added through the reduced ilmenite inlet.
[0054] Preferably, a steam inlet is also provided at the top of the reaction device.
[0055] The steam inlet is used to introduce steam, thereby raising the temperature of the mixed material, thereby promoting the removal of aluminum ions and titanium acyl ions (TiO 2+ ) hydrolysis.
[0056] Preferably, the preparation device further comprises a flocculant solution inlet, and the flocculant solution inlet is arranged at the top of the flocculation and sedimentation device, and / or the flocculant solution inlet is arranged between the reaction device and the flocculation and sedimentation device.
[0057] The flocculant solution inlet is used for adding flocculant solution.
[0058] If the flocculant solution inlet is arranged between the reaction device and the flocculation sedimentation device, Figure 1As shown, the flocculant solution and the supernatant can be mixed evenly during the transportation process, which is beneficial to the subsequent flocculation and precipitation.
[0059] If the flocculant solution inlet is arranged at the top of the flocculation sedimentation device, a second stirring device may be arranged in the flocculation sedimentation device, such as Figure 2 as shown, so that the flocculant solution and the supernatant are mixed evenly.
[0060] Preferably, a drying device is further provided between the second solid-liquid separation device and the artificial rutile storage device.
[0061] The drying device is used for drying the artificial rutile.
[0062] Preferably, the bottom end of the second solid-liquid separation device is further provided with a liquid outlet, and the bottom end of the flocculation sedimentation device is further provided with a liquid inlet, and the liquid outlet is connected to the liquid inlet.
[0063] The liquid material obtained after solid-liquid separation in the second solid-liquid separation device can be transported to the flocculation sedimentation device to further recover the ferrous sulfate solution.
[0064] The present invention also provides an iron oxide pigment, which is mainly prepared from the ferrous sulfate solution prepared by the method for preparing the ferrous sulfate solution for the iron oxide pigment as described above, or the ferrous sulfate solution prepared by the device for preparing the ferrous sulfate solution for the iron oxide pigment as described above.
[0065] Compared with the prior art, the present invention has the following beneficial effects:
[0066] (1) The method for preparing ferrous sulfate solution for iron oxide pigment provided by the present invention comprises adding reduced ilmenite, wherein the iron in the ilmenite undergoes a substitution reaction with the hydrogen ions in the ferrous sulfate solution produced as a byproduct of titanium dioxide, thereby increasing the pH of the mixture and promoting the decomposition of aluminum ions and titanium acyl ions (TiO 2+ ) hydrolyzes, thereby removing titanium and aluminum impurities, thereby improving the color and performance of iron oxide pigments. In addition, using reduced ilmenite instead of sodium hydroxide to adjust pH can reduce alkali consumption and reduce costs.
[0067] (2) The method for preparing ferrous sulfate solution for iron oxide pigment provided by the present invention can remove iron from the reduced ilmenite while adjusting the pH value by reducing ilmenite to obtain artificial rutile, which is then used to produce downstream products. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0069] Figure 1 A schematic structural diagram of a device for preparing a ferrous sulfate solution for an iron oxide pigment provided by the present invention;
[0070] Figure 2 Another schematic structural diagram of the device for preparing ferrous sulfate solution for iron oxide pigment provided by the present invention. DETAILED DESCRIPTION
[0071] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0072] The ferrous sulfate produced as a by-product of titanium dioxide in the following embodiments and comparative examples of the present invention is a by-product of the process of producing titanium dioxide pigment by the sulfuric acid method - ferrous sulfate heptahydrate crystals.
[0073] Figure 1 A schematic structural diagram of a device for preparing a ferrous sulfate solution for an iron oxide pigment provided by the present invention; Figure 2 Another schematic structural diagram of the device for preparing ferrous sulfate solution for iron oxide pigment provided by the present invention.
[0074] Example 1
[0075] The preparation device of ferrous sulfate solution for iron oxide pigment provided in this embodiment is as follows Figure 1 As shown, it includes a reaction device, a flocculation sedimentation device, a first solid-liquid separation device and a ferrous sulfate solution storage device which are connected in sequence.
[0076] The reaction device is also connected to a second solid-liquid separation device; the second solid-liquid separation device is also connected to an artificial rutile storage device.
[0077] The preparation device also includes a flocculant solution inlet, and the flocculant solution inlet is arranged between the reaction device and the flocculation sedimentation device.
[0078] A drying device is also provided between the second solid-liquid separation device and the artificial rutile storage device.
[0079] The reaction device is also provided with a first stirring device; the top of the reaction device is provided with a titanium dioxide by-product ferrous sulfate inlet, a water inlet and a reduced ilmenite inlet; the top of the reaction device is also provided with a steam inlet.
[0080] The bottom end of the second solid-liquid separation device is also provided with a liquid outlet, and the bottom end of the flocculation sedimentation device is also provided with a liquid inlet, and the liquid outlet is connected to the liquid inlet.
[0081] Example 2
[0082] This embodiment adopts the preparation device of Example 1 to prepare the ferrous sulfate solution for iron oxide pigment. The preparation method of the ferrous sulfate solution for iron oxide pigment provided in this embodiment specifically includes the following steps:
[0083] (1) adding titanium dioxide by-product ferrous sulfate and water into a reaction device, turning on a first stirring device for stirring, and obtaining a titanium dioxide by-product ferrous sulfate solution having a mass fraction of 6% of iron and a pH of 1; then introducing steam into the reaction device to raise the temperature to 80° C. (and maintaining the temperature at 80° C. during the replacement reaction and the hydrolysis reaction), and then adding reduced ilmenite into the reaction device so that the molar ratio of the iron element in the reduced ilmenite to the hydrogen ion in the titanium dioxide by-product ferrous sulfate solution is 1.1:2, and performing a replacement reaction and a hydrolysis reaction. After reacting for 40 minutes, stopping stirring and standing for 10 minutes;
[0084] (2) separating the mixed material after standing in step (1), first extracting the supernatant and pumping it into a flocculation sedimentation device, then discharging the remaining residue (containing a portion of liquid in the residue) into a second solid-liquid separation device (belt filter) for washing and solid-liquid separation, and then conveying the liquid material after solid-liquid separation into a flocculation sedimentation device, and adding a flocculant (polyacrylamide) with a mass fraction of 0.05% and a volume of 0.1% of the supernatant volume thereto for flocculation sedimentation, and conveying the supernatant to the first solid-liquid separation device (filter press) for filter pressing after 5 hours, and then pumping it into a ferrous sulfate solution storage device to obtain a ferrous sulfate solution for iron oxide pigment after impurities removal;
[0085] (3) The solid material obtained after solid-liquid separation by the second solid-liquid separation device (belt filter) in step (2) is transported to a drying device (rotary kiln) for drying, and then transported to an artificial rutile storage device to obtain artificial rutile.
[0086] Example 3
[0087] The preparation method of the ferrous sulfate solution for iron oxide pigment provided in this embodiment is basically the same as that in Example 2, except that:
[0088] In step (1), the molar ratio of the iron element in the reduced ilmenite to the hydrogen ions in the titanium dioxide by-product ferrous sulfate solution is 1.5:2; the mass fraction of the iron element in the titanium dioxide by-product ferrous sulfate solution is 8%, and the pH is 0.5;
[0089] In step (2), the mass fraction of the added flocculant is 0.15%, and the volume is 0.3% of the volume of the supernatant; the flocculation precipitation time is 3 hours.
[0090] Example 4
[0091] The preparation method of the ferrous sulfate solution for iron oxide pigment provided in this embodiment is basically the same as that in Example 2, except that:
[0092] In step (1), the molar ratio of the iron element in the reduced ilmenite to the hydrogen ions in the titanium dioxide by-product ferrous sulfate solution is 1.2:2; the mass fraction of the iron element in the titanium dioxide by-product ferrous sulfate solution is 7%, and the pH is 0.8; the temperature of the replacement reaction and the hydrolysis reaction is 85°C, and the reaction time is 30 minutes.
[0093] In step (2), the mass fraction of the added flocculant is 0.1%, and its volume is 0.2% of the volume of the supernatant; the flocculation precipitation time is 4 hours.
[0094] Comparative Example 1
[0095] The preparation method of the ferrous sulfate solution for iron oxide pigment provided in this comparative example is basically the same as that in Example 2, except that: in step (1), the reduced ilmenite is replaced by a 3% by mass sodium hydroxide solution, and the amount added is enough to maintain the same pH value as that of the mixed material in Example 2, and the titanium dioxide by-product ferrous sulfate used in this comparative example is the same batch as that in Example 2.
[0096] Experimental Example 1
[0097] The iron oxide pigments prepared in Example 2, Example 3, Example 4 and Comparative Example 1 were analyzed for element content (aluminum and titanium) using ferrous sulfate solution and titanium dioxide byproduct ferrous sulfate solution before the reaction. The results are shown in Table 1 below.
[0098] Table 1 Contents of aluminum and titanium in each group of solutions
[0099]
[0100]
[0101] As can be seen from Table 1, the use of reduced ilmenite to adjust the pH of the ferrous sulfate solution can reduce the content of aluminum to below 20ppm and the content of titanium to below 10ppm. The effect of removing impurities in Example 2 is not much different from the result of adjusting the pH with sodium hydroxide (i.e., Comparative Example 1), that is, reduced ilmenite can replace the traditional sodium hydroxide to adjust the pH so that most of the titanyl ions and aluminum ions in the ferrous sulfate solution complete the hydrolysis reaction. Therefore, the use of reduced ilmenite instead of traditional sodium hydroxide can reduce alkali consumption and reduce costs; at the same time, it can remove titanium and aluminum impurities.
[0102] At the same time, the main components of the artificial rutile prepared in Example 2, Example 3 and Example 4 were analyzed, and the results are shown in Table 2 below.
[0103] Table 2 Main composition of artificial rutile
[0104]
[0105] It can be seen from the data in Table 2 that by reducing ilmenite to adjust the pH, an artificial rutile product that meets the requirements can be obtained.
[0106] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A method for preparing ferrous sulfate solution for iron oxide pigments, characterized in that: The steps include: (a) mixing the titanium dioxide by-product ferrous sulfate solution with the reduced ilmenite, so that the iron in the reduced ilmenite undergoes a replacement reaction with the hydrogen ions in the ferrous sulfate solution, and the titanyl ions and aluminum ions in the ferrous sulfate solution undergo a hydrolysis reaction; (b), after the replacement reaction and the hydrolysis reaction are completed, the mixed material is allowed to stand and separated to obtain a supernatant and a slag respectively, the supernatant is mixed with a flocculant solution for flocculation precipitation, and then after solid-liquid separation, the ferrous sulfate solution for the iron oxide pigment is obtained, and the slag is subjected to solid-liquid separation to obtain artificial rutile; Wherein, the titanium dioxide by-product ferrous sulfate solution is obtained by dissolving ferrous sulfate heptahydrate crystals, a by-product of the production of titanium dioxide pigment by sulfuric acid method; The cations in the titanium dioxide byproduct ferrous sulfate solution include titanyl ions, aluminum ions, ferrous ions and hydrogen ions.
2. The preparation method according to claim 1, characterized in that: In step (a), the molar ratio of the iron element in the reduced ilmenite to the hydrogen ions in the titanium dioxide by-product ferrous sulfate solution is 1.1-1.5:
2.
3. The preparation method according to claim 1, characterized in that: In step (a), the mass fraction of iron in the titanium dioxide by-product ferrous sulfate solution is 6% to 8%.
4. The preparation method according to claim 1, characterized in that: In step (a), the pH value of the titanium dioxide by-product ferrous sulfate solution is 0-1.
5.
5. The preparation method according to claim 1, characterized in that: In step (a), the temperature of the mixed material is 80-95°C.
6. The preparation method according to claim 1, characterized in that: In step (a), the total reaction time is 20 to 40 minutes.
7. The preparation method according to claim 1, characterized in that: In step (b), the volume of the flocculant solution is 0.1% to 0.3% of the volume of the supernatant.
8. The preparation method according to claim 1, characterized in that: In step (b), the mass fraction of the flocculant solution is 0.05% to 0.15%.
9. The preparation method according to claim 1, characterized in that: In step (b), the flocculation sedimentation time is 3 to 5 hours.
10. A device for preparing ferrous sulfate solution for iron oxide pigment, characterized in that: The method for preparing the ferrous sulfate solution for iron oxide pigment according to any one of claims 1 to 9, wherein the preparation device comprises a reaction device, a flocculation precipitation device, a first solid-liquid separation device and a ferrous sulfate solution storage device connected in sequence; The reaction device is also connected to a second solid-liquid separation device; The second solid-liquid separation device is also connected to an artificial rutile storage device.
11. The preparation device according to claim 10, characterized in that: The reaction device is also provided with a first stirring device.
12. The preparation device according to claim 10, characterized in that: The top of the reaction device is provided with a titanium dioxide byproduct ferrous sulfate inlet, a water inlet and a reduced ilmenite inlet.
13. The preparation device according to claim 10, characterized in that: The top of the reaction device is also provided with a steam inlet.
14. The preparation device according to claim 10, characterized in that: The preparation device further comprises a flocculant solution inlet, which is arranged at the top of the flocculation and precipitation device, and / or the flocculant solution inlet is arranged between the reaction device and the flocculation and precipitation device.
15. The preparation device according to claim 10, characterized in that: A drying device is also provided between the second solid-liquid separation device and the artificial rutile storage device.
16. The preparation device according to claim 10, characterized in that: The bottom end of the second solid-liquid separation device is also provided with a liquid outlet, and the bottom end of the flocculation sedimentation device is also provided with a liquid inlet, and the liquid outlet is connected to the liquid inlet.