Ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material and preparation method

By using chemical coating method to form a "core shell" structure in ceramic capacitor dielectric materials, the problem of unstable performance of ceramic capacitors in high temperature environments is solved, and the ultra-wide temperature stability and high dielectric constant of ceramic dielectric materials are achieved. Meets the use temperature requirements of above 200℃.

CN114255986BActive Publication Date: 2024-11-15HEFEI QINGCI TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210014728.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-07
Publication Date
2024-11-15
Estimated Expiration
2042-01-07

AI Technical Summary

Technical Problem

The existing ceramic capacitors have unstable performance in high temperature environments and cannot meet the temperature requirements of above 200℃. Especially in applications such as aerospace, automobiles and deep well oil drilling, there is a problem of insufficient temperature stability.

Method used

SiO2 was precipitated on the surface of (Bi0.5Na0.5)TiO3, SrZrO3 and NaNbO3 particles by chemical coating to form a "core shell" structure, and (1-x)(0.95(Bi0.5Na0.5)TiO3@Si- 0.05SrZrO3@Si)-xNaNbO3@Si, the temperature stability and dielectric constant of the material are improved by this method.

Benefits of technology

The ultra-wide temperature range stability and high dielectric constant of ceramic dielectric materials are achieved, the temperature change rate is less than ±15%, and the dielectric constant remains stable at high temperatures, meeting the operating temperature requirements of above 200℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114255986B_ABST
    Figure CN114255986B_ABST
Patent Text Reader

Abstract

The present invention discloses a multiphase coating preparation method for a high dielectric constant ceramic capacitor dielectric material with ultra-wide temperature stability. The general chemical formula is: (1-x)(0.95(Bi 0.5 Na 0.5 )TiO3@Si‑0.05SrZrO3@Si)‑xNaNbO3@Si; the value of x satisfies the following conditions: 0.1≤x≤0.4, @ indicates coating; first, according to the stoichiometric ratio, Bi2O3, Na2CO3, and TiO2 are used to synthesize (Bi 0.5 Na 0.5 )TiO3, SrZrO3 was synthesized by SrCO3 and ZrO2, NaNbO3 was synthesized by Na2CO3 and Nb2O5, and then (Bi 0.5 Na 0.5 ) A layer of SiO2 is deposited on the surface of TiO3, SrZrO3 and NaNbO3 particles to form a "core-shell" structure. After calcination, (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders are prepared by batching, spheroidal graphite, drying, granulation, molding, and sintering according to the general chemical formula. The process is simple, low cost, lead-free and environmentally friendly, and has stability in an ultra-wide temperature range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a capacitor dielectric material and a preparation method thereof, and in particular to an ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material and a preparation method thereof which are suitable for use in the field of ceramic dielectric materials. Background Art

[0002] As an important passive component, ceramic capacitors have the properties of high capacitance, small size, low cost, high reliability and excellent high-frequency characteristics, and are widely used in instrumentation, communication, aerospace and other fields. At present, the standard of ceramic capacitors with the widest operating temperature range specified by the International Electronics Industry Association is X9R (with a capacitance change rate of less than ±15% within the range of -55 to 200°C). However, with the rapid development of aviation, deep well oil drilling, natural gas exploration and the automotive industry, there are more stringent requirements for the use temperature of electronic components. The use temperature of some key parts reaches above 200°C. For example, in the automotive industry, the temperature of the engine compartment may be higher than 140°C, and the anti-lock braking system needs to withstand high temperatures in the range of 150-250°C. In addition, the operating temperature of cylinder pressure sensors is as high as 300°C. In the aerospace industry, in order to reduce the complexity of interconnection and reduce the weight of the aircraft, the engine monitoring system is designed as a distributed control solution, and many electrical equipment must be installed near the engine, and the temperature is usually 200-300°C. In deep oil drilling, the operating temperature is usually over 200°C, and in deeper exploration, the operation of drilling equipment requires electronic components to have higher temperature stability. Therefore, it is crucial to develop dielectric materials that can operate at ultra-wide temperature stability above 200°C or even above 300°C. Summary of the invention

[0003] In view of the shortcomings of the prior art, an ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material and a preparation method are provided, which have simple preparation process, low material cost, no pollution, and the prepared ceramic dielectric material has stability in an ultra-wide temperature range.

[0004] In order to achieve the above technical objectives, the present invention provides an ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material, the chemical formula of which is:

[0005] (1-x)(0.95(Bi 0.5 Na 0.5 )TiO3@Si-0.05SrZrO3@Si)-xNaNbO3@Si;

[0006] The value of x satisfies the following conditions: 0.1≤x≤0.4, and @ indicates coating.

[0007] A method for preparing a wide temperature stable, high dielectric constant ceramic capacitor dielectric material, firstly using Bi2O3, Na2CO3, TiO2 to synthesize (Bi 0.5 Na 0.5 )TiO3, SrZrO3 was synthesized by SrCO3 and ZrO2, NaNbO3 was synthesized by Na2CO3 and Nb2O5, and then (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are deposited with a layer of SiO2 on their surfaces, thus forming a "core-shell" structure. 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles were calcined to obtain (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders are finally prepared by batching, spheroidal graphite, drying, granulation, molding and sintering according to the general chemical formula.

[0008] The specific steps include:

[0009] aFirst, synthesize (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3: According to the chemical formula (Bi 0.5 Na 0.5 )TiO3 weighs Bi2O3, Na2CO3, TiO2; according to the chemical formula SrZrO3 weighs SrCO3, ZrO2; according to the chemical formula NaNbO3 weighs Na2CO3, Nb2O5;

[0010] b will prepare (Bi 0.5 Na 0.5 ) Bi2O3, Na2CO3, TiO2 for preparing SrZrO3, SrCO3, ZrO2 for preparing SrZrO3, Na2CO3, Nb2O5 for preparing NaNbO3 are prepared according to the parameter ratio and then added with anhydrous ethanol respectively, and ZrO2 balls are used as the medium, and the ball milling is carried out for 4 hours by a planetary ball mill, and the ball milling slurry is dried at 80°C, and the dried powder is put into a calcining furnace and calcined;

[0011] c The calcined powder was added with anhydrous ethanol and ball-milled for 4 hours to be fully dispersed, and the dispersed slurry was transferred to a mechanical stirring container; according to the mass of Si element required by the doping modification formula, the corresponding mass of tetraethyl orthosilicate was weighed, and appropriate amounts of acetic acid, ethanol and water were added in sequence to prepare a tetraethyl orthosilicate organic solution, and the tetraethyl orthosilicate organic solution was added to the slurry, and then the diluted ammonia solution was slowly added to the slurry, and the pH of the slurry was adjusted to 7.6-9.3, and the slurry was stirred and aged for 1 hour to make Si 4+ Hydrolyzed and precipitated in the form of SiO2 0.5 Na 0.5 ) the surface of TiO3, SrZrO3 and NaNbO3 particles, thereby obtaining particles with a "core-shell" structure;

[0012] d The SiO2-coated (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are placed in an oven and dried at 80°C to obtain powders, which are then calcined to make (Bi 0.5 Na 0.5 )The SiO2 coating layer on the surface of TiO3, SrZrO3 and NaNbO3 powders is more fully crystallized, and (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders;

[0013] e According to the chemical formula (1-x)(0.95(Bi 0.5 Na 0.5 )TiO3@Si-0.05SrZrO3@Si)-xNaNbO3@Si weighing (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders are prepared, and the value range of x is: 0.1≤x≤0.4;

[0014] f. Add anhydrous ethanol to the powder after mixing and evenly mix it by ball milling. Then, dry the mixed slurry at 80°C, add the prepared polyvinyl alcohol adhesive to granulate it, and use a mold to press it into a green disc;

[0015] g. After debinding the pressed green disc at 600°C for 3 hours, high-temperature sintering is performed to obtain an ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material;

[0016] h Silver paste is evenly coated on the upper and lower surfaces of the disc obtained after high-temperature sintering, and the electrode is prepared by sintering at 600°C for 30 minutes for subsequent dielectric performance testing.

[0017] Furthermore, in step b, the optimal calcination conditions for the dried Bi2O3, Na2CO3, TiO2 mixed powder, SrCO3, ZrO2 mixed powder and Na2CO3, Nb2O5 mixed powder are calcination at 850°C for 5 hours, calcination at 1020°C for 3 hours and calcination at 850°C for 5 hours, respectively.

[0018] Furthermore, in step c, the mass fraction of coated SiO2 is 0.2% to 2%.

[0019] Furthermore, the calcination temperature of the powder after drying in step d is 500-700° C., and the calcination time is 1-3 hours.

[0020] Furthermore, the high-temperature sintering in step g can be carried out in one-stage sintering or two-stage sintering: the sintering temperature of the one-stage sintering is 1100-1250°C, and the temperature is kept at this temperature for 1-3 hours; in the two-stage sintering, the temperature of the first stage sintering is set to 1150-1300°C, and the heating rate is 4°C / min-60°C / min. After keeping the temperature for 1-10 minutes, the temperature is rapidly reduced to the second stage sintering temperature, 1000-1100°C, and the temperature is kept at this temperature for 3-10 hours, and then cooled to room temperature with the furnace.

[0021] Beneficial effects: The ceramic dielectric material disclosed in the present invention has excellent temperature stability, a wide operating range, a high dielectric constant, and a small capacitance-temperature change rate: when x=0.2, within the temperature range of -60 to 541°C, the capacitance-temperature change rate is less than ±15%, and the dielectric constant is 1150; when x=0.3, within the temperature range of -70 to 443°C, the capacitance-temperature change rate is less than ±5%, and the dielectric constant is 885.

[0022] The present invention uses a chemical coating method to (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 are three different phase ceramic materials. The coated SiO2 layer can inhibit the diffusion of elements during the sintering process, thereby ensuring that the ceramic sample after sintering still maintains the characteristics of multi-phase coexistence. Due to the synergistic effect of the multi-phase, the dielectric peak is broadened to ensure temperature stability. At the same time, (Bi 0.5 Na 0.5 )TiO3 has a high Curie temperature, which can increase the upper limit of the operating temperature of the composite ceramic. The coated SiO2 layer can further stabilize the temperature characteristics of the ceramic, thereby obtaining an ultra-wide temperature-stable ceramic capacitor dielectric material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the morphology of the ceramic powder obtained in Example 3 of the present invention when x=0.3 under transmission electron microscope observation:

[0024] Figure 2The dielectric temperature spectrum of the ceramic dielectric material obtained in Example 1 of the present invention when x=0.2 is tested in the temperature range of -100 to 550°C;

[0025] Figure 3 It is a dielectric temperature spectrum obtained by testing the ceramic dielectric material in the temperature range of -100 to 450° C. when x=0.25 obtained in Example 2 of the present invention;

[0026] Figure 4 This is the dielectric temperature spectrum of the ceramic dielectric material obtained in Example 3 of the present invention when x=0.3 and tested within the temperature range of -100 to 500°C. DETAILED DESCRIPTION

[0027] The embodiments of the present invention are further described below in conjunction with the accompanying drawings:

[0028] The ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material of the present invention has a general chemical formula of:

[0029] (1-x)(0.95(Bi 0.5 Na 0.5 )TiO3@Si-0.05SrZrO3@Si)-xNaNbO3@Si;

[0030] The value of x satisfies the following conditions: 0.1≤x≤0.4, and @ indicates coating.

[0031] A method for preparing a wide temperature stable, high dielectric constant ceramic capacitor dielectric material, firstly using Bi2O3, Na2CO3, TiO2 to synthesize (Bi 0.5 Na 0.5 )TiO3, SrZrO3 was synthesized by SrCO3 and ZrO2, NaNbO3 was synthesized by Na2CO3 and Nb2O5, and then (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are deposited with a layer of SiO2 on their surfaces, thus forming a "core-shell" structure. 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles were calcined to obtain (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders are finally prepared by batching, spheroidal graphite, drying, granulation, molding and sintering according to the general chemical formula.

[0032] The specific steps include:

[0033] aFirst, prepare the synthesis (Bi0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3: According to the chemical formula (Bi 0.5 Na 0.5 )TiO3 weighs Bi2O3, Na2CO3, TiO2; according to the chemical formula SrZrO3 weighs SrCO3, ZrO2; according to the chemical formula NaNbO3 weighs Na2CO3, Nb2O5;

[0034] b will prepare (Bi 0.5 Na 0.5 ) Bi2O3, Na2CO3, TiO2 powders for preparing SrZrO3, SrCO3, ZrO2 powders for preparing SrZrO3, Na2CO3, Nb2O5 powders for preparing NaNbO3 are prepared according to the parameter ratio and then added with anhydrous ethanol respectively, and ZrO2 balls are used as the medium, and a planetary ball mill is used for ball milling for 4 hours, and the ball milling slurry is dried at 80°C, and the dried powder is placed in a calcining furnace and calcined. The best calcination systems are calcining at 850°C for 5 hours, calcining at 1020°C for 3 hours and calcining at 850°C for 5 hours respectively;

[0035] c The calcined powder was added with anhydrous ethanol and ball-milled for 4 hours to be fully dispersed, and the dispersed slurry was transferred to a mechanical stirring container; according to the mass of Si element required by the doping modification formula, the corresponding mass of tetraethyl orthosilicate was weighed, and appropriate amounts of acetic acid, ethanol and water were added in sequence to prepare a tetraethyl orthosilicate organic solution, and the tetraethyl orthosilicate organic solution was added to the slurry, and then the diluted ammonia solution was slowly added to the slurry, and the pH of the slurry was adjusted to 7.6-9.3, and the slurry was stirred and aged for 1 hour to make Si 4+ Hydrolyzed and precipitated in the form of SiO2 0.5 Na 0.5 ) the surface of TiO3, SrZrO3 and NaNbO3 particles, thereby obtaining particles with a "core-shell" structure, and the mass fraction of coated SiO2 is 0.2% to 2%;

[0036] d The SiO2-coated (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are placed in an oven and dried at 80°C to obtain powders, which are then calcined at a temperature of 500 to 700°C for 1 to 3 hours to obtain (Bi 0.5 Na 0.5 )The SiO2 coating layer on the surface of TiO3, SrZrO3 and NaNbO3 powders is more fully crystallized, and (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders;

[0037] e According to the chemical formula (1-x)(0.95(Bi 0.5 Na 0.5 )TiO3@Si-0.05SrZrO3@Si)-xNaNbO3@Si weighing (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders are prepared, and the value range of x is: 0.1≤x≤0.4;

[0038] f. Add anhydrous ethanol to the powder after mixing and evenly mix it by ball milling. Then, dry the mixed slurry at 80°C, add the prepared polyvinyl alcohol adhesive to granulate it, and use a mold to press it into a green disc;

[0039] g After debinding the pressed green disc at 600°C for 3 hours, high-temperature sintering is performed to obtain an ultra-wide temperature-stable, high-dielectric-constant ceramic capacitor dielectric material; high-temperature sintering can be performed in one-stage sintering or two-stage sintering: the sintering temperature of the one-stage sintering is 1100-1250°C, and the temperature is kept for 1-3 hours; in the two-stage sintering, the temperature of the first stage sintering is set at 1150-1300°C, the heating rate is 4°C / min-60°C / min, and after keeping the temperature for 1-10 minutes, the temperature is rapidly reduced to the second stage sintering temperature, 1000-1100°C, and the temperature is kept for 3-10 hours, and then cooled to room temperature with the furnace.

[0040] h Silver paste is evenly coated on the upper and lower surfaces of the disc obtained after high-temperature sintering, and the electrode is prepared by sintering at 600°C for 30 minutes for subsequent dielectric performance testing.

[0041] Embodiment 1:

[0042] Step 1: According to the chemical formula (Bi 0.5 Na 0.5 )TiO3 weighs Bi2O3, Na2CO3, TiO2; according to the chemical formula SrZrO3 weighs SrCO3, ZrO2; according to the chemical formula NaNbO3 weighs Na2CO3, Nb2O5;

[0043] Step 2: Add the raw material powders into anhydrous ethanol respectively, use ZrO2 balls as the medium, and use a planetary ball mill for ball milling for 4 hours. The ball milled slurry is dried at 80°C, and the dried Bi2O3, Na2CO3, and TiO2 mixed powders are calcined at 850°C for 5 hours; SrCO3 and ZrO2 mixed powders are calcined at 1020°C for 3 hours; Na2CO3 and Nb2O5 mixed powders are calcined at 850°C for 5 hours and set aside.

[0044] Step 3: After calcination, add anhydrous ethanol to the powder for secondary ball milling for 4 hours. Transfer the dispersed powder to a mechanical stirring container, add Si(C2H5O4)4, and adjust the pH value of the solution to 7.6 by dropping ammonia water. 4+ Hydrolyzed and precipitated in the form of SiO2 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are coated on the surface to form a "core-shell" structure. The mass fraction of coated SiO2 is 0.4%. The coated powder is placed in an oven and dried at 80°C. The dried powder is calcined again to obtain (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders, set aside.

[0045] Step 4: Weigh according to the stoichiometric ratio of x = 0.2 (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, and NaNbO3@Si powders are prepared.

[0046] Step 5: Add the raw materials to anhydrous ethanol and mix them evenly by ball milling. The slurry is dried at 80° C., and the prepared polyvinyl alcohol adhesive is added to granulate the slurry. The slurry is then pressed into green discs using a mold.

[0047] Step 6: After debinding for 3 hours at 600°C, the pressed green disc is subjected to high-temperature sintering. The sintering system is as follows: the temperature of the first stage sintering is set at 1240°C, the heating rate is 4°C / min, and after keeping warm for 1 minute, it is quickly reduced to the second stage sintering temperature, 1090°C, and kept warm at this temperature for 5 hours, and then cooled to room temperature with the furnace.

[0048] Step 7: Silver paste is uniformly coated on the upper and lower surfaces of the prepared disc sample, and electrodes are prepared by sintering at 600°C, and electrical performance tests are performed. Figure 2 shown.

[0049] Embodiment 2:

[0050] Step 1: According to the chemical formula (Bi 0.5 Na 0.5 )TiO3 weighs Bi2O3, Na2CO3, TiO2; according to the chemical formula SrZrO3 weighs SrCO3, ZrO2; according to the chemical formula NaNbO3 weighs Na2CO3, Nb2O5;

[0051] Step 2: Add the raw material powders into anhydrous ethanol respectively, use ZrO2 balls as the medium, and use a planetary ball mill for ball milling for 4 hours. The ball milled slurry is dried at 80°C, and the dried Bi2O3, Na2CO3, and TiO2 mixed powders are calcined at 850°C for 5 hours; SrCO3, ZrO2 mixed powders are calcined at 1020°C for 3 hours; Na2CO3, Nb2O5 mixed powders are calcined at 850°C for 5 hours and set aside.

[0052] Step 3: After calcination, add anhydrous ethanol to the powder for secondary ball milling for 4 hours. Transfer the dispersed powder to a mechanical stirring container, add Si(C2H5O4)4, and adjust the pH value of the solution to 7.6 by dropping ammonia water. 4+ Hydrolyzed and precipitated in the form of SiO2 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are coated on the surface to form a "core-shell" structure. The mass fraction of coated SiO2 is 0.4%. The coated powder is placed in an oven and dried at 120°C. The dried powder is calcined again to obtain (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders, set aside.

[0053] Step 4: Weigh according to the stoichiometric ratio of x = 0.25 (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, and NaNbO3@Si powders are prepared.

[0054] Step 5: Add the raw materials to anhydrous ethanol and mix them evenly by ball milling. The slurry is dried at 80° C., and the prepared polyvinyl alcohol adhesive is added to granulate the slurry. The slurry is then pressed into green discs using a mold.

[0055] Step 6: After debinding for 3 hours at 600°C, the pressed green disc is subjected to high-temperature sintering. The sintering system is as follows: the temperature of the first stage sintering is set at 1240°C, the heating rate is 4°C / min, and after keeping warm for 1 minute, it is quickly reduced to the second stage sintering temperature, 1090°C, and kept warm at this temperature for 5 hours, and then cooled to room temperature with the furnace.

[0056] Step 7: Silver paste is uniformly coated on the upper and lower surfaces of the prepared disc sample, and electrodes are prepared by sintering at 600°C, and electrical performance tests are performed. Figure 3 shown.

[0057] Embodiment 3:

[0058] Step 1: According to the chemical formula (Bi 0.5 Na 0.5)TiO3 weighs Bi2O3, Na2CO3, TiO2; according to the chemical formula SrZrO3 weighs SrCO3, ZrO2; according to the chemical formula NaNbO3 weighs Na2CO3, Nb2O5;

[0059] Step 2: Add the raw material powders into anhydrous ethanol respectively, use ZrO2 balls as the medium, and use a planetary ball mill for ball milling for 4 hours. The ball milled slurry is dried at 80°C, and the dried Bi2O3, Na2CO3, and TiO2 mixed powders are calcined at 850°C for 5 hours; SrCO3, ZrO2 mixed powders are calcined at 1020°C for 3 hours; Na2CO3, Nb2O5 mixed powders are calcined at 850°C for 5 hours and set aside.

[0060] Step 3: After calcination, add anhydrous ethanol to the powder for secondary ball milling for 4 hours. Transfer the dispersed powder to a mechanical stirring container, add Si(C2H5O4)4, and adjust the pH value of the solution to 7.6 by dropping ammonia water. 4+ Hydrolyzed and precipitated in the form of SiO2 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are coated on the surface to form a "core-shell" structure. The mass fraction of coated SiO2 is 0.4%. The coated powder is placed in an oven and dried at 120°C. The dried powder is calcined again to obtain (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders, set aside.

[0061] Step 4: Weigh according to the stoichiometric ratio of x = 0.3 (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, and NaNbO3@Si powders are prepared.

[0062] Step 5: Add the raw materials to anhydrous ethanol and mix them evenly by ball milling. The slurry is dried at 80° C., and the prepared polyvinyl alcohol adhesive is added to granulate the slurry. The slurry is then pressed into green discs using a mold.

[0063] Step 6: After debinding for 3 hours at 600°C, the pressed green disc is subjected to high-temperature sintering. The sintering system is as follows: the temperature of the first stage sintering is set at 1240°C, the heating rate is 4°C / min, and after keeping warm for 1 minute, it is quickly reduced to the second stage sintering temperature, 1090°C, and kept warm at this temperature for 5 hours, and then cooled to room temperature with the furnace.

[0064] Step 7: Silver paste is uniformly coated on the upper and lower surfaces of the prepared disc sample, and electrodes are prepared by sintering at 600°C, and electrical performance tests are performed. Figure 4 shown.

[0065] The morphology of the ceramic powder obtained in Example 3 when x=0.3 under transmission electron microscope observation is shown in FIG. Figure 1 As shown in the figure, (a) shows the microscopic morphology of the powder after coating, where BNT represents Bi 1 / 2 Na 1 / 2 TiO3, NN represents NaNbO3, SZ represents SrZrO3; (b) and (c) are the microscopic morphologies of the coating layer partially enlarged in (a).

[0066] The main dielectric performance parameters of the specific embodiment are shown in Table 1.

[0067] Table 1

[0068]

[0069] Note: Δε is the deviation of the dielectric constant at different temperatures from the room temperature dielectric constant.

Claims

1. An ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material, characterized in that The general chemical formula of the material is: (1−x)(0.95(By 0.5 And 0.5 )TiO3@Si-0.05SrZrO3@Si)-xNaNbO3@Si: The value of x satisfies the following conditions: 0.1≤x≤0.4, @ indicates coating; The preparation method of a wide temperature stable, high dielectric constant ceramic capacitor dielectric material comprises the following steps: firstly, Bi2O3, Na2CO3, and TiO2 are used to synthesize (Bi 0.5 Na 0.5 )TiO3, SrZrO3 was synthesized by SrCO3 and ZrO2, NaNbO3 was synthesized by Na2CO3 and Nb2O5, and then (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are deposited with a layer of SiO2 on their surfaces, thus forming a "core-shell" structure. 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles were calcined to obtain (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders, and finally preparing the powders by batching, spheroidal graphite, drying, granulation, molding, and sintering according to the general chemical formula; The specific steps are as follows: aFirst, synthesize (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3: According to the chemical formula (Bi 0.5 Na 0.5 )TiO3 weighs Bi2O3, Na2CO3, TiO2; according to the chemical formula SrZrO3 weighs SrCO3, ZrO2; according to the chemical formula NaNbO3 weighs Na2CO3, Nb2O5; b will prepare (Bi 0.5 Na 0.5 ) Bi2O3, Na2CO3, TiO2 for preparing TiO3; SrCO3, ZrO2 for preparing SrZrO3; Na2CO3, Nb2O5 for preparing NaNbO3 are prepared by adding anhydrous ethanol according to the parameter ratio, using ZrO2 balls as the medium, using a planetary ball mill for 4 hours, mixing evenly, drying the ball milled slurry at 80°C, and placing the dried powder into a calcining furnace for calcining; c The calcined powder was added with anhydrous ethanol and ball-milled for 4 hours to be fully dispersed. The dispersed slurry was transferred to a mechanical stirring container. According to the mass of Si element required by the doping modification formula, the corresponding mass of tetraethyl orthosilicate was weighed, and appropriate amounts of acetic acid, ethanol and water were added in sequence to prepare a tetraethyl orthosilicate organic solution. The tetraethyl orthosilicate organic solution was added to the slurry, and then the diluted ammonia solution was slowly added to the slurry. The pH of the slurry was adjusted to 7.6-9.3, and the slurry was stirred and aged for 1 hour to allow Si to 4+ Hydrolyzed and precipitated in the form of SiO2 0.5 Na 0.5 ) the surface of TiO3, SrZrO3 and NaNbO3 particles, thereby obtaining particles with a "core-shell" structure, with a mass fraction of SiO2 of 0.2% to 2%; d The SiO2-coated (Bi 0.5 Na 0.5 )TiO3, SrZrO3 and NaNbO3 particles are placed in an oven and dried at 80°C to obtain powders, which are then calcined to make (Bi 0.5 Na 0.5 )The SiO2 coating layer on the surface of TiO3, SrZrO3 and NaNbO3 powders is more fully crystallized, and (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders; e According to the chemical formula (1-x)(0.95(Bi 0.5 Na 0.5 )TiO3@Si-0.05SrZrO3@Si)-xNaNbO3@Si weighing (Bi 0.5 Na 0.5 )TiO3@Si, SrZrO3@Si, NaNbO3@Si powders are prepared, and the value range of x is: 0.1≤x≤0.4; f. Add anhydrous ethanol to the powder after mixing and evenly mix it by ball milling. Then, dry the mixed slurry at 80°C, add the prepared polyvinyl alcohol adhesive to granulate it, and use a mold to press it into a green disc; g. After debinding the pressed green disc at 600°C for 3 hours, high-temperature sintering is performed to obtain an ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material; h Silver paste is evenly coated on the upper and lower surfaces of the disc obtained after high-temperature sintering, and the electrode is prepared by sintering at 600°C for 30 minutes for subsequent dielectric performance testing.

2. The ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material according to claim 1, characterized in that: Step b: The optimal calcination conditions for the dried Bi2O3, Na2CO3, TiO2 mixed powder, SrCO3, ZrO2 mixed powder and Na2CO3, Nb2O5 mixed powder are calcined at 850°C for 5 hours, calcined at 1020°C for 3 hours and calcined at 850°C for 5 hours respectively.

3. The ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material according to claim 1, characterized in that: The calcination temperature of the powder after drying in step d is 500-700° C., and the calcination time is 1-3 hours.

4. The ultra-wide temperature stable, high dielectric constant ceramic capacitor dielectric material according to claim 1, characterized in that: The high temperature sintering in step g can be carried out by one-stage sintering or two-stage sintering: the sintering temperature of the one-stage sintering is 1100-1250°C, and the heat preservation time is 1-3 hours; In the two-stage sintering, the temperature of the first stage sintering is set at 1150~1300℃, the heating rate is 4℃ / min~60℃ / min, and after keeping warm for 1~10 minutes, it is quickly reduced to the second stage sintering temperature, 1000~1100℃, and kept warm at this temperature for 3~10 hours, and then cooled to room temperature with the furnace.