A high performance diamond composite sheet and its manufacturing process

By using a carbon-containing metal bonding agent under high temperature and high pressure, the problem of poor performance of diamond composite sheets is solved, and the impact resistance and wear resistance are significantly improved.

CN114260453BActive Publication Date: 2024-11-26XINYA COMPOSITE SUPER HARD MATERIAL CO LTD ZHENGZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111601706.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-24
Publication Date
2024-11-26
Estimated Expiration
2041-12-24

AI Technical Summary

Technical Problem

Due to the difference in density of metal bonding agent, the existing diamond composite sheets have poor uniformity of the mixture, which affects the sintering process, and fewer D-D bonds are generated, resulting in poor impact resistance and wear resistance.

Method used

Carbon-containing metal bonding agent is used to ensure that the carbon content of the bonding agent reaches saturation value in the molten state, and directly precipitates diamond, increase the formation of covalent bonds between diamond powders, and improve the performance of composite sheets.

Benefits of technology

The impact resistance and wear resistance of diamond composite sheets are significantly improved, and the wear resistance is increased by more than 15% and the impact resistance strength is increased by more than 10%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a high-performance diamond composite sheet and a manufacturing process thereof, and relates to the field of diamond. The high-performance diamond composite sheet, according to weight percentage, includes 80-99% of diamond micropowder with a particle size D50 of 0-50 μm, and the remainder is a binder with a particle size range D50 of 0-20 μm, wherein the binder is a mixture of carbon and metal, and the maximum value of the carbon content is the saturation value of the binder in a molten state, and a manufacturing process proposed according to a high-performance diamond composite sheet, including step 1: fully mixing the diamond micropowder and the binder; step 2: pre-placing tungsten carbide with a cobalt content of 8-20%, and then placing the mixture of the diamond micropowder and the binder in a mold for heating, pressurizing and sintering. Diamond composite sheets are synthesized using a carbon-containing metal melt binder. During the synthesis process, the carbon in the binder itself can be directly precipitated and converted into diamond, reducing the dissolution and re-precipitation process of the diamond micropowder, and the diamond composite sheet has high wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diamonds, in particular to a high-performance diamond composite sheet and a manufacturing process thereof. Background Art

[0002] Diamond composite sheets are mainly composed of cemented carbide, diamond powder, metal binder (catalyst) and other materials. By sintering under high temperature and high pressure, DD covalent bonds are formed between the diamond powders, thereby forming a superhard material sintered body. The role of the binder (catalyst) in the composite sheet is to dissolve and recrystallize the carbon source of the diamond powder, so that the diamond powders grow alternately together during the recrystallization process.

[0003] At present, the binders (catalysts) used in diamond composite sheets are mostly cobalt powder, nickel powder, iron powder and their alloy powders. Since the density of diamond is 3.5g / cm 3, The density of metal cobalt, nickel, iron and their alloys is about 7.8-8.9 g / cm 3 , the large density difference leads to poor uniformity of the mixture; during the high temperature and high pressure synthesis process, the metal binder (catalyst) must first dissolve the diamond powder and the contact part with it. When the carbon concentration of the metal solid solution reaches saturation relative to diamond, diamond is precipitated from the metal-carbon melt. Affected by the uniformity of the mixture, the gaps in some mixtures are large, and the external pressure cannot completely compact the mixture. The effective contact area between the diamond particles and the binder is small, resulting in insufficient precipitation of the binder after dissolving the powder, fewer DD bonds are generated, and the comprehensive performance of the diamond composite sheet such as impact resistance and wear resistance is poor. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a high-performance diamond composite sheet and a manufacturing process thereof, which solves the problem of poor performance of the diamond composite sheet.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: A manufacturing process of a high-performance diamond composite sheet, comprising the following steps:

[0008] (1) Mixing: Diamond powder and binder are fully mixed;

[0009] (2) Assembling: Assembling the cemented carbide substrate, the uniformly mixed diamond powder and the binder;

[0010] (3) Sintering: high temperature and high pressure sintering process is used to sinter and synthesize high performance new binder diamond composite sheet;

[0011] The binder is a metal material containing carbon, and the maximum value of the carbon content is the saturation value of the binder in a molten state.

[0012] Preferably, the metal in the binder is one or more of cobalt, nickel and iron.

[0013] Preferably, the carbon in the binder may be graphite, graphene, or amorphous carbon.

[0014] Preferably, the diamond powder and the binder are in the following weight percentages: 80-99% diamond powder and the remainder binder.

[0015] Preferably, the particle size range D50 of the binder is 0-20 μm.

[0016] Preferably, the diamond powder has a particle size range D50 of 0-50 μm.

[0017] Preferably, the diamond powder may be of a single particle size or a combination of multiple particle sizes.

[0018] Preferably, the cemented carbide substrate is tungsten carbide cemented carbide in which the weight of cobalt metal accounts for 8-20%.

[0019] Preferably, in step (3), the sintering pressure ranges from 4.5 GPa to 10 GPa, the sintering temperature ranges from 1100 to 2000° C., and the sintering time ranges from 10 to 1500 s.

[0020] A diamond composite sheet is produced according to a manufacturing process of a high-performance diamond composite sheet.

[0021] (III) Beneficial effects

[0022] The present invention provides a high-performance diamond composite sheet and a manufacturing process thereof, which has the following beneficial effects:

[0023] The present invention uses a carbon-containing metal melt binder to synthesize a diamond composite sheet. During the synthesis process, the carbon in the binder itself can be directly precipitated and converted into diamond, reducing the dissolution and re-precipitation process of diamond micropowders. At the same time, the filling of the precipitated diamonds in the gaps of the diamond micropowders is further increased, more covalent bonds are formed between the diamond micropowders, and the impact resistance and wear resistance of the diamond composite sheet are improved. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] Example:

[0026] A manufacturing process for a high-performance diamond composite sheet comprises the following steps:

[0027] (1) Mixing: Diamond powder and binder are fully mixed and uniformly mixed. The mixing method can be grinding mixing, ball milling mixing, vibration mixing or the mixing method of patent "202010579730.7", the purpose of which is to mix the raw materials uniformly;

[0028] (2) Assembly: Assemble the cemented carbide matrix, the uniformly mixed diamond powder and the binder, put the mixture into a metal shielding cup for internal assembly, and then assemble it with the pyrophyllite assembly block, salt tube, carbon tube, magnesium tube, etc., and finally assemble it into a pyrophyllite assembly block that can be used for synthesis. The specific assembly block structure can refer to patents such as 2014206354359, 202121300420.3, 202120159318.X, 201910771712.6, and 201820377284.X;

[0029] (3) Sintering: high temperature and high pressure sintering process is used to sinter and synthesize high performance new binder diamond composite sheet;

[0030] The binder is a metal material containing carbon, and the maximum carbon content is the saturation value of the binder in a molten state, similar to the dissolution of a substance in a solvent. The amount of carbon used should be sufficient to ensure that the binder can be completely dissolved in a dissolved state.

[0031] The metal in the binder is one or more of cobalt, nickel, and iron, and the carbon in the binder can be graphite, graphene, or amorphous carbon.

[0032] The weight percentage of diamond powder and binder is: 80-99% of diamond powder and the rest of binder.

[0033] The particle size range of the binder D50 is 0-20 μm, the particle size range of the diamond micropowder D50 is 0-50 μm, and the diamond micropowder can be a single particle size or a combination of multiple particle sizes.

[0034] The cemented carbide matrix is ​​tungsten carbide cemented carbide in which the weight of cobalt metal accounts for 8 to 20%.

[0035] In step (3), the sintering pressure ranges from 4.5 GPa to 10 GPa, the sintering temperature ranges from 1100 to 2000° C., and the sintering time ranges from 10 to 1500 s.

[0036] A diamond composite sheet is produced according to a manufacturing process of a high-performance diamond composite sheet.

[0037] This article provides a specific production process: the median value D50 of the first particle size diamond micropowder is 10m, and the median value D50 of the second particle size diamond micropowder is 15m; the cobalt melt saturated with graphite is used as a binder, and the median value D50 of the particle size is 3m;

[0038] The weight ratio of the first-size diamond powder to the second-size diamond powder is 3:7, and the addition ratio of the binder is 4%. The above diamond powder and binder materials are mixed evenly;

[0039] Assembling the mixed raw materials with the cemented carbide matrix and auxiliary materials into a composite block;

[0040] The assembled synthetic block was sintered at a pressure of 5 GPa and a temperature of 1400 °C for 600 s.

[0041] According to tests, the wear resistance of the diamond composite sheet synthesized by using this binder is improved by more than 15%, and the impact strength is improved by more than 10% compared with the diamond composite sheet synthesized by using traditional metal binders.

[0042] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A manufacturing process for high-performance diamond composite sheets, It is characterized in that The steps include: (1) Mixing: Diamond powder and binder are fully mixed; (2) Assembling: Assembling the cemented carbide substrate, the uniformly mixed diamond powder and the binder; (3) Sintering: high temperature and high pressure sintering process is used to sinter and synthesize high performance new binder diamond composite sheet; The binder is a carbon-containing metal material, and the maximum value of the carbon content is a saturation value of the binder in a molten state. The metal in the binder is one or more of cobalt, nickel, and iron. The carbon in the binder is one or more of graphite, graphene, and amorphous carbon. In the step (3), the sintering pressure ranges from 4.5 GPa to 10 GPa, the sintering temperature ranges from 1100 to 2000° C., and the sintering time ranges from 10 to 1500 s.

2. A process for manufacturing a high-performance diamond composite sheet according to claim 1, Features: The weight percentage of the diamond powder and the binder is: 80-99% of the diamond powder and the rest of the binder.

3. A process for manufacturing a high-performance diamond composite sheet according to claim 1, Features: The particle size D50 of the binder is in the range of 0-20 μm.

4. The manufacturing process of a high-performance diamond composite sheet according to claim 1, Features: The diamond micro powder has a particle size range D50 of 0-50 μm.

5. A process for manufacturing a high-performance diamond composite sheet according to claim 4, Features: The diamond powder may be of a single particle size or a combination of multiple particle sizes.

6. A process for manufacturing a high-performance diamond composite sheet according to claim 1, Features: The cemented carbide substrate is tungsten carbide cemented carbide in which the weight of cobalt metal accounts for 8-20%.

7. A diamond composite sheet produced according to the manufacturing process of a high-performance diamond composite sheet according to any one of claims 1 to 6.