Sintered NdFeB magnet with high toughness and method for making the same
By placing the main and secondary alloys in the sintered NdFeB magnet and forming Nd-Fe-B or Pr-Fe-B shells, the problem of insufficient impact toughness of the material is solved, the toughness and magnetic properties of the magnet are improved, and the Resource waste has expanded market applications.
Patent Information
- Application Number
- CN202210066133.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-01-20
AI Technical Summary
The impact toughness of sintered NdFeB magnet materials leads to a large number of defective products during processing, reducing product pass rate and increasing resource waste, limiting its market application.
By configuring the main and secondary alloys, and replacing the Ce element with Nd and Pr elements during vacuum sintering, an Nd-Fe-B or Pr-Fe-B shell is formed to increase the impact toughness of the material, and Sn and Cu are used. , Al element reduces the melting point of the secondary phase and enhances the fluidity and the bonding force between the main and secondary phases.
It significantly improves the impact toughness of the sintered NdFeB magnet, reduces the chance of edge-crystal fracture, increases the residual magnetic induction strength and intrinsic coercive force, reduces microscopic defects, and improves product production efficiency and market application scope.
Smart Images

Figure CN114267533B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sintered NdFeB magnets, and in particular to a sintered NdFeB magnet with high toughness and a manufacturing method thereof. Background Art
[0002] Sintered NdFeB magnet is a rare earth iron permanent magnetic functional material, and its comprehensive magnetic properties are the best among the permanent magnetic materials discovered so far. The market of sintered NdFeB magnet covers many fields such as computers, communications, electroacoustics, new energy, aerospace, automobiles, industrial servo motors, and household appliances. Since sintered NdFeB magnets contain about 30% of metal Nd (neodymium), this rare earth metal is a relatively scarce and expensive material. For cost considerations, the industry usually uses relatively low-priced metal Ce (cerium) to partially replace metal neodymium for some medium and low-performance grades of sintered NdFeB magnets. However, the addition of metal cerium to the material will form Ce2Fe 14 B compound, this Ce2Fe 14 Compared with Nd2Fe produced by not using cerium to replace neodymium, 14 B compounds are more brittle. Since the vast majority of finished products of sintered NdFeB magnets are small and special-shaped, the finished products basically need to be made by various forms of mechanical processing of sintered NdFeB magnets. Common mechanical processing methods include flat grinding, centerless grinding, slicing, punching, hole punching, square cutting and rounding, wire cutting, special-shaped grinding wheel grinding, chamfering, electroplating, electrophoresis, phosphating, etc., and the above processing processes have high requirements for the impact toughness of the sintered NdFeB magnet material itself. If the impact toughness of the sintered NdFeB magnet material is poor, a large number of defective products such as knocked edges, dropped corners, and broken parts will inevitably be produced during the processing process, which will not only reduce the qualified rate of the product, but also cause a certain degree of resource waste, and will greatly reduce the production profit of the enterprise, and even seriously restrict the market application scope of sintered NdFeB magnet materials. Therefore, how to improve the impact toughness of sintered NdFeB magnets has become an important technical issue that needs to be solved in this industry. Summary of the invention
[0003] The technical problem to be solved by this technical solution is how to improve the impact toughness of sintered NdFeB magnet materials to avoid the generation of a large number of defective products in the subsequent finished product processing of sintered NdFeB magnet materials, thereby ensuring that the processed finished products have a high pass rate, and to a certain extent reduce the waste of resources, and can increase the production profit of the enterprise.
[0004] In order to solve the above technical problems, the present technical solution provides a method for manufacturing a sintered NdFeB magnet with high toughness, the steps of the manufacturing method comprising:
[0005] Configuring main and sub-phase alloys: configuring a main phase alloy, the main phase alloy comprising: 9 to 16 wt% Nd by mass, 3 to 6 wt% Pr by mass, 5 to 16 wt% Ce by mass, 0.95 to 1.1 wt% B by mass, 0.8 to 4.8 wt% of a metal mixture consisting of at least two of Gd, Co, Ga and Zr by mass, and the remainder being Fe by mass; configuring a sub-phase alloy, the sub-phase alloy comprising: 40 to 55 wt% Nd by mass, 13 to 20 wt% Pr by mass, 3 to 10 wt% Sn by mass, 5 to 10 wt% Cu by mass, 10 to 20 wt% Al by mass, and the remainder being a metal mixture consisting of at least one of Dy, Ho and Ga by mass;
[0006] Preparation of main phase alloy and sub-phase alloy castings: preparing the main phase alloy and sub-phase alloy castings by melting and strip-spinning processes respectively;
[0007] Mixing the main phase alloy flakes and the secondary phase alloy flakes: mixing the main phase alloy flakes in a ratio of 90 to 97% by mass and the secondary phase alloy flakes in a ratio of 3 to 10% by mass;
[0008] Crushing the main and sub-phase alloy flakes: crushing the mixed main and sub-phase alloy flakes by hydrogen crushing and air flow milling, and uniformly mixing the fine powders generated after crushing;
[0009] Micro powder pressing and molding: Use sintered NdFeB magnet molding molds to orient the micro powder in the magnetic field and press it to make a compact, and then vacuum package and isostatically press the compact;
[0010] Vacuum sintering of compact: remove the vacuum packaging of the compact and put it into a graphite box and send it into a vacuum sintering furnace for vacuum sintering;
[0011] Heat treatment: The vacuum sintered compact is tempered to obtain a sintered blank.
[0012] The production method of the present technical solution adds a secondary phase alloy casting sheet to the main phase alloy casting sheet so that in the subsequent vacuum sintering process, the Ce element at the boundary of the main phase of the material is replaced by the Nd and Pr elements in the secondary phase to form a Nd-Fe-B or Pr-FeB shell layer, thereby effectively improving the impact toughness of the sintered NdFeB magnet material after sintering; in addition, the addition of Sn, Cu, and Al elements in the secondary phase alloy can effectively reduce the melting point of the secondary phase, enhance the fluidity of the secondary phase, reduce the micro defects of the sintered NdFeB magnet material, and effectively enhance the wettability of the main phase and the secondary phase, improve the bonding strength of the main phase and the secondary phase, and reduce the probability of intergranular fracture.
[0013] As another implementation of the present technical solution, in the step of preparing main and sub-phase alloy castings, the maximum vacuum degree in the melting furnace is 1 to 10Pa, the pressure after argon is filled into the melting furnace during the melting process is -0.04MPa, the melting temperature of the main phase alloy is 1350 to 1450°C, and the melting temperature of the sub-phase alloy is 1100 to 1200°C.
[0014] As another implementation of the present technical solution, in the step of crushing the main and sub-phase alloy flakes, 0.1 to 0.3 MPa of hydrogen is filled into the hydrogen crushing reactor to make the main and sub-phase alloy flakes absorb hydrogen with the hydrogen, and after the hydrogen absorption is saturated, the temperature in the hydrogen crushing reactor is heated to 500 to 600°C, and then the furnace is evacuated for 2 to 5 hours for dehydrogenation and cooled to room temperature to crush the main and sub-phase alloy flakes into coarse powder.
[0015] As another implementation of the present technical solution, in the step of crushing the main and sub-phase alloy flakes, the coarse powder is placed in a jet mill for further crushing, and nitrogen protection is introduced into the crushing process to generate fine powder with an average particle size between 2.5 and 3.5 μm. The output fine powder is fully and evenly mixed to avoid component segregation.
[0016] As another implementation of the technical solution, in the micro-powder pressing step, the magnetic field intensity of the magnetic field orientation is ≥1.5T.
[0017] As another implementation of the technical solution, in the step of vacuum sintering the green compact, the sintering temperature of the vacuum sintering is 1000 to 1100° C., the holding time is 5 hours, and the green compact is cooled to below 100° C. after sintering and holding.
[0018] As another implementation of the present technical solution, in the heat treatment step, the pressed green body is subjected to two-stage tempering treatment in a vacuum or inert protective gas environment, the first-stage tempering aging temperature is 850 to 950°C and the holding time is 2 hours, the second-stage tempering aging temperature is 450 to 630°C and the holding time is 5.5 hours, and the pressed green body is cooled to room temperature to obtain a sintered green body, that is, a sintered NdFeB magnet.
[0019] The technical solution also provides a sintered NdFeB magnet with high toughness produced by the above-mentioned production method. The final composition of the sintered NdFeB magnet produced by the above-mentioned production method has a total rare earth mass content of 28.8 to 33.2wt%, wherein the mass content of Ce is ≥5wt%, the mass content of Sn is 0.1 to 0.5wt%, the mass content of Cu is 0.15 to 0.7wt%, and the mass content of Al is 0.3 to 1.2wt%. The above-mentioned Sn, Cu, and Al elements are mixed and added through the secondary phase alloy before hydrogen crushing to avoid entering the main phase grains and affecting the residual magnetic induction intensity of the sintered NdFeB magnet. In addition, the above-mentioned Sn, Cu, and Al elements exist in the rare earth-rich phase of the sintered NdFeB magnet to reduce the liquidus point of the secondary phase and increase the fluidity of the liquid phase during sintering, so that the secondary phase is more evenly distributed around the main phase of the sintered NdFeB magnet, reducing the microscopic defects at the intersection of the main and secondary phases; and can also reduce the contact angle between the main and secondary phases, making the main phase and the secondary phase more strongly bonded, and increasing the difficulty of intergranular fracture. In addition, the secondary phase alloy does not contain Ce elements. During the sintering process, the Nd and Pr elements in the secondary phase replace Ce2Fe 14 The Ce element in the outer layer of the B main phase grains forms Nd2Fe 14 B or Pr2Fe 14 B shell, the Nd2Fe formed at the grain boundary of the main phase 14 B or Pr2Fe 14 The B shell is less brittle, which can significantly increase the impact energy required for the material to fracture along the crystal. In addition, the Nd2Fe 14 B or Pr2Fe 14 The saturation magnetic polarization intensity of the B shell is higher, which can effectively increase the residual magnetic induction intensity (Br) of the material, and the Nd2Fe 14 B or Pr2Fe 14 The anisotropy field of the B shell is higher, which can greatly improve the intrinsic coercivity (Hcj) of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The present invention is a flow chart of a method for manufacturing a sintered NdFeB magnet with high toughness.
[0021] Figure 2 It is the energy spectrum at the main phase boundary of the sintered NdFeB magnet prepared from the main and sub-phase alloys of the present invention, and also shows the energy spectrum of other components at the main phase boundary.
[0022] Figure 3 It is the energy spectrum at the main phase boundary of the sintered NdFeB magnet prepared from a single-phase alloy in the existing process, and also shows the energy spectrum of other components at the main phase boundary.
[0023] Figure 4The backscattering image of the cross section of the sintered NdFeB magnet prepared from the main and sub-phase alloys of the present invention is made under a scanning electron microscope (SEM).
[0024] Figure 5 This is a backscattered image of the cross section of a sintered NdFeB magnet prepared from a single-phase alloy in the existing process, taken under a scanning electron microscope.
[0025] Explanation of symbols in the accompanying drawings:
[0026] Steps S1 to S7. DETAILED DESCRIPTION
[0027] The detailed description and technical contents of the present invention are described as follows with reference to the accompanying drawings. However, the accompanying drawings are only provided for reference and description and are not intended to limit the present invention.
[0028] like Figure 1 FIG. 1 is a flow chart of a method for manufacturing a sintered NdFeB magnet with high toughness according to the present invention, wherein the steps of the method include:
[0029] Step S1 of configuring main and sub-phase alloys: configuring a main phase alloy, wherein the main phase alloy comprises: 9 to 16 wt% Nd by mass, 3 to 6 wt% Pr by mass, 5 to 16 wt% Ce by mass, 0.95 to 1.1 wt% B by mass, 0.8 to 4.8 wt% of a metal mixture consisting of at least two of Gd, Co, Ga and Zr by mass, and the remainder being Fe by mass; configuring a sub-phase alloy, wherein the sub-phase alloy comprises: 40 to 55 wt% Nd by mass, 13 to 20 wt% Pr by mass, 3 to 10 wt% Sn by mass, 5 to 10 wt% Cu by mass, 10 to 20 wt% Al by mass, and the remainder being a metal mixture consisting of at least one of Dy, Ho and Ga by mass.
[0030] Step S2 of preparing main phase alloy and sub-phase alloy castings: preparing main phase alloy and sub-phase alloy castings through smelting and strip spinning processes respectively.
[0031] Step S3 of mixing the main phase alloy flakes and the sub-phase alloy flakes: mixing the main phase alloy flakes in a ratio of 90 to 97% by mass and the sub-phase alloy flakes in a ratio of 3 to 10% by mass.
[0032] Step S4 of crushing the main phase and the sub-phase alloy flakes: crushing the mixed main phase and the sub-phase alloy flakes by hydrogen crushing and air flow milling, and uniformly mixing the fine powders generated after crushing.
[0033] Micro-powder pressing step S5: using a sintered NdFeB magnet forming mold to orient the micro-powder in a magnetic field and press-form it to form a compact, and then vacuum-packaging and isostatically pressing the compact.
[0034] Green compact vacuum sintering step S6: removing the vacuum package from the green compact and placing it into a graphite box and sending it into a vacuum sintering furnace for vacuum sintering.
[0035] Heat treatment step S7: Tempering the vacuum sintered compact to obtain a sintered blank.
[0036] More specifically, the present invention combines 12 groups of main and auxiliary phase alloys with different mass contents, such as the 12 groups of embodiments in Table 1 below, and manufactures sintered NdFeB magnets according to the above steps:
[0037]
[0038]
[0039]
[0040] Table 1
[0041] The specific preparation process is as follows:
[0042] The main phase alloy and the sub-phase alloy are configured in step S1, according to the mass content of each component of the main phase alloy and the sub-phase alloy of each embodiment in Table 1. It is noted that the sub-phase alloy components of embodiments 1, 2, 11, and 12 may not contain a metal mixture composed of at least one of Dy, Ho, and Ga, but may only be composed of Nd, Pr, Al, Cu, and Sn.
[0043] Step S2 of preparing main and secondary phase alloy castings, respectively, melt and spin the configured main phase alloy and secondary phase alloy through a vacuum medium frequency induction strip spinning furnace to prepare main phase alloy castings and secondary phase alloy castings, wherein the maximum vacuum degree in the melting furnace is 1 to 10Pa, and the pressure after argon is filled into the melting furnace during the melting process is -0.04MPa, the melting temperature of the main phase alloy is 1350 to 1450°C, and the melting temperature of the secondary phase alloy is 1100 to 1200°C, and the thickness of the main and secondary phase alloy castings are both 0.25 to 0.35mm.
[0044] In step S3 of mixing the main phase alloy flakes and the sub-phase alloy flakes, the main phase alloy flakes and the sub-phase alloy flakes are mixed according to the mass percentages in Table 1.
[0045] The main and sub-phase alloy flakes are crushed in step S4, wherein the mixed main and sub-phase alloy flakes are crushed by hydrogen crushing and air flow milling process, wherein 0.1 to 0.3 MPa hydrogen is filled into the hydrogen crushing reactor to make the main and sub-phase alloy flakes absorb hydrogen with the hydrogen, and after the hydrogen absorption is saturated, the temperature in the hydrogen crushing reactor is heated to 500 to 600° C., and then the main and sub-phase alloy flakes are vacuumed for 2 to 5 hours for dehydrogenation and cooled to room temperature to crush the main and sub-phase alloy flakes into coarse powder; and then the coarse powder is placed in the air flow mill for further crushing, and nitrogen protection is introduced into the crushing process to generate fine powder with an average particle size between 2.5 and 3.5 μm, and the produced fine powder is fully and evenly mixed to avoid component segregation.
[0046] In the powder pressing step S5, the powder is magnetically oriented and pressed using a sintered NdFeB magnet forming mold to form a compact (i.e., a NdFeB green compact), wherein the magnetic field intensity of the magnetic field orientation is ≥1.5T, and then the compact is vacuum packaged and isostatically pressed.
[0047] In step S6 of vacuum sintering of the pressed green body, the pressed green body is removed from the vacuum packaging and placed in a graphite box and sent to a vacuum sintering furnace for vacuum sintering, or sintered under an inert gas, wherein the sintering temperature is 1000 to 1100°C and the holding time is 5 hours. After sintering and holding, the pressed green body is cooled to below 100°C.
[0048] Heat treatment step S7, the vacuum sintered green compact is subjected to two-stage tempering treatment in a vacuum or inert protective gas environment, the first stage tempering temperature is 850 to 950°C and the holding time is 2 hours, the second stage tempering temperature is 450 to 630°C and the holding time is 5.5 hours, and the green compact is cooled to room temperature to obtain a sintered green compact, that is, a sintered NdFeB magnet.
[0049] The present invention also provides 12 groups of comparative examples compared with the above 12 groups of embodiments. The 12 groups of comparative examples are prepared according to the existing preparation process and the mass content components in Table 2 below are smelted at 1350 to 1450°C in a vacuum medium frequency induction belt-spinning furnace, and then spun to prepare alloy sheets with a sheet thickness of 0.25 to 0.35 mm, and then prepared into sintered NdFeB magnets through the process steps of hydrogen crushing, air flow grinding, magnetic field orientation pressing, vacuum isostatic pressing, and vacuum sintering.
[0050]
[0051]
[0052] Table 2
[0053] The present invention conducts magnetic property detection and comparison on sintered NdFeB magnets prepared by 12 groups of embodiments and 12 groups of comparative examples, as shown in Table 3. When the final composition of the sintered NdFeB magnets is roughly the same, the sintered NdFeB magnets prepared by the main and auxiliary phase alloy method have a slight improvement of 0.09 to 0.18 kGs in residual magnetic polarization intensity (Br), and an increase of 0.5 to 0.76 kOe in intrinsic coercive force (H cj).
[0054] Br(kGs) Hcj(kOe) Hk / Hcj(%) Example 1 13.83 12.78 97.3 Comparative Example 1 13.70 12.15 97.1 Example 2 13.56 12.73 98.3 Comparative Example 2 13.44 12.10 97.9 Example 3 13.59 13.36 98.8 Comparative Example 3 13.44 12.77 98.8 Example 4 13.29 13.01 96.9 Comparative Example 4 13.11 12.31 97.1 Example 5 13.31 12.78 98.7 Comparative Example 5 13.17 12.21 98.3 Example 6 13.48 12.75 97.6 Comparative Example 6 13.37 12.25 97.3 Example 7 12.97 12.66 98.1 Comparative Example 7 12.85 12.03 97.6 Example 8 13.75 15.35 97.3 Comparative Example 8 13.62 15.03 98.1 Example 9 13.45 14.43 97.3 Comparative Example 9 13.36 13.88 97.1 Example 10 13.15 15.51 97.6 Comparative Example 10 13.01 14.76 97.1 Embodiment 11 13.90 12.45 97.8 Comparative Example 11 13.81 11.92 97.4 Example 12 13.65 13.56 97.0 Comparative Example 12 13.53 12.80 95.0
[0055] Table 3
[0056] In addition, the present invention also performs energy spectrum analysis on the main phase boundaries of the sintered NdFeB magnets prepared in Example 1 and Comparative Example 1 respectively. Figure 2 The energy spectrum at the main phase boundary of the sintered NdFeB magnet of Example 1 is shown, from which it can be known that the proportion of Ce element at the main phase boundary in Example 1 is 1.75at%. Figure 3 The energy spectrum at the grain boundary of the sintered NdFeB magnet of Comparative Example 1 is shown. It can be seen that the Ce element accounts for 4.75 at% in the grain boundary phase in Comparative Example 1. Table 4 below shows the Ce element content at the main phase boundary of the sintered NdFeB magnets prepared by 12 groups of embodiments and 12 groups of comparative examples. Figure 2 , Figure 3 It can be clearly seen from Table 4 that the Ce content at the grain boundary of the sintered NdFeB magnet prepared by the main and auxiliary phase alloys is low.
[0057]
[0058]
[0059] Table 4
[0060] In addition, the following Table 5 is the sum of the atomic percentages of Sn, Al, and Cu contained in the main phase and the rare earth-rich phase of the sintered NdFeB magnets of the 12 groups of embodiments obtained by energy spectrum analysis using a scanning electron microscope (SEM). It can be seen from Table 5 that the content of Sn, Al, and Cu elements in the main phase of the 12 groups of embodiments is significantly lower than the content of Sn, Al, and Cu elements in the rare earth-rich phase.
[0061]
[0062]
[0063] Table 5
[0064] Figure 4 This is a backscattered image of the sintered NdFeB magnet prepared in Example 1 of the present invention under a scanning electron microscope. Figure 5 The backscattered image of the sintered NdFeB magnet prepared in Comparative Example 1 under a scanning electron microscope is shown in FIG. By comparison, it can be seen that the sintered NdFeB magnet prepared by the main-subphase alloy method has a more uniform distribution of the subphase around the main phase, a smaller contact angle between the main and subphases, and a tighter combination, that is, fewer microscopic defects at the intersection of the main and subphases.
[0065] The above energy spectrum, backscattering diagram and magnetic property analysis fully illustrate that the Ce element at the grain boundary of the main phase of the sintered NdFeB magnet prepared by the method of adding the secondary phase alloy to the main phase alloy is mostly replaced by the Nd and Pr elements in the secondary phase, while the Sn, Al and Cu elements in the secondary phase are mostly left in the rare earth-rich phase, thus forming a Ce2Fe2O3 phase at the grain boundary of the main phase. 14 B, the saturation magnetic polarization intensity and magnetocrystalline anisotropy field are higher than Nd2Fe 14 B or Pr2F e 14 B shell, thus significantly improving the intrinsic coercive force (Hcj) of the magnet while increasing the residual magnetic polarization intensity (Br) of the sintered NdFeB magnet.
[0066] The sintered NdFeB magnets prepared by 12 groups of embodiments and 12 groups of comparative examples of the present invention are processed into standard size impact specimens with a length of 55 mm and a cross section of 10*10 mm with reference to "GB / T229-2007 Metal Material Charpy Pendulum Impact Test Method", with a V-shaped notch in the middle of the specimen length, a V-shaped notch angle of 45°, and a depth of 2 mm. A JB-S300 digital display pendulum impact testing machine is used to perform an impact toughness test with a 150J pendulum. The test results are shown in Table 6 below.
[0067]
[0068]
[0069] Table 6
[0070] According to the results shown in Table 6 and combined with the above comparison, it can be seen that the Ce element at the main phase boundary of the sintered NdFeB magnet in the embodiment of the present invention is mostly replaced by Nd and Pr elements in the secondary phase to form Nd2Fe 14 B or Pr2Fe14B shell; at the same time, Sn, Cu, Al elements can significantly reduce the liquidus point of the secondary phase, and can also reduce the contact angle between the main and secondary phases. Therefore, it not only increases the surface tension of the liquid phase, but also enhances the wettability of the secondary phase around the main phase, so that the probability of microscopic defects at the coupling between the main phase and the secondary phase of the sintered NdFeB magnet is significantly reduced, and the probability of intergranular fracture is reduced, thereby greatly improving the impact toughness of the sintered NdFeB magnet.
[0071] The sintered NdFeB magnet with high toughness prepared by the above-mentioned manufacturing method of the present invention has a total rare earth mass content of 28.8 to 33.2wt% in the final composition of the sintered NdFeB magnet, wherein the mass content of Ce is ≥5wt%, the mass content of Sn is 0.1 to 0.5wt%, the mass content of Cu is 0.15 to 0.7wt%, and the mass content of Al is 0.3 to 1.2wt%. The above-mentioned Sn, Cu, and Al elements are mixed and added to the main phase alloy through the secondary phase alloy before hydrogen crushing to avoid entering the main phase grains and affecting the residual magnetic induction intensity of the sintered NdFeB magnet. In addition, the above-mentioned Sn, Cu, and Al elements exist in the rare earth-rich phase of the sintered NdFeB magnet to reduce the liquidus point of the secondary phase and increase the fluidity of the liquid phase during sintering, so that the secondary phase is more evenly distributed around the main phase of the sintered NdFeB magnet, reducing the microscopic defects at the intersection of the main and secondary phases; and can also reduce the contact angle between the main and secondary phases, making the main phase and the secondary phase more strongly bonded, and increasing the difficulty of intergranular fracture. In addition, the secondary phase alloy does not contain Ce elements. During the sintering process, the Nd and Pr elements in the secondary phase replace Ce2Fe 14 The Ce element in the outer layer of the B main phase grains forms Nd2Fe 14 B or Pr2Fe 14 B shell, the Nd2Fe formed at the grain boundary of the main phase 14 B or Pr2Fe 14 The B shell is less brittle, which can significantly increase the impact energy required for the material to fracture along the crystal. In addition, the Nd2Fe 14 B or Pr2Fe 14 The saturation magnetic polarization intensity of the B shell is higher, which can effectively increase the residual magnetic induction intensity (Br) of the material, and the Nd2Fe 14 B or Pr2Fe 14 The anisotropy field of the B shell is higher, which can greatly improve the intrinsic coercivity (Hcj) of the material.
[0072] The above are only preferred embodiments of the present invention and are not intended to limit the patent scope of the present invention. Other equivalent changes made using the patent concept of the present invention should all fall within the patent protection scope of the present invention.
Claims
1. A method for producing a sintered NdFeB magnet with high toughness, characterized in that the steps include: Configuration of main and sub-phase alloys: Configuration of a main phase alloy, the main phase alloy comprising: 9 to 16 wt% Nd by mass, 3 to 6 wt% Pr by mass, 5 to 16 wt% Ce by mass, 0.95 to 1.1 wt% B by mass, 0.6 to 1.1 wt% Co by mass, 0.1 to 0.12 wt% Zr by mass, 68.55 to 71.1 wt% Fe by mass, 1 to 3.6 wt% Gd by mass and / or 0.1 to 0.15 wt% Gd by mass. % of Ga or does not contain Gd and Ga; configure a subphase alloy, the subphase alloy comprises: 40 to 55wt% of Nd by mass, 13 to 20wt% of Pr by mass, 3 to 10wt% of Sn by mass, 5 to 10wt% of Cu by mass, 10 to 20wt% of Al by mass, and 0.5 to 8.4wt% of Dy by mass and / or 1.5 to 8wt% of Ho by mass and / or 0.6 to 0.75wt% of Ga by mass, or does not contain Dy, Ho and Ga; Preparation of main phase alloy and sub-phase alloy castings: preparing the main phase alloy and the sub-phase alloy into main phase alloy castings and sub-phase alloy castings by smelting and strip-spinning processes respectively; Mixing the main phase alloy flakes and the secondary phase alloy flakes: mixing the main phase alloy flakes in a ratio of 90 to 97% by mass and the secondary phase alloy flakes in a ratio of 3 to 10% by mass; Crushing the main and sub-phase alloy flakes: crushing the mixed main and sub-phase alloy flakes by hydrogen crushing and air flow milling, and uniformly mixing the fine powders generated after crushing; Micro powder pressing and molding: using a sintered NdFeB magnet molding mold to orient the micro powder in a magnetic field and press it to form a compact, and then vacuum packaging and isostatic pressing the compact; Vacuum sintering of compact: removing the vacuum packaging of the compact and placing it in a graphite box and sending it into a vacuum sintering furnace for vacuum sintering; Heat treatment: the compact after vacuum sintering is tempered to obtain a sintered blank.
2. The method for manufacturing a sintered NdFeB magnet with high toughness according to claim 1, characterized in that: In the step of preparing the main and sub-phase alloy castings, the maximum vacuum degree in the melting furnace is 1 to 10Pa, and the pressure after argon is filled into the melting furnace during the melting process is -0.04MPa. The melting temperature of the main phase alloy is 1350 to 1450°C, and the melting temperature of the sub-phase alloy is 1100 to 1200°C.
3. The method for manufacturing a sintered NdFeB magnet with high toughness according to claim 1, characterized in that: In the step of crushing the main and sub-phase alloy flakes, 0.1 to 0.3 MPa of hydrogen is filled into the hydrogen crushing reactor to make the main and sub-phase alloy flakes absorb hydrogen with the hydrogen, and after the hydrogen absorption is saturated, the temperature in the hydrogen crushing reactor is heated to 500 to 600° C., and then vacuumed for 2 to 5 hours for dehydrogenation and cooled to room temperature to crush the main and sub-phase alloy flakes into coarse powder.
4. The method for manufacturing a sintered NdFeB magnet with high toughness according to claim 3, characterized in that: In the step of pulverizing the main phase and sub-phase alloy flakes, the coarse powder is placed in a jet mill for further pulverization, and nitrogen is introduced into the pulverization process to generate fine powder with an average particle size between 2.5 and 3.5 μm.
5. The method for manufacturing a sintered NdFeB magnet with high toughness according to claim 1, characterized in that: In the micro-powder pressing step, the magnetic field intensity of the magnetic field orientation is ≥1.5T.
6. The method for manufacturing a sintered NdFeB magnet with high toughness according to claim 1, characterized in that: In the step of vacuum sintering the green compact, the sintering temperature of the vacuum sintering is 1000 to 1100° C., the holding time is 5 hours, and the green compact is cooled to below 100° C. after sintering and holding.
7. The method for manufacturing a sintered NdFeB magnet with high toughness according to claim 1, characterized in that: In the heat treatment step, the pressed blank is subjected to two-stage tempering treatment in a vacuum or inert protective gas environment, the first-stage tempering aging temperature is 850 to 950°C and the holding time is 2 hours, the second-stage tempering aging temperature is 450 to 630°C and the holding time is 5.5 hours, and the pressed blank is cooled to room temperature to obtain a sintered blank.
8. A sintered NdFeB magnet with high toughness manufactured by the method for manufacturing a sintered NdFeB magnet with high toughness as claimed in any one of claims 1 to 7.