A black talc adsorption material and its preparation method and application

By purifying and modifying black talc, a black talc adsorbent material with a larger specific surface area and abundant surface active sites was prepared, which solved the problem of insufficient adsorption performance of black talc in the existing technology and achieved efficient adsorption of heavy metal ions.

CN114288985BActive Publication Date: 2024-11-05ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111632744.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-29
Publication Date
2024-11-05
Estimated Expiration
2041-12-29

AI Technical Summary

Technical Problem

Existing natural clay minerals, such as black talc, have drawbacks in terms of adsorption performance, including small specific surface area, few adsorption sites, and easy aggregation, making them difficult to effectively remediate contaminated soil.

Method used

By purifying and modifying black talc, including treatment with disodium hydrogen phosphate, ultrasonic dispersion with ethanol, and modification with citric acid or tartaric acid, black talc adsorbent materials with larger specific surface area and abundant surface active sites are prepared.

Benefits of technology

It improves the adsorption performance and stability of black talc, enhances its adsorption capacity for heavy metal ions, has a fast adsorption rate and high adsorption capacity, and has a simple preparation method with easy-to-control conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003441512860000011
    Figure HDA0003441512860000011
  • Figure HDA0003441512860000021
    Figure HDA0003441512860000021
Patent Text Reader

Abstract

The present invention discloses a black talc soil adsorption material and a preparation method thereof, and belongs to the field of non-metallic mineral materials. The black talc soil adsorption material prepared by the method of the present invention has abundant chemical active sites and Mg coordination unsaturated sites, and can interact with heavy metals in the soil through hydrogen bonds, electrostatic attraction, and van der Waals forces, thereby improving the ability to bind with heavy metal ions. The preparation method of the present invention is simple, and the reaction conditions are easy to control. It has the advantages of stable skeleton structure, lasting repair effect, proper adjustment of soil pH and air permeability, environmental friendliness, no secondary pollution, etc. It has good repair effects on soils contaminated by different pollutants, and has a very broad application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of non-metallic mineral materials, and specifically relates to a black talc adsorption material and a preparation method and application thereof. Background Art

[0002] Soil is a natural resource that humans rely on for survival. Soil is composed of three types of substances: solid phase, liquid phase, and gas phase, mainly including minerals, organic matter, water, air, and microorganisms. Healthy soil should include about 45% minerals, about 25% air, about 25% water, about 5% organic matter, and about 1% microorganisms. However, crop cultivation on soil has long been in a state of high intensification, high multiple cropping index, and high fertilizer input, resulting in a series of soil obstacles such as reduced crop yields, secondary soil salinization, soil acidification, and nutrient imbalance.

[0003] In the contaminated soil, more than 80% are toxic inorganic pollutants, the most common of which are Pb 2+ 、Cd 2+ Cr 3 + , Cu 2+ 、Co 2+ 、Ni 2+ 、Zn 2+ Heavy metal ions such as arsenate, chromate, selenate, and sulfate, as well as toxic anions such as arsenate, chromate, selenate, and sulfate. In addition, soil pollution caused by typical organic substances such as polycyclic aromatic hydrocarbons (PAHs), polychlorinated biphenyls (PCBs), organochlorine pesticides (OCPs), and petroleum cannot be ignored. Pollutants dispersed in the soil may affect plant growth or enter the human body through the food chain, causing great harm to human health. It can be seen that the remediation of soil pollution is imminent. Among the available treatment options, adsorption is generally considered to be the most economical technology, which can treat a variety of pollutants, has high efficiency, simple design, convenient operation, and produces fewer toxic by-products. Natural clay minerals (such as diatomaceous earth, black talc, bentonite, attapulgite, sepiolite, kaolin, etc.) have the advantages of abundant sources, low prices, and large specific surface areas. They have received more attention in recent years and have gradually become a material that can effectively replace conventional adsorbents. However, most of them have different disadvantages such as low adsorption capacity, few effective adsorption sites, and easy agglomeration. Therefore, it is important to develop an adsorption material that is efficient, stable, and easy to separate from the solvent after treatment.

[0004] As a natural clay mineral, black talc has a TOT-type layered structure, consisting of two silicon-oxygen tetrahedral sheets and one magnesium-oxygen octahedron. As a layered silicate mineral without interlayer charge, it has excellent chemical stability. At the same time, the surface of black talc contains active functional groups, such as Mg-O, Si-O, OH, Si-OH, etc. After being crushed, the surface functional groups are exposed, and surface active sites appear, which have certain adsorption properties. However, the layered structure of black talc has high surface energy, which makes it very easy to accumulate into clusters, reduce the specific surface area, and cover the surface active sites. There are few exposed functional groups and limited adsorption performance. Black talc mineral materials modified by organic acid and coupling agent grafting have the advantages of stable skeleton structure, long-lasting repair effect, proper adjustment of soil pH and air permeability, environmental friendliness, no secondary pollution, etc., and have good repair effects on soils contaminated by different pollutants, and have a very broad application prospect. Summary of the invention

[0005] The purpose of the present invention is to provide a black talc adsorption material and a preparation method thereof and application thereof in adsorbing heavy metals in soil. The black talc adsorption material of the present invention has a larger specific surface area, strong adsorption performance, lasting repair effect, can appropriately adjust the pH and air permeability of the soil, is environmentally friendly, and has no secondary pollution.

[0006] In order to solve the above problems, the present invention adopts the following technical solutions:

[0007] The present invention provides a black talc adsorption material, and the black talc adsorption material is prepared according to the following method:

[0008] (1) Purification of black talc: Add water A and disodium hydrogen phosphate to black talc powder with an average particle size of 400-500 nm, stir at 25-40° C. for 12-20 h (preferably at 30° C. for 15 h), and subject the resulting mixture to post-treatment A to obtain purified black talc powder; the mass ratio of the black talc powder to disodium hydrogen phosphate is 100:2-7 (preferably 100:2.5);

[0009] (2) Add ethanol and water B to the purified black talc powder described in step (1), mix evenly, and disperse by ultrasound; add a modifier, stir and react at 75-95°C for 6-12h (preferably 85°C for 6h), and post-treat the resulting reaction solution to obtain the black talc adsorption material; the volume ratio of the ethanol to the water B is 7-10:1 (preferably 7.5:1); the volume of the ethanol is 4-8mL / g (preferably 7.5mL / g) based on the mass of the black talc; the modifier is citric acid or tartaric acid (preferably citric acid); the mass ratio of the purified black talc powder to the modifier is 1-10:1 (preferably 1-5:1, most preferably 5:1).

[0010] Water A and water B are both water. Different letters are used only to distinguish the water added at different stages and have no other special meaning.

[0011] Furthermore, the black talc powder in step (1) is an ultrafine black talc powder with an average particle size of 400-500 nm. The black talc powder is specifically prepared by the following method: crushing and grinding black talc (black talc comes from Guangfeng District, Shangrao, Jiangxi) and sieving with a 50-mesh sieve to obtain 50-mesh black talc powder, placing it in a ball mill, adding ethanol, wet ball milling at 800 rpm for 6-9 hours, centrifuging, washing the precipitate with water, centrifuging again, and drying at 60°C for 24 hours to obtain black talc powder with an average particle size of 400-500 nm.

[0012] Preferably, the mass ratio of the black talc powder to water A in step (1) is 1:8-12 (preferably 1:9-10.5, most preferably 1:9).

[0013] Furthermore, the post-treatment A in step (1) is as follows: the mixture is allowed to stand (preferably for 12 hours), the upper black talc suspension is taken (the bottom precipitate is discarded) and centrifuged, the obtained precipitate is washed with water (three times), and dried at 80-110° C. for 6-12 hours (preferably at 105° C. for 6 hours) to obtain the purified black talc powder.

[0014] Furthermore, the post-treatment B in step (2) is: the reaction solution is centrifuged, the obtained precipitate is washed with water, water is removed, and it is dried at 80-110° C. for 6-12 h (preferably at 105° C. for 12 h) to obtain the black talc adsorption material.

[0015] The present invention also provides an application of the black talc adsorption material in adsorbing heavy metals in soil.

[0016] Preferably, the heavy metal is Pb 2+ .

[0017] Further preferably, the application is: adding the black talc adsorption material to the air-dried soil, mixing thoroughly, adding deionized water to keep the soil at a moisture content of 60%, and mixing and culturing for 7 days to complete the adsorption; wherein the mass ratio of the black talc adsorption material to the air-dried soil is 1:20.

[0018] Compared with the prior art, the beneficial effects of the present invention are: using black talc as raw material, the price is low, the raw material is easy to obtain, the black talc soil adsorption material produced by the process has a larger specific surface area, is in a regular lamellar shape and does not stack each other, and has stronger adsorption performance and high stability. The black talc soil adsorption material prepared by the method of the present invention has abundant -COOH, Si-O, -OH, long alkane chains, and Mg coordinated unsaturated sites. The black talc can interact with the modifier through hydrogen bonds, electrostatic attraction, and van der Waals forces, and is firmly combined. It has high stability and hydrophobic effect, and the surface active sites are greatly increased, which improves the ability to bind to heavy metal ions, the adsorption rate is fast, and the adsorption capacity is high, thereby achieving the purpose of adsorption and passivation. The preparation method of the present invention is simple, the reaction conditions are easy to control, and the black talc soil adsorption material has excellent mechanical stability, dispersibility, strong adsorption, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a scanning electron microscope image of modified black talc powder.

[0020] Figure 2 Infrared spectra of the black talc prepared in Example 1 (bottom) and the modified black talc (top). DETAILED DESCRIPTION

[0021] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. Without departing from the content and scope of the present invention, changes in implementation should be included in the technical scope of the present invention.

[0022] The black talc in the following examples all comes from Guangfeng District, Shangrao, Jiangxi Province;

[0023] The measurement method and conditions of the adsorption amount in the following examples are:

[0024] The soil was collected from the garden next to the laboratory building of the rockery campus of Zhejiang University of Technology. After air drying at room temperature, 500 g of soil was accurately weighed and passed through a 2 mm sieve. 200 mg / L Pb(NO 3 ) 2250mL of solution was mixed thoroughly with the soil. After 60 days of water conservation, it was naturally air-dried, ground, and sieved through a 2mm sieve to prepare simulated lead-contaminated soil as the test soil. 0.5g of dry adsorbent powder was added to the air-dried soil sample (10g), and then thoroughly mixed in a polyethylene cup. The mass of black talc adsorbent in the soil was 5% of the air-dried soil sample. Deionized water was then added to keep the soil at 60% water content and mixed for 7 days. Finally, 1.0g of soil sample was extracted with a solution containing 20mL of acetic acid solution (pH=2.88) in a 50mL centrifuge tube. The tube was shaken in a rotary shaker at 30r / min for 18 hours. Then, the supernatant was collected and the remaining heavy metal concentration in the soil leachate was tested by ICP-OES. Finally, the adsorption capacity of the adsorbent was calculated by the formula q = (Co-Ce) * V / m, where Co is the heavy metal concentration in the soil leachate without adsorbent (2.5 mg / L), Ce is the heavy metal concentration in the soil leachate with adsorbent (mg / L), V is the volume of the leachate (0.02 L), and m is the mass of the adsorbent (0.05 g).

[0025] The preparation method of black talc powder in the following examples is as follows:

[0026] 80g of black talc was manually crushed, ground, and sieved with a 50-mesh sieve to obtain 70g of 50-mesh black talc powder. 50g of black talc powder was weighed and placed in a ball mill, 80ml of ethanol was added, and the ball mill was wet-milled at 800 rpm for 6h, centrifuged, and the resulting precipitate was washed with water 3 times, centrifuged, and dried at 60°C for 24h to prepare 40g of black talc powder. The average particle size of the prepared black talc powder was 400nm when observed by scanning electron microscopy.

[0027] Example 1

[0028] (1) Add 20 g of black talc powder into a 300 ml conical flask, then add 180 g of water and 0.5 g of disodium hydrogen phosphate, and stir at 30° C. for 15 h; let stand for 12 h, draw out the upper layer of black talc suspension, centrifuge, wash three times with water, and dry at 105° C. for 6 h to obtain 11.3 g of purified black talc powder.

[0029] (2) Add 1.0g of the obtained purified black talc into a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.2g of the modifier citric acid, stir and react at 85℃ for 6h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.95g of black talc soil adsorption material. Mix 0.5g of the black talc adsorption material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of the soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.481mg / L; the black talc adsorption material has a strong affinity for Pb 2+ The adsorption capacity is 7.6 mg / kg.

[0030] Example 2

[0031] (1) Add 20 g of black talc powder into a 300 ml conical flask, then add 210 g of water and 0.7 g of disodium hydrogen phosphate, and stir at 30° C. for 15 h; let stand for 12 h, draw out the upper layer of black talc suspension, centrifuge, wash three times with water, and dry at 105° C. for 6 h to obtain 10.4 g of purified black talc powder.

[0032] (2) Add 1.0g of the obtained purified black talc into a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.5g of citric acid, stir and react at 85℃ for 6h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.92g of black talc soil adsorption material. Mix 0.5g of the black talc adsorption material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.491mg / L; the black talc soil adsorption material has a strong affinity for Pb 2+ The adsorption capacity is 3.6 mg / kg.

[0033] Example 3

[0034] (1) Add 20 g of black talc powder into a 300 ml conical flask, then add 240 g of water and 0.7 g of disodium hydrogen phosphate, and stir at 30°C for 15 h; let stand for 12 h, draw out the upper layer of black talc suspension, centrifuge, wash three times with water, and dry at 105°C for 6 h to obtain 9.9 g of purified black talc powder.

[0035] (2) Add 1.0g of the obtained purified black talc into a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.1g of citric acid, stir and react at 85℃ for 6h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.92g of black talc soil adsorption material. Mix 0.5g of the black talc adsorption material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.489mg / L; the black talc soil adsorption material has a strong affinity for Pb 2+ The adsorption capacity is 4.4 mg / kg.

[0036] Example 4

[0037] (1) Add 20 g of black talc powder into a 300 ml conical flask, then add 210 g of water and 0.5 g of disodium hydrogen phosphate, and stir at 30° C. for 15 h; let stand for 12 h, draw out the upper layer of black talc suspension, centrifuge, wash three times with water, and dry at 105° C. for 6 h to obtain 11.0 g of purified black talc powder.

[0038] (2) Add 1.0g of the obtained purified black talc into a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.2g of citric acid, stir and react at 85℃ for 12h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.90g of black talc soil adsorption material. Mix 0.5g of the black talc adsorption material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.482mg / L; the black talc soil adsorption material has a strong affinity for Pb 2+ The adsorption capacity is 7.2 mg / kg.

[0039] Example 5

[0040] (1) Add 20 g of black talc powder into a 300 ml conical flask, then add 180 g of water and 0.4 g of disodium hydrogen phosphate, and stir at 30° C. for 15 h; let stand for 12 h, draw out the upper layer of black talc suspension, centrifuge, wash three times with water, and dry at 105° C. for 6 h to obtain 10.8 g of purified black talc powder.

[0041] (2) Add 1.0g of the obtained purified black talc into a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.2g of citric acid, stir and react at 60℃ for 12h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.85g of black talc soil adsorption material. Mix 0.5g of the black talc adsorption material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of the soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.491mg / L; the black talc soil adsorption material has a strong affinity for Pb 2+ The adsorption capacity is 3.6 mg / kg.

[0042] Example 6

[0043] (1) Add 20 g of black talc powder into a 300 ml conical flask, then add 240 g of water and 0.4 g of disodium hydrogen phosphate, and stir at 30° C. for 15 h; let stand for 12 h, draw out the upper layer of black talc suspension, centrifuge, wash three times with water, and dry at 105° C. for 6 h to obtain 9.0 g of purified black talc powder.

[0044] (2) Add 1.0g of the obtained purified black talc into a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.2g of citric acid, stir and react at 95℃ for 6h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.93g of black talc soil adsorption material. Mix 0.5g of the black talc adsorption material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.485mg / L; the black talc soil adsorption material has a strong affinity for Pb 2+ The adsorption capacity is 6.0 mg / kg.

[0045] Example 7

[0046] (1) Add 20 g of black talc powder into a 300 ml conical flask, then add 180 g of water and 0.7 g of disodium hydrogen phosphate, and stir at 30° C. for 15 h; let stand for 12 h, draw out the upper layer of black talc suspension, centrifuge, wash three times with water, and dry at 105° C. for 6 h to obtain 9.4 g of purified black talc powder.

[0047] (2) Add 1.0g of the obtained purified black talc into a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.2g of tartaric acid as a modifier, stir and react at 85℃ for 6h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.92g of modified black talc adsorbent. Mix 0.5g of the black talc adsorbent material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of the soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.486mg / L; the black talc soil adsorbent has a strong affinity for Pb 2+ The adsorption capacity is 5.6 mg / kg.

[0048] Comparative Example 1

[0049] (1) Take 1.0g of black talc powder (unpurified) directly and add it to a 50ml three-necked bottle, then add 7.5ml of ethanol and 1ml of water to mix evenly, and ultrasonically disperse for 30min; add 0.2g of citric acid as a modifier, stir and react at 85℃ for 6h, centrifuge, wash with water, and dry at 105℃ for 12h to obtain 0.92g of black talc adsorption material. Mix 0.5g of the black talc soil adsorption material with 10g of the test soil and add 6ml of water. After incubation at room temperature for 7 days, air-dry the soil, take 1.0g of the soil, and extract the soil sample with acetic acid solution (pH=2.88). The volume of the leaching solution is 0.02L. ICP-OES measures the heavy metal concentration in the soil leaching solution to be 2.494mg / L; the black talc adsorption material has a strong affinity for Pb 2+ The adsorption capacity is 2.4 mg / kg.

[0050] Comparative Example 2

[0051] (1) 0.5 g of unmodified black talc (purified) was mixed with 10 g of test soil and 6 ml of water was added. After incubation at room temperature for 7 days, the soil was air-dried and 1.0 g of soil was taken. The soil sample was extracted with acetic acid solution (pH = 2.88). The volume of the leaching solution was 0.02 L. ICP-OES measured the heavy metal concentration in the soil leaching solution to be 2.499 mg / L. The black talc adsorption material had a good effect on Pb 2+ The adsorption capacity is 0.4 mg / kg.

Claims

1. A method for preparing a black talc adsorption material, Features: (1) Purification of black talc: adding water A and disodium hydrogen phosphate to black talc powder with an average particle size of 400-500 nm, stirring at 25-40° C. for 12-20 h, and subjecting the resulting mixture to post-treatment A to obtain purified black talc powder; the mass ratio of the black talc powder to disodium hydrogen phosphate is 100:2-7; (2) Add ethanol and water B to the purified black talc powder described in step (1), mix evenly, and disperse by ultrasonication; add a modifier, stir and react at 75-95° C. for 6-12 hours, and post-treat the resulting reaction solution to obtain the black talc adsorption material; the volume ratio of the ethanol to the water B is 7-10:1; the volume of the ethanol is 4-8 mL / g based on the mass of the black talc; the modifier is citric acid or tartaric acid; the mass ratio of the purified black talc powder to the modifier is 1-10:

1.

2. The method for preparing the black talc adsorption material according to claim 1, Features: The black talc powder in step (1) is prepared as follows: the black talc is crushed, ground, and sieved with a 50-mesh sieve to obtain a 50-mesh black talc powder, which is placed in a ball mill, ethanol is added, and wet ball milled at 800 rpm for 6-9 hours, centrifuged, washed with water, and precipitated, centrifuged again, and dried at 60°C for 24 hours to obtain a black talc powder with an average particle size of 400-500 nm.

3. The method for preparing the black talc adsorption material according to claim 1, Features: The mass ratio of the black talc powder to water A in step (1) is 1:8-12.

4. The method for preparing the black talc adsorption material according to claim 1, Features: The post-treatment A in step (1) is as follows: the mixture is allowed to stand, the upper black talc suspension is centrifuged, the obtained precipitate is washed with water, and dried at 80-110° C. for 6-12 hours to obtain the purified black talc powder.

5. The method for preparing the black talc adsorption material according to claim 1, Features: The modifier is citric acid.

6. The method for preparing the black talc adsorption material according to claim 1, Features: The mass ratio of the purified black talcum powder to the modifier is 1-5:

1.

7. The method for preparing the black talc adsorption material according to claim 1, Features: The post-treatment B in step (2) is as follows: the reaction solution is centrifuged, the obtained precipitate is washed with water, water is removed, and the precipitate is dried at 80-110° C. for 6-12 hours to obtain the black talc adsorption material.